4H-SiC Schottky radiation detector based on hexagonal boron nitride two-dimensional thin film and preparation method of 4H-SiC Schottky radiation detector
By using hexagonal boron nitride film to optimize the interface in the silicon carbide radiation detector, the Schottky contact junction is formed, which solves the performance degradation caused by the interface defect state under high temperature and high radiation conditions, and achieves higher carrier separation and transmission The radiation resistance performance ensures the stable operation of the detector in harsh environments.
Patent Information
- Application Number
- CN202310537848.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-12
AI Technical Summary
The existing silicon carbide radiation detectors have degraded performance due to interface defects under high temperature and high radiation conditions. The durability of traditional silicon dioxide insulator materials is insufficient, making it difficult to meet the stable working requirements in high temperature and high radiation environments.
Hexagonal boron nitride film is used as an insulating medium to optimize the contact interface between silicon carbide and metal, form Schottky contact junction, reduce interface defect state, improve carrier separation and transportation capacity, and use the high band of hexagonal boron nitride Width and radiation resistance improve the performance of the device under high temperature and high radiation conditions.
Through the use of hexagonal boron nitride film, the carrier separation and radiation resistance of the detector are significantly improved, ensuring that the device maintains good performance in high temperature and high radiation environments, and reducing interfacial charge and lattice mismatch problems.
Smart Images

Figure CN118943231A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor devices and detection technology, and in particular to a 4H-SiC Schottky radiation detector based on hexagonal boron nitride film. Technical Background
[0002] Silicon carbide has the characteristics of large bandgap width, high breakdown electric field strength, high saturated electron drift velocity, large thermal conductivity, small dielectric constant, strong radiation resistance, and good chemical stability. It is considered to be a wide bandgap semiconductor material with great potential for making high-temperature, high-frequency, high-power and radiation-resistant devices. Based on the excellent high-temperature resistance and radiation resistance of silicon carbide materials, silicon carbide materials have received widespread attention in the field of nuclear detection in recent years and have been used in the detection of ionized particles and neutrons. Using the metal / insulator / semiconductor structure, high-resolution detector manufacturing under low bias and thin sensitive layer conditions is achieved. The insulating layer of the above-mentioned structure is usually a bulk material such as silicon oxide, but since the interface charge generated by chemical vapor deposition growth of bulk materials such as silicon oxide on the surface of silicon carbide is about two orders of magnitude higher than that of silicon, there are a large number of interface defect states that greatly reduce the performance of the device. And because the device works under high temperature and high radiation conditions, this working environment is a challenge for traditional silicon dioxide-based insulating materials.
[0003] Therefore, there is an urgent need for wide-bandgap semiconductor radiation detectors that are resistant to high temperature and high radiation, and to design wide-bandgap semiconductor radiation detector structures with low defect states, reduce material interface defect states, and improve the performance of devices under high temperature and high radiation conditions. Summary of the invention
[0004] The present invention provides a 4H-SiC Schottky radiation detector based on a hexagonal boron nitride film, which can optimize the contact interface through the hexagonal boron nitride film, thereby improving the carrier separation and transport, and improving the device performance of the detector. The hexagonal boron nitride (h-BN) film is a two-dimensional material with a structure similar to that of graphene. Unlike the high conductivity of graphene, hexagonal boron nitride has good insulation properties. In addition, as a two-dimensional dielectric material, the surface of hexagonal boron nitride has no dangling bonds, and the surface is strongly covalently bonded. The hexagonal boron nitride layers are bonded by van der Waals forces, and the material is also bonded to the bulk material by van der Waals forces, just like stacking blocks, and the defect state problem caused by lattice mismatch between different materials can be ignored. Therefore, compared with other bulk materials, the two-dimensional material, hexagonal boron nitride film, can provide a uniform, low-wrinkle surface and reduce the surface interface charge. Replacing the traditional bulk material insulating layer with hexagonal boron nitride film can optimize the contact interface between silicon carbide, hexagonal boron nitride and metal, forming an excellent Schottky contact junction, thereby improving carrier separation and transport, and improving the device performance of the detector. At the same time, due to the high temperature and radiation resistance of hexagonal boron nitride, the overall device still maintains good device performance under high temperature and high radiation conditions.
[0005] The solution provided by the present invention:
[0006] The 4H-SiC Schottky radiation detector based on hexagonal boron nitride film comprises:
[0007] The substrate layer is a highly doped silicon carbide that supports the entire device and is placed above the n-type silicon carbide ohmic contact lower electrode and below the buffer layer. The preferred thickness of the substrate layer is 300 to 350 μm; the preferred doping concentration of the substrate layer is 1 to 5×10 18 cm -3 .
