Quantum dot-graphene detector and preparation method thereof

By introducing a nickel oxide layer and a quantum dot film into the graphene detector, combining the heterojunction structure of PbS quantum dots and graphene, the problem of dark current and low responsiveness of the graphene detector is solved, and high gain and Quick response effect.

CN118943208APending Publication Date: 2024-11-12INST OF SEMICONDUCTORS - CHINESE ACAD OF SCI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310517673.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional graphene detectors have problems with high dark current and low responsiveness, resulting in high power consumption and low response.

Method used

The structural design of the quantum dot-graphene detector is adopted, and the nickel oxide layer and quantum dot film are formed on the graphene layer, and the dark current is reduced by using the barrier effect of the nickel oxide layer, and PbS quantum dots are used as the main light absorbing material. Graphene acts as a carrier transport layer, forming the characteristics of high gain and fast response.

Benefits of technology

It effectively reduces the dark current of the graphene detector, while achieving high gain and fast response, partially solving the dark current and low responsiveness problems of the graphene detector.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943208A_ABST
    Figure CN118943208A_ABST
Patent Text Reader

Abstract

The invention provides a quantum dot-graphene detector and a preparation method thereof, and is applied to the technical field of semiconductors, and the method comprises the steps: carrying out the evaporation of a metal bottom electrode on one side of an oxidized silicon wafer substrate through a negative photoresist photoetching technology; sputtering a nickel oxide layer on the metal bottom electrode through a negative photoresist photoetching process; transferring a single graphene layer on the nickel oxide layer; patterning the graphene layer through a positive photoresist photoetching process and oxygen plasma etching to enable the graphene layer to cover part of the surface of the nickel oxide layer and the surface of the other side of the silicon oxide substrate; evaporating a metal top electrode on the graphene layer through a negative photoresist photoetching process to obtain a prepared detector; and spin-coating a quantum dot film on the upper surface of the prepared detector. And the graphene dark current can be inhibited.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of semiconductor technology, and in particular to a quantum dot-graphene detector and a preparation method thereof. Background Art

[0002] As a classic two-dimensional material, graphene has attracted widespread attention since its discovery. Graphene's ultra-high carrier mobility and zero-bandgap semiconductor material have led to extensive research in optics and electronics. In theory, graphene's zero-bandgap structure can absorb electromagnetic waves of any wavelength, making it an ideal wide-spectrum absorption material. In addition, graphene has an extremely high carrier mobility (~2×10 5 cm 2 V -1 s -1 ). Broadband absorption, ultrahigh carrier mobility, and ultrafast response make graphene an ideal optoelectronic material. However, the defects of single-layer graphene are also obvious. The absorbance of single-layer graphene is only 2.3%. Due to the lack of a band gap, graphene-based devices cannot achieve switching characteristics and have extremely high dark current, resulting in high power consumption of graphene devices.

[0003] At present, most of the methods to solve the large dark current of graphene detectors are to use heterojunction structures, such as heterojunction detectors with two-dimensional materials such as molybdenum disulfide, and heterojunction detectors with bulk materials such as silicon and germanium. These heterojunction structures can effectively reduce the dark current of graphene, but such devices have no gain mechanism, resulting in low detector response. Another method is to make graphene nanostrips to open the band gap of graphene, but this method limits the active area of ​​the detector. Summary of the invention

[0004] The main purpose of the present disclosure is to provide a quantum dot-graphene detector and a preparation method thereof, aiming to at least partially solve the technical problems of large dark current and low responsivity of traditional graphene detectors.

[0005] To achieve the above-mentioned purpose, the first aspect of the present disclosure provides a method for preparing a quantum dot-graphene detector, comprising:

[0006] A metal bottom electrode is evaporated on one side of the oxide silicon wafer substrate by a negative photolithography process;

[0007] sputtering a nickel oxide layer on the metal bottom electrode by a negative photolithography process;

[0008] transferring a single layer of graphene on the nickel oxide layer;

[0009] Patterning the graphene layer by positive photolithography and oxygen plasma etching, so that the graphene layer covers a portion of the surface of the nickel oxide layer and the surface of the other side of the silicon oxide substrate;

[0010] Vapor-depositing a metal top electrode on the graphene layer by a negative resist photolithography process to obtain a preliminary detector;

[0011] A quantum dot film is spin-coated on the upper surface of the prepared detector.

