Nanocrystalline alloy magnetic core and preparation process thereof

The nanocrystalline alloy magnetic core fabrication process, which combines vacuum heat treatment and copper strip spiral winding, solves the problem of uneven grain size and improves the uniformity and soft magnetic properties of the magnetic core.

CN118942829AActive Publication Date: 2024-11-12TIANJIN AONA TECH
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411010414.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

In the current process of preparing nanocrystalline alloy magnetic cores, the difference in cooling rate between the free surface and the roller surface leads to uneven grain size, which affects the magnetic properties.

Method used

The method of vacuum heat treatment combined with copper strip spiral winding is used to reduce the temperature difference by uniformly delaying the heating of the inner and outer surfaces of the magnetic core, and passivation and curing treatment is performed to improve insulation.

Benefits of technology

This achieves uniform grain size inside and outside the magnetic core, improves magnetic properties, reduces losses, and enhances soft magnetic properties and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118942829A_ABST
    Figure CN118942829A_ABST
Patent Text Reader

Abstract

The invention discloses a nanocrystalline alloy magnetic core and a preparation process thereof, and relates to the technical field of magnetic materials, and the nanocrystalline alloy magnetic core is prepared from the following components in percentage by weight: 81%-85% of pure iron, 0.8%-1.2% of pure copper, 8%-10% of silicon iron and 5.5%-8.5% of ferroboron. According to the nanocrystalline alloy magnetic core and the preparation process thereof, the copper sheets are uniformly and spirally wound on the inner and outer sides of the magnetic core, so that the temperature rise of the inner and outer surfaces of the magnetic core can be delayed, the temperature difference between the middle part and the inner and outer sides of the magnetic core is reduced, the temperature distribution of the middle part and the two sides of the magnetic core is more uniform, and the internal stress is more uniformly eliminated; and simultaneous nucleation and growth at different positions of the magnetic core during second-step annealing are facilitated, so that the sizes of crystal grains inside and outside the magnetic core are more uniform, and the performance of the magnetic core is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of magnetic materials, in particular to a nanocrystalline alloy magnetic core and a preparation process thereof. Background Art

[0002] The measurement of AC current, voltage and electric energy is usually measured by mutual inductors. The core component of the mutual inductor is the magnetic core, and its performance directly determines the measurement accuracy of the mutual inductor. Nanocrystalline materials are composed of crystals of nanometer size (1-10nm). Because the crystals are extremely fine, the grain boundaries can account for 50% or more of the entire material. Its atomic arrangement is different from the ordered crystalline state and the disordered amorphous state (glass state). Its performance is also different from that of crystals or amorphous states with the same composition. In many occasions, traditional ferrite materials can no longer meet the needs. More and more EMC rectification plans use inductors made of a new material, called nanocrystalline magnetic cores. When measuring sinusoidal currents without DC components, high magnetic permeability soft magnetic materials are usually used to make magnetic cores to improve the measurement accuracy. Amorphous and nanocrystalline alloys have excellent soft magnetic properties, especially nanocrystalline alloy cores have excellent comprehensive magnetic properties, high saturation magnetic induction, high initial magnetic permeability, low Hc, low high-frequency loss under high magnetic induction, and higher resistivity than Permalloy. After longitudinal or transverse magnetic field treatment, high Br or low Br value can be obtained. It is the material with the best comprehensive performance on the market and is widely used in high-power switching power supplies, inverters, magnetic amplifiers, high-frequency transformers, etc.

[0003] A Chinese patent with publication number CN115881380A discloses a nanocrystalline alloy magnetic core, comprising Cu, Si, B, Sr, Ir, Bi, Ni, Te, rare earth elements, and Fe, wherein the contents of Cu, Si, B, Sr, Ir, Bi, Ni, Te, rare earth elements, and Fe are respectively Cu 0.6-1.0%, Si 8.0-10.0%, B 5.5-8.0%, Sr 0.1-0.3%, Ir 0.05-0.15%, Bi0.03-0.10%, Ni0.8-1.5%, Te 0.1-0.3%, rare earth elements 0.01-0.04%, and the balance is Fe. The present invention adopts vacuum heat treatment to the iron-based nanocrystalline magnetic core: heating at a heating rate of 1°C / min, taking 200°C as the furnace exit temperature, 540°C as the annealing temperature, and 60 minutes as the heat preservation annealing time, which is the best processing technology for the iron-based nanocrystalline magnetic core; however, the above-mentioned prior art solution has the following disadvantages: during the preparation process, due to the difference in cooling rate between the free surface and the roller surface, the grain size difference between the two surfaces is large, which affects the magnetic properties of the magnetic core; therefore, the present invention provides a nanocrystalline alloy magnetic core and a preparation process thereof to solve the above problems. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a nanocrystalline alloy magnetic core and a preparation process thereof, which solves the problems mentioned in the above background technology.