[0008] The buffer layer is placed on the substrate layer, away from the n-type silicon carbide ohmic contact lower electrode, and plays a role in reducing the electric field gradient at the interface with the substrate layer. It is preferably n-type silicon carbide with a doping concentration lower than that of the substrate layer, and has a thickness of 1 to 500 nm. The preferred doping concentration of the buffer layer is 1 to 1×10 18 cm -3 .
[0009] The sensitive layer is placed on the buffer layer and away from the substrate layer, and is made of silicon carbide to absorb charged particles. The preferred thickness of the sensitive layer structure is 1 to 100 μm; the preferred doping concentration of the sensitive layer is 1 to 1×10 14 cm -3 .
[0010] Hexagonal boron nitride film layer, the hexagonal boron nitride film layer is a hexagonal boron nitride film, placed on the sensitive layer, away from the buffer layer, to optimize the contact between silicon carbide and metal, improve carrier separation and transport, and reduce the thickness of the sensitive layer. Preferably, the hexagonal boron nitride film can be a single layer or a multilayer.
[0011] The upper electrode has a Schottky contact type and is placed on the hexagonal boron nitride film layer, away from the sensitive layer, and forms a Schottky junction with the hexagonal boron nitride film layer and the sensitive layer. Preferably, the material of the upper electrode is any one of Ti, Al, Ni, and Au. Furthermore, the electrode can also be formed by stacking a two-dimensional graphene film with any one of Ti, Al, Ni, and Au.
[0012] The lower electrode has an ohmic contact type and is placed below the substrate layer, away from the buffer layer, and forms an ohmic contact with the substrate layer. The material of the lower electrode is any one of Ti, Al, Ni, and Au.
[0013] The characteristics and advantages of the present invention are:
[0014] (1) As a two-dimensional dielectric material, the hexagonal boron nitride film has no dangling bonds on the surface, and is strongly covalently bonded within the surface. The hexagonal boron nitride layers are bonded by van der Waals forces, and the material is also bonded to the bulk material by van der Waals forces, just like stacking blocks. The defect state problem caused by the lattice mismatch between different materials can be ignored. Therefore, compared with other bulk materials, the two-dimensional material - hexagonal boron nitride film can provide a uniform, low-wrinkle surface and reduce the surface interface charge. As an insulating dielectric layer, the hexagonal boron nitride film can optimize the contact interface, thereby improving carrier separation and transport, and improving the device performance of the detector.
[0015] (2) The hexagonal boron nitride film has a high bandgap width (about 5.97 eV) and is resistant to high temperatures and radiation, so that the device can maintain good device performance under high temperature and high radiation conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is a structural diagram of a 4H-SiC Schottky radiation detector based on a hexagonal boron nitride film without a graphene-related electrode implemented in the present invention.
[0017] Figure 2 A structural diagram of a 4H-SiC Schottky radiation detector based on a hexagonal boron nitride film with graphene participating electrodes implemented in the present invention.
[0018] Figure 3 This is a process flow chart of the electrode without graphene implemented in the present invention.
[0019] Figure 4 The present invention is a process flow chart of graphene-involved electrodes. DETAILED DESCRIPTION
[0020] Implementation 1:
[0021] In order to implement the present invention, the following will be combined with the attached embodiment of the present invention. Figure 1 , the technical solutions in the embodiments of the present invention are clearly and completely described. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. The described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0022] The present invention provides a 4H-SiC Schottky radiation detector based on a two-dimensional hexagonal boron nitride film. Figure 1As shown, the substrate layer 1 is silicon carbide, and a silicon carbide buffer layer 2, a silicon carbide sensitive layer 3, a hexagonal boron nitride film layer 4, and a silicon carbide Schottky contact upper electrode 5 are sequentially covered on the upper surface of the substrate layer 1, and an n-type silicon carbide ohmic contact lower electrode 6 is formed on the lower surface of the substrate 1.
[0023] Among them, the preferred material of the hexagonal boron nitride film layer 4 is a hexagonal boron nitride film, and the hexagonal boron nitride film is preferably a single layer or a multilayer. The thickness of the sensitive layer 3 is preferably 1 to 100 μm. The thickness of the buffer layer 2 is preferably 1 to 500 nm, and the material is silicon carbide. The material of the upper electrode 5 and the lower electrode 6 can be any one of Ti, Al, Ni, and Au, but is not limited thereto.