[0012] In one embodiment of the present disclosure, transferring a single-layer graphene layer on the nickel oxide layer comprises:

[0013] A single-layer graphene layer is transferred onto the nickel oxide layer by wet transfer.

[0014] In one embodiment of the present disclosure, during the growth process of the quantum dot film, oleic acid is used as a quantum dot ligand reagent.

[0015] In one embodiment of the present disclosure, the sputtering of a nickel oxide layer on the metal bottom electrode comprises:

[0016] A nickel target material with a radio frequency sputtering purity of 99.99% is used to sputter a nickel oxide layer on the metal bottom electrode in an atmosphere of oxygen and argon.

[0017] In one embodiment of the present disclosure, the spin coating of the quantum dot film on the upper surface of the prepared detector comprises:

[0018] A lead sulfide quantum dot film is spin-coated on the upper surface of the prepared detector by using a hot injection method and a layer-by-layer self-assembly method.

[0019] In one embodiment of the present disclosure, the layer-by-layer self-assembly method includes:

[0020] Drop the quantum dot solution;

[0021] Repeat the process at least once: after the surface of the prepared detector is dried, dripping ethanedithiol solution, and starting a gelling machine to perform ligand replacement;

[0022] Use non-polar organic solvents and acetonitrile for cleaning.

[0023] A second aspect of the embodiments of the present disclosure provides a quantum dot-graphene detector prepared by the preparation method described in the first aspect, comprising:

[0024] Silicon oxide substrate;

[0025] A metal bottom electrode formed on one side of the silicon oxide substrate;

[0026] a nickel oxide layer formed on a portion of the metal bottom electrode;

[0027] A graphene layer is integrally formed on the other side of the silicon oxide substrate, on a portion of the nickel oxide layer, and on one side of the metal bottom electrode and the nickel oxide layer;

[0028] a metal top electrode formed on the graphene layer on the other side of the silicon oxide substrate and separated from the metal bottom electrode and the nickel oxide layer by the graphene layer formed on one side of the metal bottom electrode and the nickel oxide layer;

[0029] A quantum dot film is formed on the upper outer surfaces of the metal bottom electrode, the nickel oxide layer, the graphene layer and the metal top electrode.

[0030] In one embodiment of the present disclosure, the thickness of the nickel oxide layer is 50 nm.

[0031] In one embodiment of the present disclosure, the material of the nickel oxide layer is a P-type semiconductor material.

[0032] In one embodiment of the present disclosure, the thickness of the quantum dot film is 100 nm.

[0033] It can be seen from the above-mentioned embodiments of the present disclosure that the quantum dot-graphene detector and its preparation method provided by the present disclosure, in order to solve the technical difficulties of large dark current and low responsiveness of graphene detectors, designs a PbS quantum dot-graphene detector that can be in a vertical structure and can suppress the dark current of graphene. The dark current of the graphene detector is effectively reduced through the partial blocking effect of nickel oxide, and at the same time, PbS quantum dots are used as the main light absorption material and graphene is used as the carrier transport layer, so that the device has the characteristics of high gain mechanism and fast response. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the embodiments of the present disclosure or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.