[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions: a nanocrystalline alloy magnetic core, comprising the following components in percentage by weight: 81% to 85% pure iron, 0.8% to 1.2% pure copper, 8% to 10% ferrosilicon, and 5.5% to 8.5% ferroboron.

[0006] A preparation process of a nanocrystalline alloy magnetic core comprises the following preparation steps:

[0007] S1. Preparation of master alloy:

[0008] S11, using pure iron, pure copper, ferrosilicon and ferroboron as raw materials, performing ultrasonic cleaning on the raw materials, removing surface dirt and then performing drying treatment;

[0009] S12, then placing in a vacuum melting furnace, and repeatedly melting, to obtain a master alloy with uniform component distribution;

[0010] S2, winding the master alloy to obtain a magnetic core;

[0011] S3. Vacuum heat treatment is applied to the magnetic core: the magnetic core is placed in a tubular furnace and nitrogen is introduced, then the temperature is raised to 500-510°C at a rate of 10°C / min, and then kept at this temperature for 15-20 minutes, then the temperature is raised to 540-550°C at a rate of 1°C / min, and then kept at this temperature for 50-60 minutes, and then the temperature is lowered to 180-200°C before being taken out of the furnace to obtain a nanocrystalline alloy magnetic core.

[0012] Preferably, the preparation process of the nanocrystalline alloy magnetic core also includes: S4, placing the nanocrystalline alloy magnetic core in a passivation solution and soaking it at room temperature for 100 to 120 minutes; then soaking and cleaning it with anhydrous ethanol, and then placing it in a drying oven at a temperature of 50 to 60° C. for drying for 40 to 60 minutes.

[0013] Preferably, the passivation solution is an iron-based phosphide passivation solution, and is diluted into an 8% solution before use.

[0014] Preferably, the preparation process of the nanocrystalline alloy magnetic core also includes: S5, immersing the passivated nanocrystalline alloy magnetic core in a curing agent, then pumping the air pressure to 0.01-0.03MPa, standing until no bubbles emerge on the surface and then restoring the atmospheric pressure, finally taking out the nanocrystalline alloy magnetic core and placing it in a drying oven at 90-100°C for 1.5-2h.

[0015] Preferably, the curing agent is any one selected from a silicone curing agent and a polyurethane curing agent.

[0016] Preferably, in S12, the internal pressure of the vacuum melting furnace is 3×10 -3 ~5×10 -3 Pa, the smelting times are 5 to 6 times.

[0017] Preferably, in S3, during the heat treatment process, copper tape is wound around the inside and outside of the magnetic core in a spiral shape, and the thickness of a single layer of copper tape is 0.1 to 0.3 mm.

[0018] Beneficial Effects

[0019] The present invention provides a nanocrystalline alloy magnetic core and a preparation process thereof. Compared with the prior art, the present invention has the following beneficial effects:

[0020] (1) The nanocrystalline alloy magnetic core and its preparation process can delay the temperature rise of the inner and outer surfaces of the magnetic core by evenly spirally winding the copper sheet on the inner and outer sides of the magnetic core, reduce the temperature difference between the middle part of the magnetic core and the inner and outer sides, make the temperature distribution between the middle part and the two sides of the magnetic core more uniform, promote more uniform elimination of internal stress, and facilitate simultaneous nucleation and growth at different positions of the magnetic core during the second step annealing, so that the grain size at the inner and outer positions of the magnetic core is more uniform, thereby improving the performance of the magnetic core.

[0021] (2) The nanocrystalline alloy magnetic core and its preparation process increase the insulation between the magnetic core layers by passivating and curing the magnetic core, thereby helping to reduce the loss of the magnetic core and improve the soft magnetic properties of the magnetic core. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 A schematic diagram of copper coating of a nanocrystalline alloy magnetic core provided by the present invention for a nanocrystalline alloy magnetic core and a preparation process thereof;

[0023] Figure 2 A DSC graph of a nanocrystalline alloy magnetic core provided by the present invention for a nanocrystalline alloy magnetic core and its preparation process;

[0024] Figure 3 TEM image of a nanocrystalline alloy magnetic core provided by the present invention and its preparation process;