[0024] Implementation 2:
[0025] In order to implement the present invention, the following will be combined with the attached embodiment of the present invention. Figure 2 , the technical solutions in the embodiments of the present invention are clearly and completely described. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. The described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0026] The present invention provides a 4H-SiC Schottky radiation detector based on a two-dimensional hexagonal boron nitride film. Figure 2 As shown, the substrate layer 1 ′ For silicon carbide, the substrate layer 1 ′ The upper surface is sequentially covered with a silicon carbide buffer layer 2 ′ , Silicon carbide sensitive layer 3 ′ , hexagonal boron nitride thin film layer 4 ′ 、Silicon carbide Schottky contact power level 5 ′ , wherein the metal upper electrode further includes a graphene insertion layer 52 ′ and metal layer 51 ′ , on the substrate 1 ′ The n-type silicon carbide ohmic contact lower electrode 6 is formed on the lower surface ′ .
[0027] Wherein, the hexagonal boron nitride 4 ′ The preferred material is hexagonal boron nitride film, and the preferred hexagonal boron nitride film is a single layer or multiple layers. ′ The thickness of the buffer layer 2 is preferably 1 to 100 μm. ′ The thickness of the metal upper electrode layer 51 is preferably 1 to 500 nm and the material is silicon carbide. ′Any one of Ti, Al, Ni, and Au can be used with the graphene insertion layer 52 ′ The lower electrode 6 ′ The material can be any one of Ti, Al, Ni, and Au, but is not limited thereto. The specific steps for implementing the preparation of the embodiments 1 and 2 are as follows.
[0028] Implementation 1:
[0029] Step 1: 4H-SiC sample cleaning: SiC substrate cleaning is mainly to remove impurities on the surface of the material, such as organic pollutants, some metal impurities, etc. The specific cleaning process is as follows:
[0030] (1) The sample (5 mm × 5 mm) was ultrasonically cleaned in an acetone solution to remove organic contaminants on the SiC surface.
[0031] (2) Ultrasonic cleaning in anhydrous ethanol solution, followed by rinsing with deionized water. Since acetone is only soluble in organic solvents, the function of the anhydrous ethanol solution is to remove the residual acetone solution on the surface of the sample; finally, rinsing with deionized water to remove the anhydrous ethanol solution;
[0032] (3) Deionized water, ammonia water and hydrogen peroxide are prepared into cleaning solution No. 1 in a ratio of 2:1:1. The sample is placed in the cleaning solution No. 1 for ultrasonic cleaning. After being taken out, it is repeatedly rinsed with a large amount of deionized water. The function of the cleaning solution No. 1 is alkaline oxidation to remove particles on the surface of the material;
[0033] (4) Deionized water, hydrochloric acid and hydrogen peroxide are prepared into cleaning solution No. 2 in a ratio of 2:1:1. The sample is placed in the cleaning solution No. 2 for ultrasonic cleaning. After being taken out, it is repeatedly rinsed with a large amount of deionized water. The function of the cleaning solution No. 2 is acidic oxidation to remove active metals on the surface of the material;
[0034] (5) Pour the HF solution into a polytetrafluoroethylene container and completely immerse the sample in the HF solution to remove the natural oxide layer on the SiC surface; after taking it out, rinse it repeatedly with a large amount of deionized water, and then blow dry it with N2 for later use;
[0035] Step 2: Preparation of ohmic contact electrode: Place the electrode mask (electrode size is 3×3mm 2 ) is covered on the C surface of the SiC sample, and a high vacuum thermal evaporation table is used, and the vacuum degree of the reaction chamber is 2×10 -3 Pa, three layers of metal films, Al, Ti and Au, are uniformly deposited on the C surface of the SiC sample in sequence; the sample is thermally annealed in a N2 atmosphere at a temperature of 850°C to form an ohmic contact electrode.
[0036] Step 3, transfer of hexagonal boron nitride: using methane as the carbon source and hydrogen as the protective gas, a hexagonal boron nitride film is grown on the copper foil, polymethyl methacrylate (PMMA) is coated on the upper surface of the hexagonal boron nitride as a protective layer, and the PMMA / hexagonal boron nitride / Cu is first cleaned with a hydrogen peroxide / hydrochloric acid mixed solution, and then placed in a potassium persulfate solution to remove the copper foil. After all the copper is removed, the PMMA / hexagonal boron nitride is transferred to the SiC surface. Finally, acetone is used to dissolve PMMA to complete the hexagonal boron nitride transfer process.
[0037] Step 4: Preparation of Schottky contact electrode:
[0038] The electrode mask (electrode size is 3×3mm 2 ) is covered on the hexagonal boron nitride surface, using a high vacuum thermal evaporation table, and the vacuum degree of the reaction chamber is 2×10 -3 Pa, three layers of metal films, Al, Ti and Au, are uniformly deposited on the hexagonal boron nitride surface in sequence; the sample is thermally annealed in a N2 atmosphere to form a Schottky contact electrode.