[0035] Figure 1 A flowchart of a method for preparing a quantum dot-graphene detector according to an embodiment of the present disclosure is schematically shown;

[0036] Figure 2 The process flow chart of the quantum dot-graphene detector according to the embodiment of the present disclosure is schematically shown;

[0037] Figure 3 A schematic diagram of a quantum dot-graphene detector according to an embodiment of the present disclosure is schematically shown;

[0038] Figure 4 Schematically shows a cross-sectional schematic diagram of a quantum dot-graphene detector according to an embodiment of the present disclosure;

[0039] Description of Figure Numbers:

[0040] 31: silicon oxide substrate;

[0041] 32: metal bottom electrode;

[0042] 33: nickel oxide layer;

[0043] 34: graphene layer;

[0044] 35: metal top electrode;

[0045] 36: Quantum dot film. DETAILED DESCRIPTION

[0046] In order to make the disclosure purpose, features, and advantages of the present disclosure more obvious and easy to understand, the technical solutions in the embodiments of the present disclosure will be clearly and completely described below in conjunction with the drawings in the embodiments of the present disclosure. Obviously, the described embodiments are only part of the embodiments of the present disclosure, not all of the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present disclosure.

[0047] Figure 1 The flowchart of the method for preparing a quantum dot-graphene detector according to an embodiment of the present disclosure is schematically shown. Figure 2 The process flow chart of the quantum dot-graphene detector according to the embodiment of the present disclosure is schematically shown;

[0048] like Figure 1 and Figure 2 As shown, the method for preparing the quantum dot-graphene detector includes operations S1 to S6.

[0049] In operation S1, a metal bottom electrode is evaporated on one side of an oxidized silicon wafer substrate by a negative photolithography process.

[0050] In operation S2, a nickel oxide layer is sputtered on the metal bottom electrode by a negative photolithography process.

[0051] In operation S3, a single graphene layer is transferred to the nickel oxide layer.

[0052] In operation S4, the graphene layer is patterned by positive photolithography and oxygen plasma etching, so that the graphene layer covers a portion of the surface of the nickel oxide layer and the surface of the other side of the silicon oxide substrate.

[0053] In operation S5, a metal top electrode is evaporated on the graphene layer by a negative resist photolithography process to obtain a preliminary detector.

[0054] In operation S6, a quantum dot film is spin-coated on the upper surface of the prepared detector.

[0055] In one embodiment, S1, S2, and S5 may all include: the photolithography process is spin coating AR-4340 negative resist, pre-baking, UV exposure, post-baking, and development, and the pattern exposed after development is the pattern corresponding to the metal electrode and nickel oxide.

[0056] In one embodiment, S2, sputtering a nickel oxide layer on the metal bottom electrode includes: using a nickel target with a purity of 99.99% by radio frequency sputtering, and sputtering the nickel oxide layer on the metal bottom electrode in an atmosphere of oxygen and argon.

[0057] In one embodiment, S3 includes: the transfer of graphene adopts the current mainstream wet transfer, PMMA is used as the transfer protective layer, and the copper etching solution adopts a mixed solution of copper sulfate and hydrochloric acid in a ratio of CuSO4: HCl: H2O = 1g: 5ml: 5ml. The specific steps are as follows 1)-8):

[0058] 1) Place the metal film with graphene on a flat substrate (such as a silicon wafer or a glass slide) as a support, fix the copper sheet with tape, and prevent PMMA from seeping down so that the back side is stained with PMMA and is difficult to remove during etching;

[0059] 2) Use the laboratory's coating machine to perform multi-step spin coating on PMMA, first at 500 r / min for 15 s, then at 2000 r / min for 45 s;

[0060] 3) Place the copper foil with PMMA on a heating plate and heat at 100°C for 9 minutes to solidify the PMMA into a film;

[0061] 4) After the heating and curing is completed, the copper foil is placed in a copper etching solution for etching. The etching time is generally controlled to be more than 3 hours, and finally a PMMA / graphene film suspended on the surface of the copper etching solution is obtained;

[0062] 5) Use a flat substrate (such as a glass slide or silicon wafer) to pick up the copper etching solution, and rinse it in deionized water for 2 to 3 times to remove the ionic solution attached to the PMMA / graphene film;

[0063] 6) Prepare the clean silicon wafer treated with acetone and ultrasound and transfer it to deionized water. After completion, let it stand and air dry;

[0064] 7) Place the air-dried PMMA / graphene / silicon substrate on a heating plate and heat at 150°C for 15 min to flatten the graphene and ensure good contact between the graphene and the silicon substrate;

[0065] 8) After heating, allow it to cool naturally, soak it in an appropriate amount of acetone for 30 minutes, repeat twice, and finally wash it with anhydrous ethanol and deionized water.

