Coercive force enhanced ternary magnetic material and ternary magnetic strip and preparation method thereof
By preparing Pr1-xTbxCo3 ternary magnetic material, the mixing of light rare earth Pr and heavy rare earth Tb is used to form a PuNi3-type rhombus structure, which solves the problem of insufficient coercivity of existing rare earth-cobalt-based magnetic materials and achieves a higher Improved coercive force and magnetic properties.
Patent Information
- Application Number
- CN202411103155.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-12
AI Technical Summary
The existing rare earth-cobalt-based binary magnetic materials have low coercive forces and are difficult to meet the needs of high-performance permanent magnet materials.
The ternary magnetic material of Pr1-xTbxCo3 is prepared by smelting and heat treatment processes to form a PuNi3-type rhombus single-phase crystal structure, combining the mixture of light rare earth Pr and heavy rare earth Tb to enhance the coercive force of the magnetic material.
The coercive force and magnetic properties of magnetic materials have been significantly improved, and the cost is reduced, and the coercive force is greatly improved compared with the binary compounds of PrCo3 and TbCo3.
Smart Images

Figure CN118942825A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of magnetic materials, and in particular relates to a ternary magnetic material with enhanced coercivity and a ternary magnetic strip and a preparation method thereof. Background Art
[0002] Permanent magnetic materials are widely used in sensors, instruments, electronics, electromechanics, medical treatment, teaching, automobiles, aviation, military, precision instruments, precision meters, advanced electroacoustic and telecommunication devices, etc. At present, the demand for permanent magnetic materials is increasing, which means that the performance of existing permanent magnetic materials needs to be continuously improved, requiring the magnet to maintain a high magnetic energy product (BH) at high operating temperatures, and on this basis, developing new permanent magnetic materials.
[0003] Since their discovery in the late 1960s, rare earth-cobalt-based magnetic materials (R-Co) have attracted widespread attention due to their large anisotropic magnetic field HA, high saturation magnetization Ms, and high Curie temperature Tc. Most of the interest in this type of alloy has focused on SmCo5 because it has extremely high HA, high coercivity Hc, and a relatively high maximum energy product (BH). max , which is an important performance index of permanent magnets. After different process treatments, rare earth cobalt-based compounds have attracted people's attention due to their good magnetic properties.
[0004] Melt quenching is currently a hot topic for preparing nanocrystalline rare earth permanent magnet materials. Through melt quenching, uniform and fine grains can be obtained. Melt quenching is to inject molten metal or alloy under a certain pressure into a high-speed rotating copper hub wheel under a high vacuum state, so that it solidifies under a very large degree of supercooling to obtain a non-equilibrium structure with an ultra-fine structure. Since this method has an extremely high cooling rate, the grain size of metals and alloys can reach the nanometer level or obtain an amorphous structure, so that the prepared metal or alloy has completely different mechanical and physical properties from general non-equilibrium cooling metals. Moreover, since the rotation speed of the copper hub and the injection pressure of the liquid metal are adjustable, the cooling rate can be strictly controlled, thereby achieving the purpose of controlling the grain size of the metal or alloy. The process of preparing nanocrystals by melt quenching is easy to control, and can be mass-produced and industrialized.
[0005] The rare earth (R)-cobalt binary intermetallic compound RCo3 crystallizes in a PuNi3-type rhombohedral structure (space group R-3m). In this single unit cell, R atoms occupy the 3a and 6c crystal sites; cobalt atoms are located in the 3b, 6c and 18h crystal sites. In RCo3, the localized magnetic sublattice of 4f electrons can be well isolated from the itinerant magnetic sublattice formed by 3d-5d hybrid band electrons. In RCo3 compounds (except R=Tm and Y), the Co sublattice is in a strong ferromagnetic ground state. Both Co-Co and R-Co exchange interactions strongly affect the magnetic state of the Co sublattice. When light rare earth and heavy rare earth form compounds with Co at the same time, the magnetic moment of the light rare earth sublattice is parallel to that of the Co sublattice; the magnetic moment of the heavy rare earth sublattice is antiparallel to that of the Co sublattice. Traditional binary cobalt-based magnetic materials are mainly PrCo3 and TbCo3, but they still have the defect of low coercivity. Summary of the invention
[0006] The object of the present invention is to provide a ternary magnetic material and a ternary magnetic strip with enhanced coercivity and a preparation method thereof. The ternary magnetic material or the ternary magnetic strip provided by the present invention has a relatively high coercivity.
