Processing and manufacturing method of wafer with deep hole structure and wafer
By using low-speed spin-coated photoresist in the deep-pore zone structure of the wafer, baking and curing, and then rotating and cleaning at high speed, the photoresist escape problem is solved, and the film retention rate and light of the photoresist are improved Accuracy and quality of the engraving process.
Patent Information
- Application Number
- CN202411032181.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
AI Technical Summary
The existing wafer preparation methods are prone to escape of photoresist when coating photoresist, resulting in poor uniformity of photoresist coating in deep pore structures, affecting the accuracy and quality of the photoresist process in subsequent processes.
The photoresist is coated in the center of the deep pore area structure of the wafer with a lower speed, and baked to cure it into a film, and then the edge is cleaned at the second rotation speed at a higher speed, reducing light The centrifugal force and escape of resist improve the membrane retention rate of photoresist.
By reducing the spin coating speed and performing high-speed cleaning after curing and forming the film, the filling effect of the photoresist in the deep-hole area structure is improved, the accuracy and quality of the photoresist process are improved, and the photoresist escape phenomenon is reduced.
Smart Images

Figure CN118943008A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present invention relate to the field of semiconductor technology, and in particular to a method for processing and manufacturing a wafer with a deep hole structure and a wafer. Background Art
[0002] With the development of semiconductor technology, people have higher and higher requirements for semiconductor devices. When preparing existing semiconductor devices, they generally need to be made on a wafer and then cut into independent semiconductor devices.
[0003] In the existing wafer preparation method, when coating the photoresist, the photoresist is prone to escape, resulting in poor uniformity of photoresist coating on wafers including deep hole structures, affecting the accuracy and quality of the photolithography process of subsequent processes. Summary of the invention
[0004] The embodiment of the present invention provides a method for processing and manufacturing a wafer with a deep hole structure and a wafer, so as to solve the problem that the photoresist coated in the deep hole structure of the wafer manufactured by the existing wafer processing and manufacturing method is not uniform enough.
[0005] In order to achieve the above technical problems, the present invention adopts the following technical solutions:
[0006] An embodiment of the present invention provides a wafer processing and manufacturing method, comprising:
[0007] Providing a wafer, and forming a deep hole region structure on the surface of the wafer;
[0008] Using a first rotation speed, coating a photoresist on the center of the wafer having the deep hole region structure;
[0009] Baking the wafer to solidify the photoresist into a film;
[0010] The edge of the wafer is cleaned using a second rotation speed; wherein the first rotation speed is less than the second rotation speed.
[0011] Optionally, providing a wafer and forming a deep hole region structure on a surface of the wafer includes:
[0012] Providing wafer substrates;
[0013] At least two device units are arranged on the surface of the wafer substrate, and a deep cutting path is formed between two adjacent device units;
[0014] A passivation layer is formed on the device unit, the passivation layer covers the deep cut road, and the deep cut road is covered by the passivation layer to form the deep hole region structure.
[0015] Optionally, the aspect ratio of the deep hole region structure is less than or equal to 1:5;
[0016] The depth of the deep hole structure is greater than or equal to 10 μm;
[0017] The width of the deep hole region structure ranges from 50 μm to 80 μm.
[0018] Optionally, the step of coating the photoresist at the center of the wafer having the deep hole region structure at the first rotation speed includes:
[0019] Pre-wetting the surface of the wafer having the deep hole area structure;
[0020] The wafer is rotated at the first rotation speed, and a photoresist is spin-coated on the surface of the wafer having the center of the deep hole region structure, so as to fill the deep hole region structure with the photoresist.
[0021] Optionally, pre-wetting the surface of the wafer having the deep hole region structure includes:
[0022] The wafer is rotated at a third rotation speed, and photoresist is coated on the surface of the wafer so that the photoresist uniformly infiltrates the wafer; wherein the third rotation speed is lower than the first rotation speed.
[0023] Optionally, the first rotation speed is greater than or equal to 400 rpm and less than or equal to 650 rpm;
[0024] The second rotation speed is greater than or equal to 1800 rpm and less than or equal to 2200 rpm.