[0025] Figure 4 A nanocrystalline alloy magnetic core volt-ampere characteristic test provided for a nanocrystalline alloy magnetic core and its preparation process of the present invention;

[0026] Figure 5 Physical properties of a nanocrystalline alloy magnetic core provided by the present invention and its preparation process;

[0027] Figure 6 The invention discloses an AC soft magnetic test of a nanocrystalline alloy magnetic core and a preparation process thereof. DETAILED DESCRIPTION

[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] A nanocrystalline alloy magnetic core and a preparation process thereof, comprising the following preparation steps:

[0031] S1. Preparation of master alloy:

[0032] S11, using 81% pure iron, 1.2% pure copper, 9.3% ferrosilicon and 8.5% ferroboron as raw materials, ultrasonically cleaning the raw materials, removing surface dirt and then drying them;

[0033] S12, then placed under internal pressure of 3×10 -3 Pa vacuum melting furnace, and repeated melting for 5 times to obtain a master alloy with uniform composition distribution;

[0034] S2, winding the master alloy to obtain a magnetic core;

[0035] S3. Vacuum heat treatment is applied to the magnetic core: copper tape is wound around the inside and outside of the magnetic core in a spiral shape, and the thickness of the single-layer copper tape is 0.1 mm. The magnetic core is then placed in a tubular furnace and nitrogen is introduced. The temperature is then raised to 500°C at a rate of 10°C / min, and the temperature is kept for 15 minutes. The temperature is then raised to 540°C at a rate of 1°C / min, and the temperature is kept for 50 minutes. The magnetic core is then taken out of the furnace when the temperature is lowered to 180°C, and a nanocrystalline alloy magnetic core is obtained.

[0036] S4, placing the nanocrystalline alloy core in an iron phosphide passivation solution diluted to 8%, soaking it at room temperature for 100 minutes; then soaking and cleaning it with anhydrous ethanol, and then drying it in a drying oven at a temperature of 50°C for 40 minutes;

[0037] S5. Immerse the passivated nanocrystalline alloy core in the silicone curing agent, then reduce the air pressure to 0.01 MPa, and let it stand until no bubbles emerge from the surface and then restore the atmospheric pressure. Finally, take out the nanocrystalline alloy core and dry it in a drying oven at 9°C for 1.5 hours.

[0038] Example 2

[0039] A nanocrystalline alloy magnetic core and a preparation process thereof, comprising the following preparation steps:

[0040] S1. Preparation of master alloy:

[0041] S11, using 83% pure iron, 1.0% pure copper, 10% ferrosilicon and 6% ferroboron as raw materials, ultrasonically cleaning the raw materials, removing surface dirt and then drying them;

[0042] S12, then placed under an internal pressure of 4×10 -3 Pa vacuum melting furnace, and repeated melting for 6 times to obtain a master alloy with uniform composition distribution;

[0043] S2, winding the master alloy to obtain a magnetic core;

[0044] S3. Vacuum heat treatment is applied to the magnetic core: copper tape is wound around the inside and outside of the magnetic core in a spiral shape, and the thickness of the single-layer copper tape is 0.2 mm. The magnetic core is then placed in a tubular furnace and nitrogen is introduced. The temperature is then raised to 505°C at a rate of 10°C / min, and the temperature is kept for 18 minutes. The temperature is then raised to 545°C at a rate of 1°C / min, and the temperature is kept for 55 minutes. The magnetic core is then taken out of the furnace when the temperature is lowered to 190°C, and a nanocrystalline alloy magnetic core is obtained.

[0045] S4, placing the nanocrystalline alloy core in an iron phosphide passivation solution diluted to 8%, soaking it at room temperature for 110 minutes; then soaking and cleaning it with anhydrous ethanol, and then drying it in a drying oven at a temperature of 55°C for 50 minutes;

[0046] S5. Immerse the passivated nanocrystalline alloy core in the silicone curing agent, then reduce the air pressure to 0.02MPa, and let it stand until no bubbles emerge from the surface and then restore the atmospheric pressure. Finally, take out the nanocrystalline alloy core and dry it in a drying oven at 95°C for 2h.