[0007] In order to achieve the above object, the present invention provides the following technical solutions:
[0008] The present invention provides a ternary magnetic material with enhanced coercivity, wherein the chemical composition of the ternary magnetic material is Pr 1-x Tb x Co3, where x is 0.1<x<0.9;
[0009] The ternary magnetic material has a PuNi3 type rhombohedral single-phase crystal structure.
[0010] The present invention also provides a method for preparing the ternary magnetic material described in the above technical solution, comprising the following steps:
[0011] According to the chemical composition of the ternary magnetic material, required raw materials are mixed and then smelted to obtain an alloy;
[0012] The alloy is heat treated to obtain the ternary magnetic material.
[0013] Preferably, the arc current of the smelting is 80-120A, and the smelting is repeated 4-6 times;
[0014] The smelting is carried out under a protective atmosphere.
[0015] Preferably, the heat treatment temperature is 600-900° C., and the time is 1 hour to 7 days.
[0016] Preferably, after the heat treatment, the obtained alloy material is placed in ice water to cool to room temperature and then soaked for 30 minutes.
[0017] The present invention also provides a ternary magnetic strip with enhanced coercivity, wherein the chemical composition of the ternary magnetic strip is Pr 1-x Tb x Co3, where x is 0.1<x<0.9;
[0018] The ternary magnetic strip has a PuNi3 type rhombohedral single-phase crystal structure.
[0019] The present invention also provides a method for preparing the ternary magnetic strip described in the above technical solution, comprising the following steps:
[0020] According to the chemical composition of the ternary magnetic strip, required raw materials are mixed and then smelted to obtain an alloy;
[0021] The alloy is subjected to strip-spinning treatment to obtain the ternary magnetic strip.
[0022] Preferably, the conditions for the belt-spinning treatment include: induction melting the alloy into a liquid state under argon conditions at a chamber pressure of 0.04-0.06 MPa, and then performing the belt-spinning treatment at a roller speed of 30 m / s.
[0023] Preferably, after the strip-spinning process, the obtained strip is further subjected to heat treatment.
[0024] Preferably, the heat treatment temperature is 600-900°C and the time is 1 hour to 7 days;
[0025] After the heat treatment, the obtained alloy material is placed in ice water to cool to room temperature and then soaked for 30 minutes.
[0026] The present invention provides a ternary magnetic material with enhanced coercivity, wherein the chemical composition of the ternary magnetic material is Pr 1-x Tb x Co3, wherein the value of x is 0.1<x<0.9; the ternary magnetic material has a PuNi3 type rhombohedral single-phase crystal structure. The present invention mixes light rare earth Pr and heavy rare earth Tb and simultaneously adds them to form a ternary compound Pr 1-x Tb x Co3, this magnetic compound shows the characteristics of enhanced coercivity. While reducing the cost, the coercivity is greatly improved compared with the binary compounds of PrCo3 and TbCo3.
[0027] The present invention also provides a ternary magnetic strip with enhanced coercivity, wherein the chemical composition of the ternary magnetic strip is Pr 1-x Tbx Co3, wherein the value of x is 0.1<x<0.9; the ternary magnetic strip has a PuNi3 type rhombohedral single-phase crystal structure. The magnetic strip provided by the present invention has greater coercivity and better magnetic properties, and the coercivity enhancement phenomenon is more significant. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 The single-phase XRD patterns of the magnetic materials obtained in Examples 1 to 7 and Comparative Examples 1 to 4;
[0029] Figure 2 This is the metallographic structure diagram of the magnetic material obtained in Example 5;
[0030] Figure 3 hysteresis loops of the magnetic materials obtained in Examples 1 to 7 and Comparative Examples 1 to 4 at room temperature;
[0031] Figure 4 The coercive force and saturation magnetization intensity of the magnetic materials obtained in Examples 1 to 7 and Comparative Examples 1 to 4 at room temperature are shown in FIG.