[0066] In one embodiment, S4 includes a photolithography process of spin coating BP-701 positive photoresist, pre-baking, UV exposure, development, and post-baking, and the pattern left after development corresponds to the graphene pattern left after etching.

[0067] In one embodiment, in S6, the growth of quantum dots can be achieved by dissolving a sulfur source and PbO in an organic solvent to prepare solution A and solution B respectively; heating solution B to 120°C to 180°C, and then rapidly injecting solution A into solution B for reaction; stopping heating and waiting for the solution to gradually cool to room temperature; centrifuging and purifying, dispersing the centrifugal product in a non-polar organic solvent, and completing the preparation of PbS quantum dots.

[0068] In one embodiment, a hot injection method is used to grow PbS quantum dots, and a quantum dot film is deposited by layer-by-layer self-assembly. It should be noted that after stopping heating, the solution is allowed to gradually cool down to room temperature. The gradual cooling method allows multiple temperature gradients during the quantum dot growth process and sufficient time to enter Ostwald ripening. Compared with traditional quantum dot growth, the quantum dots grown in the present disclosure have a technical effect of wide spectral response.

[0069] In one embodiment, the layer-by-layer self-assembly method includes: dripping a quantum dot solution; repeating at least once: dripping an ethanedithiol solution after the surface is dry, and starting a gelling machine for ligand replacement; and washing the surface with a non-polar organic solvent and acetonitrile after the surface is dry.

[0070] In one embodiment, oleic acid can be used as a quantum dot ligand reagent during the quantum dot growth process. Oleic acid is a long-chain ligand that is not conducive to carrier transport. By using ethanedithiol solution to perform ligand replacement, the quantum dots are replaced with short-chain ligands with better conductivity, which is more conducive to the formation of a heterojunction between graphene and quantum dots.

[0071] In one embodiment, the thickness of the quantum dot film can be controlled by the concentration of the quantum dot solution, the spin coating speed and the number of spin coating times during the self-assembly process. The thickness is, for example, about 100 nm.

[0072] In one example, when evaporating the metal top electrode, the metal bottom electrode and the sputtering NiO layer, the photolithography process spin-coated AR-4340 negative photoresist (rotation speed 6000rpm, 20s), pre-baked (110℃, 2min), UV exposed (300W, 30s), post-baked (100℃, 2min), and developed (2min 30s).

[0073] In one example, when graphene is patterned, the photolithography process includes spin coating BP-701 positive photoresist (rotation speed 4000 rpm, 20 seconds), pre-baking (100°C, 1 min 30 seconds), UV exposure (300 W, 20 seconds), development (30 seconds), and post-baking (100°C, 1 min 30 seconds).

[0074] In one example, magnetron sputtering the nickel oxide layer includes: using a power of 200 W, radio frequency sputtering a nickel target with a purity of 99.99%, performing magnetron sputtering in an oxygen and argon atmosphere and a vacuum degree of 0.5 mTorr.

[0075] In one example, PbS quantum dots are grown by hot injection, and a quantum dot film is deposited by layer-by-layer self-assembly. The specific steps are as follows:

[0076] 1. Prepare the lead source: weigh 0.9g PbO, 20mL 1-octadecene, and 3mL oleic acid into a three-necked flask, add a stirring magnet, and seal with sealing tape;

[0077] 2. Turn on the vacuum pump, rotate the Black system to vacuum, remove water and oxygen in the lead source, set the magnetic stirring to 400r / min, and set the heating end temperature to 90°C. The lead source preparation time is relatively long, generally 3 to 4 hours, until the solution is clear and transparent;

[0078] 3. Preparation of sulfur source: first, measure more than 10 mL of 1-octadecene into another three-necked flask, add a magnetic particle, seal it with sealing tape, rotate the Black system to vacuum, and adjust the magnetic particle speed to 500 r / min to exclude reagent water and oxygen.