[0047] Example 3

[0048] A nanocrystalline alloy magnetic core and a preparation process thereof, comprising the following preparation steps:

[0049] S1. Preparation of master alloy:

[0050] S11, using 85% pure iron, 0.8% pure copper, 8.7% ferrosilicon and 5.5% ferroboron as raw materials, ultrasonically cleaning the raw materials, removing surface dirt and then drying them;

[0051] S12, then placed under an internal pressure of 5×10 -3 Pa vacuum melting furnace, and repeated melting for 6 times to obtain a master alloy with uniform composition distribution;

[0052] S2, winding the master alloy to obtain a magnetic core;

[0053] S3. Vacuum heat treatment is applied to the magnetic core: copper tape is wound around the inside and outside of the magnetic core in a spiral shape, and the thickness of the single-layer copper tape is 0.3 mm. The magnetic core is then placed in a tubular furnace and nitrogen is introduced. The temperature is then raised to 510°C at a rate of 10°C / min, and the temperature is kept for 20 minutes. The temperature is then raised to 550°C at a rate of 1°C / min, and the temperature is kept for 60 minutes. The magnetic core is then taken out of the furnace when the temperature drops to 200°C, and a nanocrystalline alloy magnetic core is obtained.

[0054] S4, placing the nanocrystalline alloy core in an iron phosphide passivation solution diluted to 8%, soaking it at room temperature for 120 minutes; then soaking and cleaning it with anhydrous ethanol, and then drying it in a drying oven at a temperature of 60°C for 60 minutes;

[0055] S5. Immerse the passivated nanocrystalline alloy core in the polyurethane curing agent, then reduce the air pressure to 0.03 MPa, and let it stand until no bubbles emerge from the surface and then restore the atmospheric pressure. Finally, take out the nanocrystalline alloy core and dry it in a drying oven at 100°C for 2 hours.

[0056] Comparative Example 1

[0057] A nanocrystalline alloy magnetic core and a preparation process thereof, comprising the following preparation steps:

[0058] S1. Preparation of master alloy:

[0059] S11, using 81% pure iron, 1.2% pure copper, 9.3% ferrosilicon and 8.5% ferroboron as raw materials, ultrasonically cleaning the raw materials, removing surface dirt and then drying them;

[0060] S12, then placed under internal pressure of 3×10 -3 Pa vacuum melting furnace, and repeated melting for 5 times to obtain a master alloy with uniform composition distribution;

[0061] S2, winding the master alloy to obtain a magnetic core;

[0062] S3. Vacuum heat treatment is applied to the magnetic core: the magnetic core is placed in a tubular furnace and nitrogen is introduced, then the temperature is raised to 500°C at a rate of 10°C / min, and the temperature is kept for 15 minutes, then the temperature is raised to 540°C at a rate of 1°C / min, and the temperature is kept for 50 minutes, and the core is removed from the furnace when the temperature is lowered to 180°C to obtain a nanocrystalline alloy magnetic core.

[0063] Test of the volt-ampere characteristics of the magnetic core: This paper uses Shanghai Hengtong HT35 core measuring instrument to measure the volt-ampere characteristics of the annealed magnetic core, that is, the U-1 curve; the experimental parameters are: power frequency 50Hz, single-turn AC magnetization, specific operation method: start the machine and preheat for 5 minutes, adjust the measuring instrument range according to the size of the magnetic core, then put the magnetic core with the protective box directly on the core measuring instrument, adjust the current value, and record the output electromotive force U.

[0064] Thermal stability analysis: NETZSCH-C404 differential scanning calorimeter (DSC) was used for analysis. The specific experimental parameters were: heating rate of 0.60°C / S, Pt crucible, sample weight of 10-20 mg, temperature measurement range of 500-1050K, and experimental conditions: vacuum argon.

[0065] like Figure 2 As shown in the figure, with the increase of temperature, two exothermic peaks appeared, corresponding to two different crystallization processes. The first crystallization peak corresponds to the a-Fe(Si) phase. The precipitation of the a-Fe(Si) phase is beneficial to improving the soft magnetic properties of the strip. The second crystallization exothermic peak corresponds to the secondary phase Fe2B phase. The precipitation of Fe2B will transform ferromagnetism into paramagnetism, destroy the spontaneous magnetic properties, and reduce the magnetic properties. Figure 2 Medium T X1 The first crystallization begins, and the soft magnetic phase precipitates. p1 The first exothermic peak appears at T, and the crystallization rate reaches its maximum value, after which the grain growth is the main process; x2 The second crystallization begins at T and the secondary phase Fe2B phase precipitates. X1 To T x2 In this wide temperature range, only the ferromagnetic phase is precipitated, ensuring that an amorphous-nanocrystalline dual-phase structure is formed after heat treatment, and no secondary phase is precipitated. Therefore, during heat treatment, the temperature must not exceed T x2( 973K).