[0032] Figure 5 The single-phase XRD patterns of the magnetic strips obtained in Examples 8 to 14 and Comparative Examples 5 to 8;
[0033] Figure 6 This is the metallographic structure diagram of the magnetic strip obtained in Example 12;
[0034] Figure 7 hysteresis loops of the magnetic strips obtained in Examples 8 to 14 and Comparative Examples 5 to 8 at room temperature;
[0035] Figure 8 The coercive force and saturation magnetization intensity of the magnetic strips obtained in Examples 8 to 14 and Comparative Examples 5 to 8 at room temperature are shown in FIG.
[0036] Fig. 9 The single-phase XRD patterns of the magnetic strips obtained in Examples 15 to 21 and Comparative Examples 9 to 12;
[0037] Fig.10 This is the metallographic structure diagram of the magnetic strip obtained in Example 19;
[0038] Fig.11 hysteresis loops of the magnetic strips obtained in Examples 15 to 21 and Comparative Examples 9 to 12 at room temperature;
[0039] Fig.12 The coercive force and saturation magnetization intensity of the magnetic strips obtained in Examples 15 to 21 and Comparative Examples 9 to 12 at room temperature are shown in FIG.
[0040] Fig.13hysteresis loops of the magnetic strips obtained in Examples 15 to 21 and Comparative Examples 9 to 12 measured at a low temperature of 10 K;
[0041] Fig.14 The coercive force and saturation magnetization intensity variation diagram of the magnetic strips obtained in Examples 15 to 21 and Comparative Examples 9 to 12 measured at a low temperature of 10K;
[0042] Fig.15 This is a comparison chart of the coercive force of the magnetic strips obtained in Examples 1 to 21 and Comparative Examples 1 to 12 at room temperature. DETAILED DESCRIPTION
[0043] The present invention provides a ternary magnetic material with enhanced coercivity, wherein the chemical composition of the ternary magnetic material is Pr 1-x Tb x Co3, where x is 0.1<x<0.9;
[0044] The ternary magnetic material has a PuNi3 type rhombohedral single-phase crystal structure.
[0045] In the present invention, the value of x is 0.1<x<0.9, more preferably 0.2 to 0.8, and more preferably 0.3 to 0.7. In a specific embodiment of the present invention, the value of x is 0.2, 0.3, 0.4, 0.5, 0.6, 0.7 or 0.8.
[0046] In the present invention, the coercive force of the ternary magnetic material is preferably 0.13-0.41 kOe; the saturation magnetization intensity of the ternary magnetic material is preferably 4.98-17.60 emu / g.
[0047] The present invention also provides a method for preparing the ternary magnetic material described in the above technical solution, comprising the following steps:
[0048] According to the chemical composition of the ternary magnetic material, required raw materials are mixed and then smelted to obtain an alloy;
[0049] The alloy is heat treated to obtain the ternary magnetic material.
[0050] According to the chemical composition of the ternary magnetic material, the invention mixes the required raw materials and then smelts them to obtain the alloy.
[0051] In the present invention, the smelting method is preferably argon arc smelting. In the present invention, the arc current of the smelting is preferably 80-120A, and the number of repetitions of the smelting is preferably 4-6 times; the smelting is preferably carried out under a protective atmosphere, and the protective atmosphere is preferably argon.
[0052] After obtaining the alloy, the present invention performs heat treatment on the alloy to obtain the ternary magnetic material.
[0053] In the present invention, the temperature of the heat treatment is preferably 600°C to 900°C, more preferably 800°C; the time is preferably 1 hour to 7 days, more preferably 7 days. In the present invention, the heat treatment method is preferably: sealing the alloy in a vacuum quartz tube, and then placing the vacuum quartz tube in an annealing furnace for heat treatment.
[0054] In the present invention, after the heat treatment, the obtained alloy material is preferably placed in ice water to cool to room temperature and then soaked for 30 minutes.
