Flip LED chip and preparation method thereof
By transferring the substrate of the flip LED chip and thinning the first semiconductor layer, combined with mechanical grinding and chemical mechanical polishing technology, the problems of low light transmittance and secondary radiation effects of GaN materials are solved, and the luminous efficiency of the chip is significantly improved .
Patent Information
- Application Number
- CN202411022801.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
The brightness increase of the flip-flop LED chip is lower than expected, mainly due to the low light transmittance of GaN materials and the reduction in the light output brightness caused by the secondary radiation effect. Reducing the thickness of the N-GaN layer will damage the epitaxial quality, resulting in the non-increasing luminous efficiency. drop.
By transferring the substrate of the LED chip and thinning the first semiconductor layer, the barrier to the emitted light is reduced. The first semiconductor layer is thinned by mechanical grinding and chemical mechanical polishing technology, and the thickness is controlled between 1 μm and 3 μm, and the reduction is carried out. A light layer is deposited on the thin layer to improve luminous efficiency.
The luminescence efficiency of the flip LED chip is improved. The surface roughness of the thinned first semiconductor layer is less than 5 nm, and the refractive index of the light-emitting layer material is less than that of the first semiconductor layer material, reducing total reflection, and significantly improving the light-emitting efficiency of the chip.
Smart Images

Figure CN118943257A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a flip-chip LED chip and a preparation method thereof. Background Art
[0002] At present, there are three main types of LED chip structures: vertical structure, upright structure and flip-chip structure. Among them, flip-chip LED chips have become the mainstream development direction of LED chips due to their superior heat dissipation performance, compact structural design and excellent optical performance. Different from the design of upright LED chips that emit light from the front, flip-chip LED chips emit light from the back, thus avoiding the situation where the metal electrode blocks the light-emitting surface and effectively increasing the light-emitting area. Therefore, the light brightness of flip-chip LED chips of the same area is often higher than that of upright chips.
[0003] Although benefiting from the increase in the effective luminous area, the brightness of the flip-chip LED chip has not increased as much as people expected. Part of the reason is that the radiated light from the multi-quantum well layer needs to pass through the thicker N-GaN epitaxial layer and the patterned sapphire substrate layer before it can be emitted, and the GaN material itself has a low transmittance and absorbs visible light in the blue light band to produce secondary radiation, resulting in a decrease in the brightness of the light. Although the transmittance can be increased by reducing the thickness of the N-GaN layer during epitaxial growth, the epitaxial quality will be greatly reduced, and the total luminous efficiency will decrease instead of increase. This is because during epitaxial growth, most of the N-GaN layer close to the sapphire substrate side acts as an epitaxial buffer layer to offset the lattice stress of the sapphire substrate. A hasty reduction in the thickness of the N-GaN layer will reduce the epitaxial quality of the multi-quantum well layer, resulting in a decrease in the brightness of the LED device. Therefore, how to further improve the brightness of the flip-chip LED chip has become a current technical problem. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for preparing a flip-chip LED chip, by transferring the substrate of the LED chip and thinning the first semiconductor layer, thereby reducing the obstruction of the emitted light and improving the luminous efficiency.
[0005] Another technical problem to be solved by the present invention is to provide a flip-chip LED chip with high luminous efficiency.
[0006] In order to solve the above problems, the present invention discloses a method for preparing a flip-chip LED chip, comprising the following steps:
[0007] (1) providing an epitaxial wafer, the epitaxial wafer comprising a substrate and a first semiconductor layer, a multi-quantum well layer, and a second semiconductor layer sequentially deposited on the substrate;
[0008] (2) etching the epitaxial wafer to obtain a MESA step exposing the first semiconductor layer;
[0009] (3) forming a first electrode on the MESA step, and forming a current spreading layer and a second electrode on the second semiconductor layer;
[0010] (4) depositing a reflective layer and opening a hole to expose the first electrode and the second electrode, and forming a first soldering pad and a second soldering pad on the first electrode and the second electrode, respectively, to obtain an LED chip;
[0011] (5) preparing a first bonding layer on the surface of the LED chip and opening a hole to expose the first pad and the second pad;
[0012] (6) providing a substrate with a second bonding layer, and bonding the substrate to the LED chip through the first bonding layer and the second bonding layer;
[0013] (7) peeling off the substrate and thinning the first semiconductor layer;
[0014] (8) depositing a light emitting layer on the thinned first semiconductor layer;
[0015] (9) thinning the substrate and opening a hole to expose the first pad and the second pad;
[0016] (10) Fill the holes on the surface of the substrate with solder paste and form ohmic contact with the first solder pad and the second solder pad to obtain a flip-chip LED chip.