[0025] Optionally, baking the wafer to solidify the photoresist into a film includes:
[0026] The wafer is soft-baked to volatilize the solvent in the photoresist and solidify the resin in the photoresist into a film; wherein the temperature of the soft-baking is greater than or equal to 80° C. and less than or equal to 120° C.
[0027] Optionally, the step of performing edge cleaning on the wafer using a second rotation speed includes:
[0028] Infiltrating the edge area and the back side of the wafer with an organic solvent;
[0029] The wafer is rotated at the second rotation speed, and an organic solvent is sprayed on the edge region and the back side of the wafer to perform edge and back cleaning on the wafer.
[0030] Optionally, the organic solvent used for edge washing includes propylene glycol methyl ether and propylene glycol methyl ether acetate;
[0031] The width of the edge area is greater than or equal to 2 mm and less than or equal to 5 mm.
[0032] According to another aspect of the present invention, this embodiment provides a wafer, including:
[0033] The deep hole area structure is arranged on the surface of the wafer;
[0034] A cured photoresist layer is provided in the deep hole area structure, and the photoresist layer is formed by the wafer processing and manufacturing method proposed in any item of the first aspect.
[0035] The wafer processing and manufacturing method provided by the embodiment of the present invention adopts a first rotation speed with a lower speed to coat photoresist at the center of the surface of the wafer having the deep hole area structure, and then bakes the wafer to solidify the photoresist into a film, and then adopts a second rotation speed with a higher speed to clean the wafer. Compared with the conventional wafer coating photoresist film forming process, the spin coating rotation speed adopted is higher, and the conventional process combines the wafer edge washing / back washing process in the step of coating, and finally bakes the wafer to form a film. The existing wafer preparation process is easy to cause the photoresist to suffer a large centrifugal force in the spin coating rotation speed for the wafer with the deep hole area structure, and escape from the deep hole area structure, resulting in poor filling effect of the photoresist in the deep hole area structure. The wafer processing and manufacturing method provided by this embodiment adopts a first rotation speed with a lower speed to spin coat the photoresist, so that the centrifugal force borne by the photoresist in the deep hole area structure is reduced, while taking into account the coating uniformity, reducing the escape of the photoresist from the deep hole area structure, thereby improving the film retention rate of the photoresist in the deep hole area structure. In addition, since the wafer side / back washing must be performed at a higher second rotation speed, the present application ingeniously bakes the wafer to solidify the photoresist into a film, and then uses a higher second rotation speed to clean the wafer. This arrangement better improves the filling effect of the photoresist in the deep hole area structure of the wafer, thereby improving the accuracy and quality of the photolithography process. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments of the present invention. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the contents of the embodiments of the present invention and these drawings without paying any creative work.
[0037] Figure 1 It is a flow chart of a wafer processing and manufacturing method provided by an embodiment of the present invention;
[0038] Figure 2 is a flow chart of another wafer processing and manufacturing method provided by an embodiment of the present invention;
[0039] Figure 3 It is a structural schematic diagram of a wafer produced by a wafer processing and manufacturing method in the prior art;
[0040] Figure 4 It is a structural schematic diagram of a wafer provided by an embodiment of the present invention. DETAILED DESCRIPTION
[0041] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention. It should also be noted that, for ease of description, only parts related to the present invention, rather than all structures, are shown in the accompanying drawings.
[0042] Based on the above technical problems, this embodiment proposes the following solutions:
[0043] Figure 1 1 is a flow chart of a wafer processing and manufacturing method provided by an embodiment of the present invention. Figure 1 The wafer manufacturing method provided by the embodiment of the present invention includes:
[0044] S101, providing a wafer, and forming a deep hole region structure on the surface of the wafer.
[0045] Specifically, a device unit may be arranged on the wafer. The device unit may include at least one film layer. Between the film layers of the device unit, a deep hole area structure may be formed on the wafer surface. The deep hole area structure refers to a hole with a relatively deep depth, which penetrates at least two film layers. When the film layer thickness is relatively thick, the depth of the formed deep hole area structure may be relatively deep. When the deep hole area structure is coated with photoresist, there may be pit positions, resulting in poor uniformity of the surface of the photoresist.