[0055] The present invention also provides a ternary magnetic strip with enhanced coercivity, wherein the chemical composition of the ternary magnetic strip is Pr 1-x Tb x Co3, where x is 0.1<x<0.9;
[0056] The ternary magnetic strip has a PuNi3 type rhombohedral single-phase crystal structure.
[0057] In the present invention, the value of x is 0.1<x<0.9, more preferably 0.2 to 0.8, and more preferably 0.3 to 0.7. In a specific embodiment of the present invention, the value of x is 0.2, 0.3, 0.4, 0.5, 0.6, 0.7 or 0.8.
[0058] In the present invention, the coercive force of the ternary magnetic strip is preferably 0.55-7.53 kOe; the saturation magnetization of the ternary magnetic strip is preferably 3.26-23.05 emu / g.
[0059] The present invention also provides a method for preparing the ternary magnetic strip described in the above technical solution, comprising the following steps:
[0060] According to the chemical composition of the ternary magnetic strip, required raw materials are mixed and then smelted to obtain an alloy;
[0061] The alloy is subjected to strip-spinning treatment to obtain the ternary magnetic strip.
[0062] In the present invention, the smelting process is consistent with the smelting process defined in the above technical solution, and will not be repeated here.
[0063] In the present invention, the conditions for the strip-spinning treatment preferably include: induction melting the alloy into liquid under argon conditions at a chamber pressure of 0.04-0.06 MPa, and then performing the strip-spinning treatment at a roller speed of 30 m / s.
[0064] In the present invention, after the strip-spinning treatment, it is also preferred to heat-treat the obtained strip. In the present invention, the temperature of the heat treatment is preferably 600°C to 900°C, more preferably 800°C; the time is preferably 1 hour to 7 days, more preferably 4 hours. In the present invention, the heat treatment method is preferably: the obtained strip is sealed in a vacuum quartz tube, and then the vacuum quartz tube is placed in an annealing furnace for heat treatment. After the heat treatment, the present invention also preferably includes placing the obtained alloy material in ice water to cool to room temperature and soaking it for 30 minutes.
[0065] Unless otherwise specified, the materials and equipment used in the present invention are all commercially available products in the art.
[0066] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0067] Examples 1 to 7
[0068] According to the chemical composition of the ternary magnetic material, the required raw materials are melted by argon arc melting, wherein the arc current is 100A, and the melting is repeated 4 times to obtain an alloy;
[0069] The alloy is sealed in a vacuum quartz tube, placed in an annealing furnace at 800° C. for heat treatment for 7 days, then placed in an ice-water mixture to be rapidly cooled to room temperature and soaked for half an hour to obtain the ternary magnetic material.
[0070] The chemical compositions of the ternary magnetic materials in Examples 1 to 7 are shown in Table 1;
[0071] Table 1 Chemical composition of ternary magnetic materials in Examples 1 to 7
[0072] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 <![CDATA[Pr 0.8 Tb 0.2 Co3]]> <![CDATA[Pr 0.7 Tb 0.3 Co3]]> <![CDATA[Pr 0.6 Tb 0.4 Co3]]> <![CDATA[Pr 0.5 Tb 0.5 Co3]]> <![CDATA[Pr 0.4 Tb 0.6 Co3]]> <![CDATA[Pr 0.3 Tb 0.7 Co3]]> <![CDATA[Pr 0.2 Tb 0.8 Co3]]>
[0073] Comparative Examples 1 to 4
[0074] The ternary magnetic material was prepared in the manner of Example 1; wherein the chemical compositions of the ternary magnetic materials obtained in Comparative Examples 1 to 4 are shown in Table 2;
[0075] Table 2 Chemical composition of ternary magnetic materials in Comparative Examples 1 to 4
[0076] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 <![CDATA[PrCo3]]> <![CDATA[Pr 0.9 Tb 0.1 Co3]]> <![CDATA[Pr 0.1 Tb 0.9 Co3]]> <![CDATA[TbCo3]]>
[0077] Test Example 1
[0078] (1) In order to detect the sample composition structure, the ternary magnetic materials obtained in Examples 1 to 7 and Comparative Examples 1 to 4 were subjected to X-ray diffraction test, and the obtained XRD patterns are as follows: Figure 1 As shown, it can be seen that the obtained magnetic material exhibits a PuNi3-type rhombohedral single-phase crystal structure, but as the x value changes, the diffraction peak of XRD shifts.