[0079] 4. Put the 1-octadecene from which water and oxygen have been removed into a glove box, measure 10 mL of 1-octadecene, and use a dropper to take 0.28 mL of (bistrimethylsilyl) sulfide in the glove box to prepare a sulfur precursor.

[0080] 5. After the lead source becomes clear and transparent, introduce nitrogen into it and then evacuate it. Repeat this process three times. Finally, after introducing nitrogen, close the Black system and set the temperature at 150°C. When the temperature reaches 150°C, use a syringe to draw out 10 mL of sulfur precursor and quickly inject it into the lead precursor.

[0081] 6. The solution turns black quickly. At this time, turn off the heating system and wait for the solution to cool to room temperature. When the reaction is over, remove the sealing tape, pour the post-reaction solution into a centrifuge tube, and add MOS-grade methanol as a precipitant.

[0082] 7. Set the centrifugation parameters, set the centrifugal speed to 8000r / min, set the centrifugal time to 8min, pour out the supernatant after centrifugation, add an appropriate amount of n-hexane to dissolve the precipitate, then add an appropriate amount of MOS methanol for centrifugation, and repeat 2-3 times.

[0083] 8. The obtained precipitate was dried, and then n-hexane was used as a dispersant to prepare a PbS quantum dot solution with a concentration of 30 mg / mL.

[0084] In one example, the steps for preparing quantum dot film by layer-by-layer self-assembly are as follows: adjust the speed of the coating machine to 3000r / min, the spin coating time to 20s, and use a dropper to drip 1-2 drops of quantum dot solution; after the surface of the film is dry, drip 1-2 drops of ethanedithiol solution, start the coating machine for ligand replacement, repeat this step 3 times to ensure complete ligand replacement; after the film is dry, wash it with quantum dot solution solvent and acetonitrile.

[0085] Figure 3 A schematic diagram of a quantum dot-graphene detector according to an embodiment of the present disclosure is schematically shown. Figure 4 Schematically shows a cross-sectional schematic diagram of a quantum dot-graphene detector according to an embodiment of the present disclosure;

[0086] like Figure 3 and Figure 4 As shown, the quantum dot-graphene detector includes: a silicon oxide substrate 31; a metal bottom electrode 32 formed on one side of the silicon oxide substrate 31; a nickel oxide layer 33 formed on a portion of the metal bottom electrode 31; a graphene layer 34 formed integrally on the other side of the silicon oxide substrate 31, on a portion of the nickel oxide layer 33, and on one side of the metal bottom electrode 32 and the nickel oxide layer 33; a metal top electrode 35 formed on the graphene layer 34 on the other side of the silicon oxide substrate 31, separated from the metal bottom electrode 32 and the nickel oxide layer 33 by the graphene layer 34 formed on one side of the metal bottom electrode 32 and the nickel oxide layer 33; a quantum dot film 363 formed on the upper outer surfaces of the metal bottom electrode 32, the nickel oxide layer 33, the graphene layer 34 and the metal top electrode 35.

[0087] In one embodiment, the thickness of the nickel oxide layer 33 is 50 nm.

[0088] In one embodiment, the nickel oxide layer 33 is made of a P-type semiconductor material.

[0089] In one embodiment, the thickness of the quantum dot film 36 is 100 nm. The quantum dot film is a lead sulfide quantum dot film.

[0090] According to the disclosed embodiment, the quantum dot-graphene detector of the present disclosure uses an extremely thin nickel oxide layer as an isolation layer, blocking most of the dark current during the period, and at the same time, under the action of the electric field, allowing some carriers to tunnel through the isolation layer to form a light response. At the same time, a PbS quantum dot-modified graphene detector is used. While suppressing the dark current, the device also has a high light gain, which partially solves the technical difficulties of large dark current and low response of the current graphene detector.