[0046] S102 , using a first rotation speed to coat photoresist at the center of the wafer having the deep hole region structure.
[0047] Specifically, the first rotation speed can be set to be a rotation speed with a lower speed. The first rotation speed with a lower rotation speed is adopted, so that when the photoresist is applied to the center of the wafer, it is convenient to evenly apply the photoresist to the surface of the wafer with the deep hole area structure. Applying the photoresist to the center of the wafer means applying the photoresist to the central area of the wafer or an area close to the center. Since the first rotation speed is slow, the photoresist in the deep hole area structure is not easy to escape during the rotation process, thereby improving the film retention rate of the photoresist in the deep hole area structure.
[0048] S103, baking the wafer to solidify the photoresist into a film.
[0049] Specifically, the wafer is baked to evaporate a portion of the solvent in the photoresist, and the photoresist is solidified into a film, thereby increasing the adhesion between the photoresist and the wafer surface.
[0050] S104, using a second rotation speed to clean the edge of the wafer; wherein the first rotation speed is lower than the second rotation speed.
[0051] Specifically, the second rotation speed is greater than the first rotation speed. The second rotation speed with a higher rotation speed is used to perform edge cleaning of the wafer, such as edge cleaning and back cleaning. Since the second rotation speed is higher, it is convenient to clean the photoresist on the edge and back of the wafer, thereby improving the cleaning efficiency. In addition, by arranging the cleaning of the wafer after the baking process of the wafer, the photoresist located in the deep hole area structure can be solidified into a film, and even if the second rotation speed for cleaning the wafer is higher, the film retention rate in the deep hole area structure can be increased, thereby further improving the filling effect of the photoresist in the deep hole area structure.
[0052] The existing wafer preparation process is prone to cause the photoresist to be subjected to a large centrifugal force during the spin coating speed for wafers with deep hole area structures, causing the photoresist to escape from the deep hole area structure, resulting in poor filling effect of the photoresist in the deep hole area structure.
[0053] The wafer manufacturing method provided in this embodiment adopts a first rotation speed with a relatively low speed to coat photoresist at the center of the surface of the side of the wafer having the deep hole area structure, and then bakes the wafer to solidify the photoresist into a film, and then adopts a second rotation speed with a relatively high speed to clean the wafer. Compared with the conventional wafer coating photoresist film forming process, the spin coating rotation speed is relatively high, and the conventional process combines the wafer edge washing / back washing process in the glue coating step, and finally the wafer is baked to form a film.
[0054] The manufacturing method of the wafer provided by the present embodiment adopts the first rotational speed with lower speed to carry out the spin coating of photoresist, so that the centrifugal force that the photoresist in the deep hole area structure bears is reduced, while taking into account the coating uniformity, the photoresist is reduced to escape from the deep hole area structure, thereby improving the film retention rate of the photoresist in the deep hole area structure. In addition, because the wafer edge washing / back washing must be cleaned with a higher second rotational speed, the application is cleverly baked by setting the wafer, the photoresist is cured into a film, and then the higher second rotational speed is adopted to clean the wafer. Such arrangement preferably improves the filling effect of the photoresist in the deep hole area structure of the wafer, thereby improving the precision and quality of the photolithography process.
[0055] Optional, Figure 2FIG. 1 is a flow chart of another wafer processing and manufacturing method provided by an embodiment of the present invention. Figure 2 The wafer manufacturing method provided by the embodiment of the present invention includes:
[0056] S201. Provide a wafer substrate.
[0057] Specifically, the wafer substrate may include, for example, a silicon substrate, a sapphire substrate or a glass substrate.
[0058] S202, setting at least two device units on the surface of the wafer substrate, and forming a deep cutting path between two adjacent device units.
[0059] Specifically, the wafer may include at least two device units, such as gallium nitride devices, etc. A deep cut may be provided between adjacent device units. A deep cut refers to a cut that separates at least two device units to form an independent device unit and penetrates at least two film layers. The deep cut is used to cut each device unit after wafer fabrication is completed, so as to protect the yield of the device unit cutting.
[0060] S203, forming a passivation layer on the device unit, wherein the passivation layer covers the deep cut road, and the deep cut road is covered by the passivation layer to form the deep hole region structure.