[0079] (2) In order to verify that the sample is a single-phase structure, metallographic testing is used. The specific method is to grind out the metallographic structure of the sample after embedding it and observe the metallographic structure with a scanning electron microscope (SEM). Figure 2 The ternary magnetic material Pr obtained in Example 5 0.4 Tb 0.6 From the scanning electron microscopy results of Co3, it can be seen that the SEM image shows that the sample has only one phase.
[0080] (3) In order to test the hysteresis loop of the sample at room temperature, the magnetic properties of the sample are tested using a vibrating sample magnetometer (VSM). The specific method is as follows:
[0081] Select 1 to 20 mg of sample, apply a maximum external magnetic field of 2T, place the magnetic material to be tested parallel to the external magnetic field, and its magnetic moment has reached saturation under the 2T external magnetic field. Figure 3 is the hysteresis loop of the magnetic material, Figure 4 The coercive force and saturation magnetization intensity of the magnetic material at room temperature are shown in Table 3.
[0082] Table 3 Coercive force and saturation magnetization of magnetic materials obtained in Examples 1 to 7 and Comparative Examples 1 to 4
[0083]
[0084]
[0085] Embodiments 8 to 14
[0086] According to the chemical composition of the ternary magnetic strip, the required raw materials are melted by argon arc melting, wherein the arc current is 100A, and the melting is repeated 4 times to obtain the alloy;
[0087] The alloy was induction melted into liquid under the condition of argon gas at a chamber pressure of 0.05 MPa, and then subjected to strip spinning treatment at a roller speed of 30 m / s to obtain a ternary magnetic strip.
[0088] The chemical compositions of the ternary magnetic strips in Examples 8 to 14 are shown in Table 4;
[0089] Table 4 Chemical composition of the ternary magnetic strips in Examples 8 to 14
[0090] Example 8 Example 9 Example 10 Embodiment 11 Example 12 Example 13 Embodiment 14 <![CDATA[Pr 0.8 Tb 0.2 Co3]]> <![CDATA[Pr 0.7 Tb 0.3 Co3]]> <![CDATA[Pr 0.6 Tb 0.4 Co3]]> <![CDATA[Pr 0.5 Tb 0.5 Co3]]> <![CDATA[Pr 0.4 Tb 0.6 Co3]]> <![CDATA[Pr 0.3 Tb 0.7 Co3]]> <![CDATA[Pr 0.2 Tb 0.8 Co3]]>
[0091] Comparative Examples 5 to 8
[0092] The ternary magnetic strip was prepared in the manner of Example 8; wherein the chemical compositions of the ternary magnetic strips obtained in Comparative Examples 5 to 8 are shown in Table 5;
[0093] Table 5 Chemical composition of the ternary magnetic strips in Comparative Examples 5 to 8
[0094] Comparative Example 5 Comparative Example 6 Comparative Example 7 Comparative Example 8 <![CDATA[PrCo3]]> <![CDATA[Pr 0.9 Tb 0.1 Co3]]> <![CDATA[Pr 0.1 Tb 0.9 Co3]]> <![CDATA[TbCo3]]>
[0095] Test Example 2
[0096] (1) In order to detect the composition structure of the samples, X-ray diffraction test was performed on the ternary magnetic strips obtained in Examples 8 to 14 and Comparative Examples 5 to 8. The obtained XRD patterns are as follows: Figure 5 As shown, it can be seen that the magnetic strip has a PuNi3-type rhombohedral single-phase crystal structure. As the x value changes, the XRD diffraction peak shifts. The scanning electron microscopy results of the magnetic strip obtained in Example 12 are shown in Figure 6 shown.