[0039] Step 5: Sample packaging: Evenly coat the ohmic contact of the SiC sample with silver paste and bond it to the PCB board; use wires to lead out the Schottky electrode and connect it to the PCB board.
[0040] Implementation 2:
[0041] Step 1: 4H-SiC sample cleaning: SiC substrate cleaning is mainly to remove impurities on the surface of the material, such as organic pollutants, some metal impurities, etc. The specific cleaning process is as follows:
[0042] (1) The sample (5 mm × 5 mm) was ultrasonically cleaned in an acetone solution to remove organic contaminants on the SiC surface.
[0043] (2) Ultrasonic cleaning in anhydrous ethanol solution, followed by rinsing with deionized water. Since acetone is only soluble in organic solvents, the function of the anhydrous ethanol solution is to remove the residual acetone solution on the surface of the sample; finally, rinsing with deionized water to remove the anhydrous ethanol solution;
[0044] (3) Deionized water, ammonia water and hydrogen peroxide are prepared into cleaning solution No. 1 in a ratio of 2:1:1. The sample is placed in the cleaning solution No. 1 for ultrasonic cleaning. After being taken out, it is repeatedly rinsed with a large amount of deionized water. The function of the cleaning solution No. 1 is alkaline oxidation to remove particles on the surface of the material;
[0045] (4) Deionized water, hydrochloric acid and hydrogen peroxide are prepared into cleaning solution No. 2 in a ratio of 2:1:1. The sample is placed in the cleaning solution No. 2 for ultrasonic cleaning. After being taken out, it is repeatedly rinsed with a large amount of deionized water. The function of the cleaning solution No. 2 is acidic oxidation to remove active metals on the surface of the material;
[0046] (5) Pour the HF solution into a polytetrafluoroethylene container and completely immerse the sample in the HF solution to remove the natural oxide layer on the SiC surface; after taking it out, rinse it repeatedly with a large amount of deionized water, and then blow dry it with N2 for later use;
[0047] Step 2: Preparation of ohmic contact electrode: Place the electrode mask (electrode size is 3×3mm 2 ) is covered on the C surface of the SiC sample, and a high vacuum thermal evaporation table is used, and the vacuum degree of the reaction chamber is 2×10 -3 Pa, three layers of metal films, Al, Ti and Au, are uniformly deposited on the C surface of the SiC sample in sequence; the sample is thermally annealed in a N2 atmosphere at a temperature of 850°C to form an ohmic contact electrode.
[0048] Step 3, transfer of hexagonal boron nitride: using methane as the carbon source and hydrogen as the protective gas, a hexagonal boron nitride film is grown on the copper foil, polymethyl methacrylate (PMMA) is coated on the upper surface of the hexagonal boron nitride as a protective layer, and the PMMA / hexagonal boron nitride / Cu is first cleaned with a hydrogen peroxide / hydrochloric acid mixed solution, and then placed in a potassium persulfate solution to remove the copper foil. After all the copper is removed, the PMMA / hexagonal boron nitride is transferred to the SiC surface. Finally, acetone is used to dissolve PMMA to complete the hexagonal boron nitride transfer process.
[0049] Step 4: Preparation of Schottky contact electrode with graphene:
[0050] (1) Transfer of graphene: Using methane as the carbon source and hydrogen as the protective gas, a graphene film is grown on a copper foil. Polymethyl methacrylate (PMMA) is coated on the upper surface of the graphene as a protective layer. The PMMA / graphene / Cu is first cleaned with a hydrogen peroxide / hydrochloric acid mixed solution and then placed in a potassium persulfate solution to remove the copper foil. After all the copper is removed, the PMMA / graphene is transferred to the hexagonal boron nitride surface. Finally, acetone is used to dissolve the PMMA to complete the graphene transfer process.
[0051] (2) Preparation of Schottky contact electrode: Place the electrode mask (electrode size 3×3mm 2 ) is covered on the graphene surface, and a high vacuum thermal evaporation table is used, and the vacuum degree of the reaction chamber is 2×10 -3 Pa, three layers of metal films, Al, Ti and Au, are uniformly deposited on the hexagonal boron nitride surface in sequence; the sample is thermally annealed in a N2 atmosphere to form a Schottky contact electrode.