[0061] Specifically, the device unit may include a passivation layer, and at the deep cut position, the wafer will still form a deep hole region structure after being covered by the passivation layer. When the thickness of the passivation layer is thick, the depth of the deep hole region structure formed at the deep cut position will be deeper. When the photoresist is applied to the deep hole region structure with a deep depth, there is a pit position, resulting in poor uniformity of the surface of the photoresist.
[0062] S102 , using a first rotation speed to coat photoresist at the center of the wafer having the deep hole region structure.
[0063] S103, baking the wafer to solidify the photoresist into a film.
[0064] S104, using a second rotation speed to clean the edge of the wafer; wherein the first rotation speed is lower than the second rotation speed.
[0065] The wafer processing and manufacturing method provided in this embodiment adopts a first rotation speed with a relatively low speed to spin-coat the photoresist, so that the centrifugal force of the photoresist in the deep hole area structure with a relatively deep depth formed by the passivation layer is reduced, and while taking into account the coating uniformity, the photoresist is reduced from escaping from the deep hole area structure, thereby improving the film retention rate of the photoresist in the deep hole area structure formed by the passivation layer. In addition, by setting the wafer to be baked, the photoresist is solidified into a film, and then the wafer is cleaned by adopting a second rotation speed with a relatively high speed, the filling effect of the photoresist layer in the deep hole area structure formed by the passivation layer of the wafer is better improved, thereby further improving the accuracy and quality of the photolithography process.
[0066] Optionally, based on the above embodiment, continue to refer to Figure 2 The aspect ratio of the deep hole region structure is less than or equal to 1:5; the depth of the deep hole region structure is greater than or equal to 10 μm; and the width range of the deep hole region structure includes 50 μm to 80 μm.
[0067] Specifically, when the aspect ratio of the deep hole area structure is less than or equal to 1:5, the depth of the deep hole area structure is deeper, which easily leads to the problem of low film retention rate of the photoresist. When the aspect ratio of the deep hole area structure of the wafer is less than or equal to 1:5, the depth of the deep hole area structure is greater than or equal to 10μm, and the width range of the deep hole area structure includes 50μm to 80μm, the wafer preparation method provided in this embodiment can better improve the filling effect of the photoresist layer in the deep hole area structure of the wafer, further improve the accuracy and quality of the photolithography process, and reduce the failure rate of the photolithography exposure alignment signal acquisition.
[0068] Optionally, based on the above embodiment, continue to refer to Figure 2 , the step of coating the photoresist at the center of the wafer having the deep hole area structure with the first rotation speed may include: pre-wetting the surface of the wafer having the deep hole area structure; rotating the wafer at the first rotation speed, and spin coating the photoresist on the surface of the wafer having the deep hole area structure at the center to fill the deep hole area structure with the photoresist.
[0069] Specifically, the surface of the wafer having the deep hole area structure is pre-wetted. Since the initial spin coating speed is slow, the photoresist can be pre-wetted more evenly, which can better improve the spin coating effect of the photoresist.
[0070] Optionally, based on the above embodiment, continue to refer to Figure 2 The pre-wetting of the surface of the wafer having the deep hole area structure may include: rotating the wafer at a third rotation speed, coating photoresist on the surface of the wafer, and allowing the photoresist to uniformly wet the wafer; wherein the third rotation speed is less than the first rotation speed.
[0071] Specifically, the third rotation speed is lower than the first rotation speed. Rotating the wafer at the low third rotation speed can make the photoresist more uniformly infiltrate the wafer and the deep hole area structure.
[0072] After the wafer is pre-moistened, the photoresist is applied at a first rotation speed so that the wafer surface is fully covered with the photoresist to achieve initial film formation of the photoresist. During the photoresist coating stage, the rotation speed is greatly reduced, and it is necessary to ensure that the photoresist is evenly coated.
[0073] This arrangement, by reducing the main rotation speed of the photoresist spin coating once and separating the wafer edge washing process with a high rotation speed to after the photoresist baking, greatly reduces the centrifugal force exerted on the photoresist during the spin coating stage, thereby weakening the escape ability of the wet photoresist in the deep hole area structure, and effectively improving the film retention rate of the photoresist in the deep hole area structure.