[0097] (2) The magnetic properties of the obtained ternary magnetic strip were tested according to the method in Test Example 1. Figure 7 is the hysteresis loop of the ternary magnetic strip, Figure 8 The coercive force and saturation magnetization intensity of the ternary magnetic strip at room temperature are shown in Table 6.
[0098] Table 6 Coercive force and saturation magnetization of magnetic strips obtained in Examples 8 to 14 and Comparative Examples 5 to 8
[0099] Example 8 Example 9 Example 10 Embodiment 11 Example 12 Example 13 Coercivity(kOe) 0.91 1.09 1.75 2.77 3.93 1.75 Saturation magnetization (emu / g) 23.05 16.89 15.94 11.06 5.87 3.26 Embodiment 14 Comparative Example 5 Comparative Example 6 Comparative Example 7 Comparative Example 8 Coercivity(kOe) 1.60 0.42 0.58 0.42 0.26 Saturation magnetization (emu / g) 11.11 25.00 24.89 16.68 29.81
[0100] Examples 15 to 21
[0101] According to the chemical composition of the ternary magnetic strip, the required raw materials are melted by argon arc melting, wherein the arc current is 100A, and the melting is repeated 4 times to obtain the alloy;
[0102] The alloy is induction melted into liquid under the condition of argon gas at a chamber pressure of 0.05 MPa, and then subjected to belt spinning treatment at a roller speed of 30 m / s;
[0103] The obtained strip was sealed in a vacuum quartz tube, placed in an annealing furnace at 800° C. for heat treatment for 4 hours, then placed in an ice-water mixture to be quickly cooled to room temperature and soaked for half an hour to obtain the ternary magnetic strip.
[0104] The chemical compositions of the ternary magnetic material strips in Examples 15 to 21 are shown in Table 7;
[0105] Table 7 Chemical composition of the ternary magnetic strips in Examples 15 to 21
[0106] Embodiment 15 Example 16 Embodiment 17 Embodiment 18 Embodiment 19 Embodiment 20 Embodiment 21 <![CDATA[Pr 0.8 Tb 0.2 Co3]]> <![CDATA[Pr 0.7 Tb 0.3 Co3]]> <![CDATA[Pr 0.6 Tb 0.4 Co3]]> <![CDATA[Pr 0.5 Tb 0.5 Co3]]> <![CDATA[Pr 0.4 Tb 0.6 Co3]]> <![CDATA[Pr 0.3 Tb 0.7 Co3]]> <![CDATA[Pr 0.2 Tb 0.8 Co3]]>
[0107] Comparative Examples 9 to 12
[0108] The ternary magnetic strip was prepared in the manner of Example 15; wherein the chemical compositions of the ternary magnetic strips obtained in Comparative Examples 9 to 12 are shown in Table 8;
[0109] Table 8 Chemical composition of ternary magnetic strips in comparative examples 9 to 12
[0110] Comparative Example 9 Comparative Example 10 Comparative Example 11 Comparative Example 12 <![CDATA[PrCo3]]> <![CDATA[Pr 0.9 Tb 0.1 Co3]]> <![CDATA[Pr 0.1 Tb 0.9 Co3]]> <![CDATA[TbCo3]]>
[0111] Test Example 3
[0112] (1) In order to detect the composition structure of the samples, X-ray diffraction test was performed on the ternary magnetic strips obtained in Examples 15 to 21 and Comparative Examples 9 to 12. The obtained XRD patterns are as follows: Fig. 9 As shown, it can be seen that the magnetic strip has a PuNi3-type rhombohedral single-phase crystal structure, but as the x value changes, the XRD diffraction peak shifts; the scanning electron microscopy results of the magnetic strip obtained in Example 19 are as follows Fig.10 As shown, the SEM image shows that the sample has only one phase.