[0091] It should be noted that, for the above-mentioned method embodiments, for the sake of simplicity of description, they are all expressed as a series of action combinations, but those skilled in the art should know that the present disclosure is not limited by the described action sequence, because according to the present disclosure, certain steps can be performed in other sequences or simultaneously. Secondly, those skilled in the art should also know that the embodiments described in the specification are all preferred embodiments, and the actions and modules involved are not necessarily required by the present disclosure.

[0092] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0093] The above is a description of a quantum dot-graphene detector and a preparation method thereof provided by the present disclosure. For technicians in this field, according to the ideas of the embodiments of the present disclosure, there may be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as a limitation on the present disclosure.

Claims

1. A method for preparing a quantum dot-graphene detector, characterized in that: include: A metal bottom electrode is evaporated on one side of the oxide silicon wafer substrate by a negative photolithography process; sputtering a nickel oxide layer on the metal bottom electrode by a negative photolithography process; transferring a single layer of graphene on the nickel oxide layer; Patterning the graphene layer by positive photolithography and oxygen plasma etching, so that the graphene layer covers a portion of the surface of the nickel oxide layer and the surface of the other side of the silicon oxide substrate; Vapor-depositing a metal top electrode on the graphene layer by a negative resist photolithography process to obtain a preliminary detector; A quantum dot film is spin-coated on the upper surface of the prepared detector.

2. The method for preparing a quantum dot-graphene detector according to claim 1, characterized in that: The transferring of a single-layer graphene layer on the nickel oxide layer comprises: A single-layer graphene layer is transferred onto the nickel oxide layer by wet transfer.

3. The method for preparing a quantum dot-graphene detector according to claim 1, characterized in that: In the growth process of the quantum dot film, oleic acid is used as a quantum dot ligand reagent.

4. The method for preparing a quantum dot-graphene detector according to claim 1, characterized in that: The sputtering of a nickel oxide layer on the metal bottom electrode comprises: A nickel target material with a radio frequency sputtering purity of 99.99% is used to sputter a nickel oxide layer on the metal bottom electrode in an atmosphere of oxygen and argon.

5. The method for preparing a quantum dot-graphene detector according to claim 1, characterized in that: The spin coating of the quantum dot film on the upper surface of the prepared detector comprises: A lead sulfide quantum dot film is spin-coated on the upper surface of the prepared detector by using a hot injection method and a layer-by-layer self-assembly method.

6. The method for preparing a quantum dot-graphene detector according to claim 1, characterized in that: The layer-by-layer self-assembly method includes: Drop the quantum dot solution; Repeat the process at least once: after the surface of the prepared detector is dried, dripping ethanedithiol solution, and starting a gelling machine to perform ligand replacement; Use non-polar organic solvents and acetonitrile for cleaning.

7. A quantum dot-graphene detector prepared by the preparation method according to any one of claims 1 to 6, characterized in that: include: Silicon oxide substrate; A metal bottom electrode formed on one side of the silicon oxide substrate; a nickel oxide layer formed on a portion of the metal bottom electrode; A graphene layer is integrally formed on the other side of the silicon oxide substrate, on a portion of the nickel oxide layer, and on one side of the metal bottom electrode and the nickel oxide layer; a metal top electrode formed on the graphene layer on the other side of the silicon oxide substrate and separated from the metal bottom electrode and the nickel oxide layer by the graphene layer formed on one side of the metal bottom electrode and the nickel oxide layer; A quantum dot film is formed on the upper outer surfaces of the metal bottom electrode, the nickel oxide layer, the graphene layer and the metal top electrode.

8. The quantum dot-graphene detector according to claim 7, characterized in that: The thickness of the nickel oxide layer is 50 nm.

9. The quantum dot-graphene detector according to claim 7, characterized in that: The material of the nickel oxide layer is a P-type semiconductor material.

10. The quantum dot-graphene detector according to claim 7, characterized in that: The thickness of the quantum dot film is 100 nm.

Citation Information

Cited By

  • A photodetector with double interface layers and a preparation method thereof

    CN122871743A