[0074] Optionally, based on the above embodiment, the first rotation speed can be set to be greater than or equal to 400 rpm and less than or equal to 650 rpm; the second rotation speed can be set to be greater than or equal to 1800 rpm and less than or equal to 2200 rpm.
[0075] Specifically, such a configuration can significantly reduce the rotation speed of the wafer during the photoresist coating stage, thereby preventing the photoresist from escaping from the deep hole structure and ensuring uniform photoresist coating, and can also clean the edge area of the wafer and the back of the wafer.
[0076] Optionally, based on the above embodiment, the baking of the wafer to solidify the photoresist into a film may include: soft baking the wafer to volatilize the solvent in the photoresist and solidify the resin in the photoresist into a film; wherein the temperature of the soft baking is greater than or equal to 80°C and less than or equal to 120°C.
[0077] Specifically, a part of the solvent in the photoresist is evaporated by soft baking. The wafer coated with photoresist can be placed in a soft baking chamber at a temperature of 80-120°C and left to stand for a certain period of time. The solvent in the photoresist film can be evaporated to less than 10%, increasing the adhesion of the photoresist and releasing the stress in the photoresist film to prevent the photoresist film from cracking. Soft baking methods include conduction, convection and radiation.
[0078] Optionally, based on the above embodiment, the edge cleaning of the wafer using a second rotation speed may include: infiltrating the edge area and the back side of the wafer with an organic solvent; rotating the wafer using the second rotation speed, spraying the organic solvent on the edge area and the back side of the wafer, and washing the edges and the back of the wafer.
[0079] Specifically, the wafer is rotated at a second higher rotation speed, and an organic solvent is sprayed on the edge area and back of the wafer. The organic solvent is sprayed while the wafer is rotated to wash the edge and back of the wafer, thereby saving time for washing the edge and back of the wafer and improving the cleaning efficiency of the wafer.
[0080] Optionally, the organic solvent used for edge washing may include propylene glycol methyl ether (PGME) and propylene glycol methyl ether acetate (PGMEA). Optionally, propylene glycol methyl ether / propylene glycol methyl ether acetate=7:3 may be set. Optionally, the width of the edge area of the wafer is greater than or equal to 2 mm and less than or equal to 5 mm.
[0081] Specifically, such an arrangement facilitates cleaning the edge and back of the wafer and improves the cleaning efficiency. This embodiment advances the step of soft-baking the photoresist and separates the wafer edge / back washing process. The photoresist on the wafer surface and in the deep hole area structure is preferentially baked and cured to form a film, and then the wafer is washed at a high speed edge / back to prevent the liquid photoresist in the deep hole from escaping, further improving the filling effect of the photoresist in the deep hole area structure of the wafer, further improving the precision and quality of the photolithography process on the wafer surface, especially at the corresponding position of the deep hole area structure, and further reducing the failure rate when acquiring the photolithography exposure alignment signal.
[0082] This embodiment provides a wafer. Figure 3 It is a structural schematic diagram of a wafer produced by a wafer processing and manufacturing method in the prior art. Figure 4 Schematic diagram of the structure of a wafer provided by an embodiment of the present invention. Figure 4 The wafer provided in this embodiment may include: a deep hole area structure 1, which is arranged on the surface of the wafer; a cured photoresist layer 2 is arranged in the deep hole area structure 1, and the photoresist layer 2 is formed by the wafer processing and manufacturing method proposed in any of the above embodiments.
[0083] For details, see Figure 3 The existing wafer preparation process makes it easy for the photoresist 2 to be subjected to a large centrifugal force during the spin coating speed for the wafer with a deep hole area structure 1, and escape from the deep hole area structure 1, resulting in poor filling effect of the photoresist 2 in the deep hole area structure 1, the presence of deeper pits, and the low flatness of the photoresist 2 and poor uniformity of the photoresist 2.
[0084] See also Figure 4The photoresist 2 in the deep hole area structure 1 of the wafer provided in this embodiment is spin-coated at a first relatively low rotation speed, so that the centrifugal force borne by the photoresist 2 in the deep hole area structure 1 is reduced. While taking into account the coating uniformity, the escape of the photoresist 2 from the deep hole area structure 1 is reduced, thereby improving the film retention rate of the photoresist 2 in the deep hole area structure 1.