[0113] (2) The magnetic properties of the obtained ternary magnetic strip were tested according to the method in Test Example 1. Fig.11 is the hysteresis loop of the ternary magnetic strip, Fig.12 is a graph showing the coercive force and saturation magnetization intensity of the ternary magnetic strip at room temperature. The specific test results are shown in Table 9;
[0114] Table 9 Coercive force and saturation magnetization of magnetic strips obtained in Examples 15 to 21 and Comparative Examples 9 to 12
[0115]
[0116]
[0117] (3) According to the method in Test Example 1, the magnetic properties of the obtained ternary magnetic strip were tested at a low temperature of 10K. Fig.13 is the hysteresis loop of the ternary magnetic strip at low temperature, Fig.14 The coercive force and saturation magnetization intensity variation diagram of the ternary magnetic strip at low temperature. The specific test results are shown in Table 10.
[0118] Table 10 Coercive force and saturation magnetization of magnetic strips obtained in Examples 15 to 21 and Comparative Examples 9 to 12
[0119] Embodiment 15 Example 16 Embodiment 17 Embodiment 18 Embodiment 19 Embodiment 20 Coercivity(kOe) 25.58 31.17 27.40 24.70 15.94 18.45 Saturation magnetization (emu / g) 41.16 41.31 16.13 21.09 20.80 33.22 Embodiment 21 Comparative Example 9 Comparative Example 10 Comparative Example 11 Comparative Example 12 Coercivity(kOe) 17.55 10.83 15.19 7.17 3.19 Saturation magnetization (emu / g) 50.34 47.19 45.39 56.97 75.73
[0120] Fig.15 The coercivity curves of the magnetic materials or magnetic strips obtained in Examples 1 to 21 and Comparative Examples 1 to 12 at room temperature are shown in FIG. Fig.15 It can be seen that the magnetic material Pr 1-x Tb x Co3, the coercivity and magnetic properties of Co-based magnetic materials can be enhanced by mixing light rare earth Pr and heavy rare earth Tb. The enhanced coercivity at room temperature is of great significance for the in-depth research and development of the magnetic properties of light and heavy rare earth-cobalt-based compounds.
[0121] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A ternary magnetic material with enhanced coercivity, It is characterized in that The chemical composition of the ternary magnetic material Pr 1- x Tb x Co 3 , where the value of x is 0.1<x<0.9; The ternary magnetic material has PuNi 3 Rhombohedral single-phase crystal structure.
2. The method for preparing the ternary magnetic material according to claim 1, It is characterized in that The following steps are involved: According to the chemical composition of the ternary magnetic material, required raw materials are mixed and then smelted to obtain an alloy; The alloy is heat treated to obtain the ternary magnetic material.
3. The preparation method according to claim 2, It is characterized in that The arc current of the smelting is 80-120A, and the smelting is repeated 4-6 times; The smelting is carried out under a protective atmosphere.
4. The preparation method according to claim 2, It is characterized in that The heat treatment temperature is 600-900° C., and the time is 1 hour-7 days.
5. The preparation method according to claim 4, It is characterized in that After the heat treatment, the obtained alloy material is placed in ice water to cool to room temperature and then soaked for 30 minutes.
6. A ternary magnetic strip with enhanced coercivity, It is characterized in that The chemical composition of the ternary magnetic strip is Pr 1-x Tb x Co 3 , where the value of x is 0.1<x<0.9; The ternary magnetic strip has PuNi 3 Rhombohedral single-phase crystal structure.
7. The method for preparing the ternary magnetic strip according to claim 6, It is characterized in that The following steps are involved: According to the chemical composition of the ternary magnetic strip, required raw materials are mixed and then smelted to obtain an alloy; The alloy is subjected to strip-spinning treatment to obtain the ternary magnetic strip.
8. The preparation method according to claim 7, It is characterized in that The conditions of the strip-spinning treatment include: induction melting the alloy into a liquid state under the condition of a cavity pressure of 0.04-0.06 MPa and argon gas, and then performing the strip-spinning treatment under the condition of a roller speed of 30 m / s.
9. The preparation method according to claim 7 or 8, It is characterized in that After the strip-spinning process, the obtained strip is further subjected to heat treatment.
10. The preparation method according to claim 9, It is characterized in that The heat treatment temperature is 600-900°C and the time is 1 hour-7 days; After the heat treatment, the obtained alloy material is placed in ice water to cool to room temperature and then soaked for 30 minutes.