[0052] Step 5: Sample packaging: Evenly coat the ohmic contact of the SiC sample with silver paste and bond it to the PCB; Use wires to lead out the Schottky electrode and connect it to the PCB
[0053] Of course, the 4H-SiC Schottky radiation detector based on hexagonal boron nitride two-dimensional film of the present invention can also have a variety of changes and modifications, and is not limited to the specific structure of the above-mentioned embodiment. In short, the protection scope of the present invention should include those changes or substitutions and modifications that are obvious to ordinary technicians in the field.
Claims
1. A 4H-SiC Schottky radiation detector based on a two-dimensional hexagonal boron nitride film, characterized in that: include:
1. Silicon carbide substrate layer 2. Silicon carbide buffer layer 3. Silicon carbide sensitive layer 4. Hexagonal boron nitride film layer 5. Silicon carbide Schottky contact upper electrode 6. N-type silicon carbide ohmic contact lower electrode. The substrate layer is highly doped silicon carbide and supports the entire device. It is placed above the n-type silicon carbide ohmic contact lower electrode and below the buffer layer. Preferably, the substrate layer has a thickness of 300-350 μm. The buffer layer is placed on the substrate layer, away from the n-type silicon carbide ohmic contact lower electrode, to reduce the electric field gradient at the interface with the substrate layer. It is preferably n-type silicon carbide with a doping concentration lower than that of the substrate layer, and has a thickness of 1 to 500 nm. The sensitive layer is placed on the buffer layer and away from the substrate layer, and silicon carbide plays a role in absorbing charged particles. The preferred thickness of the sensitive layer structure is 1 to 100 μm. The hexagonal boron nitride film layer is a hexagonal boron nitride film, which is placed on the sensitive layer and away from the buffer layer. It optimizes the contact between silicon carbide and metal, improves carrier separation and transport, and reduces the thickness of the sensitive layer. Preferably, the hexagonal boron nitride film can be a single layer or a multilayer. The upper electrode contact type is a Schottky contact, which is placed on the hexagonal boron nitride film layer, away from the sensitive layer, and forms a Schottky junction with the hexagonal boron nitride film layer and the sensitive layer. Preferably, the material of the upper electrode is any one of Ti, Al, Ni, and Au. Furthermore, the electrode can also be formed by stacking a two-dimensional graphene film with any one of Ti, Al, Ni, and Au metals. The lower electrode has an ohmic contact type and is placed below the substrate layer, away from the buffer layer, and forms an ohmic contact with the substrate layer. The material of the lower electrode is any one of Ti, Al, Ni, and Au.
2. The method for preparing a 4H-SiC Schottky radiation detector based on a two-dimensional hexagonal boron nitride film according to claim 1, characterized in that: The following steps are involved: Step 1: Cleaning the grown 4H-SiC sample; Step 2: Prepare an ohmic contact electrode on the back of the 4H-SiC sample; Step 3: Transfer the hexagonal boron nitride layer on the surface of the 4H-SiC sample: Spin polymethyl methacrylate (PMMA) onto the surface of the hexagonal boron nitride grown on the copper foil, wash the PMMA / hexagonal boron nitride / Cu with a hydrogen peroxide / hydrochloric acid mixed solution, then remove the copper foil in a potassium persulfate solution, and then wash it repeatedly with deionized water for several times, then transfer the cleaned PMMA / hexagonal boron nitride to the SiC surface and blow it dry with nitrogen. Finally, dissolve the PMMA with acetone to complete the hexagonal boron nitride transfer process. Step 4, Schottky contact electrode preparation, divided into Schottky contact electrode preparation with graphene and Schottky contact electrode preparation without graphene. The preparation process of Schottky contact electrode with graphene is as follows: (1) Transfer graphene film and hexagonal boron nitride film, spin-coat polymethyl methacrylate (PMMA) as a protective layer on the surface of graphene film / Cu, first wash PMMA / graphene / Cu with a hydrogen peroxide / hydrochloric acid mixed solution, then place it in a potassium persulfate solution to remove the copper foil, repeatedly wash it with deionized water, and then transfer PMMA / graphene to the hexagonal boron nitride surface and blow dry with nitrogen. Finally, dissolve PMMA with acetone to complete the graphene transfer process. (2) On graphene, complete the preparation of Schottky contact electrode by metal sputtering stripping. The preparation process of Schottky contact electrode without graphene is: directly complete the preparation of Schottky contact electrode on the hexagonal boron nitride surface by metal sputtering stripping. Step 5: Sample packaging: Evenly coat the ohmic contact of the SiC sample with silver paste and bond it to the PCB board; use wires to lead out the Schottky electrode and connect it to the PCB board.
Citation Information
Cited By
Electrode-integrated quantum light source and manufacturing method therefor
WO2026121860A1