[0066] like Figure 3 As shown, the average size of the precipitated grains on the free surface is larger than that on the roller surface. Compared with Comparative Example 1, the copper-clad auxiliary annealing in Example 1 helps to reduce the size of the precipitated grains and improve the uniformity, which is beneficial to improving the uniformity of the grains on the free surface and the roller surface.

[0067] like Figure 4 As shown, compared with Comparative Example 1, the induced potential of Examples 1-3 is significantly improved under different excitation currents.

[0068] like Figure 5 As shown, compared with Examples 1-3, the oxidation color of Comparative Example 1 is deepened and the degree of oxidation is serious, resulting in continuous deterioration of the magnetic properties; the brittleness test θ range is continuously reduced, that is, the better the toughness of the magnetic core, the less the magnetic core is affected by external forces, and the more stable the performance.

[0069] like Figure 6 As shown, compared with Comparative Example 1, the loss of Examples 1-3 is as low as 0.04KW / m 3 , the saturation magnetic permeability and coercivity are significantly improved.

[0070] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.

[0071] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0072] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A nanocrystalline alloy magnetic core, characterized in that: The invention is made of the following components in percentage by weight: 81% to 85% of pure iron, 0.8% to 1.2% of pure copper, 8% to 10% of ferrosilicon and 5.5% to 8.5% of ferroboron.

2. A process for preparing a nanocrystalline alloy magnetic core according to claim 1, characterized in that: The method comprises the following preparation steps: S1. Preparation of master alloy: S11, using pure iron, pure copper, ferrosilicon and ferroboron as raw materials, ultrasonically cleaning the raw materials to remove surface dirt and then drying them; S12, then placing it in a vacuum melting furnace and repeatedly melting it to obtain a master alloy with uniform composition distribution; S2, winding the master alloy to obtain a magnetic core; S3. Vacuum heat treatment is applied to the magnetic core: the magnetic core is placed in a tubular furnace and nitrogen is introduced, then the temperature is raised to 500-510°C at a rate of 10°C / min, and the temperature is kept at that temperature for 15-20 minutes, and then the temperature is raised to 540-550°C at a rate of 1°C / min, and the temperature is kept at that temperature for 50-60 minutes, and the core is taken out of the furnace when the temperature is lowered to 180-200°C to obtain a nanocrystalline alloy magnetic core.

3. The process for preparing a nanocrystalline alloy magnetic core according to claim 1, wherein: The preparation process of the nanocrystalline alloy magnetic core also includes: S4, placing the nanocrystalline alloy magnetic core in a passivation solution and soaking it at room temperature for 100-120 minutes; then soaking and cleaning it with anhydrous ethanol, and then placing it in a drying oven at a temperature of 50-60°C for drying for 40-60 minutes.

4. The process for preparing a nanocrystalline alloy magnetic core according to claim 3, wherein: The passivation solution is an iron-based phosphide passivation solution, and is diluted to an 8% solution before use.

5. The process for preparing a nanocrystalline alloy magnetic core according to claim 3, wherein: The preparation process of the nanocrystalline alloy magnetic core also includes: S5, placing the passivated nanocrystalline alloy magnetic core in a curing agent for immersion, then pumping the air pressure to 0.01-0.03 MPa, standing until no bubbles emerge on the surface and then restoring the atmospheric pressure, finally taking out the nanocrystalline alloy magnetic core and placing it in a drying oven at 90-100°C for drying for 1.5-2 hours.

6. The process for preparing a nanocrystalline alloy magnetic core according to claim 5, characterized in that: The curing agent is any one selected from silicone curing agents and polyurethane curing agents.

7. The process for preparing a nanocrystalline alloy magnetic core according to claim 1, wherein: In S12, the internal pressure of the vacuum melting furnace is 3×10 -3 ~5×10 -3 Pa, the smelting times are 5 to 6 times.

8. The process for preparing a nanocrystalline alloy magnetic core according to claim 1, wherein: In S3, during the heat treatment process, the magnetic core is wound with copper tape inside and outside, and the winding is spiral, and the thickness of a single layer of copper tape is 0.1 to 0.3 mm.

Citation Information

Patent Citations

  • Fe-based amorphous nanocrystalline soft magnetic alloy material and preparation method thereof

    CN102953020A

  • Preparation and coating method of high-performance iron-based amorphous metal powder core

    CN103065789A

  • Preparation method of amorphous soft-magnetic composite material

    CN104032241A

  • Nanogold alloy and manufacturing method thereof

    CN104726800A

  • Iron-based micro-nano magnetic powder material and preparation method thereof