[0085] In addition, since the wafer side / back cleaning must be performed at a higher second rotation speed, the wafer is first baked to solidify the photoresist 2 into a film, and then the wafer is cleaned at a higher second rotation speed. This arrangement improves the filling effect of the photoresist 2 in the deep hole area structure 1 of the wafer, thereby improving the accuracy and quality of the photolithography process, and further improving the yield of the wafer.
[0086] Note that the above are only preferred embodiments of the present invention and the technical principles used. Those skilled in the art will understand that the present invention is not limited to the specific embodiments described herein, and that various obvious changes, readjustments and substitutions can be made by those skilled in the art without departing from the scope of protection of the present invention. Therefore, although the present invention has been described in more detail through the above embodiments, the present invention is not limited to the above embodiments, and may include more other equivalent embodiments without departing from the concept of the present invention, and the scope of the present invention is determined by the scope of the appended claims.
Claims
1. A wafer processing and manufacturing method, characterized in that: include: Providing a wafer, and forming a deep hole region structure on the surface of the wafer; Using a first rotation speed, coating a photoresist on the center of the wafer having the deep hole region structure; Baking the wafer to solidify the photoresist into a film; The edge of the wafer is cleaned using a second rotation speed; wherein the first rotation speed is less than the second rotation speed.
2. The method according to claim 1, characterized in that The step of providing a wafer and forming a deep hole region structure on the surface of the wafer comprises: Providing wafer substrates; At least two device units are arranged on the surface of the wafer substrate, and a deep cutting path is formed between two adjacent device units; A passivation layer is formed on the device unit, the passivation layer covers the deep cut road, and the deep cut road is covered by the passivation layer to form the deep hole region structure.
3. The method according to claim 1, characterized in that The aspect ratio of the deep hole region structure is less than or equal to 1:5; The depth of the deep hole structure is greater than or equal to 10 μm; The width of the deep hole region structure ranges from 50 μm to 80 μm.
4. The method according to claim 1, characterized in that: The method of coating the photoresist at the center of the wafer having the deep hole region structure by using the first rotation speed comprises: Pre-wetting the surface of the wafer having the deep hole area structure; The wafer is rotated at the first rotation speed, and photoresist is spin-coated on the surface of the wafer having the center of the deep hole region structure, so as to fill the deep hole region structure with the photoresist.
5. The method according to claim 4, characterized in that The pre-wetting of the surface of the wafer having the deep hole area structure comprises: The wafer is rotated at a third rotation speed, and photoresist is coated on the surface of the wafer so that the photoresist uniformly infiltrates the wafer; wherein the third rotation speed is lower than the first rotation speed.
6. The method according to any one of claims 1 to 5, characterized in that: The first rotation speed is greater than or equal to 400 rpm and less than or equal to 650 rpm; The second rotation speed is greater than or equal to 1800 rpm and less than or equal to 2200 rpm.
7. The method according to claim 1, characterized in that The step of baking the wafer to solidify the photoresist into a film comprises: The wafer is soft-baked to volatilize the solvent in the photoresist and solidify the resin in the photoresist into a film; wherein the temperature of the soft-baking is greater than or equal to 80° C. and less than or equal to 120° C.
8. The method according to claim 1 or 7, characterized in that: The step of using the second rotation speed to clean the edge of the wafer comprises: Infiltrating the edge area and the back side of the wafer with an organic solvent; The wafer is rotated at the second rotation speed, and an organic solvent is sprayed on the edge area and the back side of the wafer to perform edge cleaning and back cleaning on the wafer.
9. The method according to claim 8, characterized in that The organic solvent used in the edge washing includes propylene glycol methyl ether and propylene glycol methyl ether acetate; The width of the edge area is greater than or equal to 2 mm and less than or equal to 5 mm.
10. A wafer, characterized in that: include: The deep hole area structure is arranged on the surface of the wafer; A cured photoresist layer is provided in the deep hole region structure, and the photoresist layer is formed by the wafer processing and manufacturing method according to any one of claims 1 to 9.