[0017] As an improvement of the above technical solution, the thickness of the thinned first semiconductor layer is 1 μm to 3 μm.
[0018] As an improvement of the above technical solution, in step (7), the first semiconductor layer is thinned by mechanical grinding and chemical mechanical polishing;
[0019] The grinding pressure of the mechanical grinding is 1 kPa to 5 kPa, the grinding disc speed is 40 r / min to 80 r / min, the average particle size of the abrasive in the grinding liquid is 1 μm to 10 μm, and after mechanical grinding, the surface roughness of the first semiconductor layer is 0.1 μm to 5 μm;
[0020] The polishing pressure of the chemical mechanical polishing is 5kPa~12kPa, the polishing disk rotation speed is 60r / min~120r / min, the pH of the polishing liquid is 9~12, the average particle size of the abrasive in the polishing liquid is 50nm~70nm, and after chemical mechanical polishing, the surface roughness of the first semiconductor layer is 0.5nm~5nm.
[0021] As an improvement of the above technical solution, the mechanical grinding includes a first mechanical grinding and a second mechanical grinding;
[0022] The grinding pressure of the first mechanical grinding is 1 kPa to 5 kPa, the grinding disc speed is 40 r / min to 80 r / min, the average particle size of the abrasive in the grinding liquid is 5 μm to 10 μm, and after the first mechanical grinding, the thickness of the first semiconductor layer is reduced by 30% to 50%, and the surface roughness is 1 μm to 5 μm;
[0023] The grinding pressure of the second mechanical grinding is 1kPa-5kPa, the grinding disc speed is 40r / min-80r / min, the average particle size of the abrasive in the grinding liquid is 1μm-5μm, and after the second mechanical grinding, the surface roughness of the first semiconductor layer is 0.1μm-1μm.
[0024] As an improvement of the above technical solution, after the first semiconductor layer is thinned, the first semiconductor layer is cleaned.
[0025] As an improvement of the above technical solution, the material of the light emitting layer includes Al 2 O 3 、SiO 2 、Si 3 N 4 MgF 2 、TiO 2 and Ti 2 O 5 One or more of;
[0026] The thickness of the light-emitting layer is 50nm-1200nm.
[0027] As an improvement of the above technical solution, the light-emitting layer comprises Al 2 O 3 Layer and SiO 2 Layer, Al 2 O 3 Layer and SiO 2 The thickness of the layers is 30 nm to 500 nm.
[0028] As an improvement of the above technical solution, it also includes performing surface treatment on the surface of the substrate, and the surface treatment includes oxidation treatment and / or evaporation of an insulating layer.
[0029] As an improvement of the above technical solution, the LED chip and the substrate are bonded by direct bonding or adhesive bonding.
[0030] Correspondingly, the present invention also discloses a flip-chip LED chip, wherein the flip-chip LED is manufactured by the above-mentioned method for manufacturing the flip-chip LED chip.
[0031] The implementation of the present invention has the following beneficial effects:
[0032] 1. The method for preparing a flip-chip LED chip provided by the present invention is to thin the first semiconductor layer after peeling off the substrate, thereby reducing the blocking and absorption of the outgoing light by the substrate and the first semiconductor layer. The prepared flip-chip LED chip has high luminous efficiency, and the preparation method is simple and efficient.
[0033] 2. The preparation method of the flip-chip LED chip provided by the present invention performs mechanical grinding and chemical mechanical polishing on the first semiconductor layer, which causes little damage to the first semiconductor layer, has high grinding and polishing precision, controls the thinning time within 5 hours, and the surface roughness of the first semiconductor layer after thinning is less than 5 nm.
[0034] 3. The method for preparing a flip-chip LED chip provided by the present invention provides a light-emitting layer on the thinned first semiconductor layer, and the refractive index of the light-emitting layer material is smaller than that of the first semiconductor layer material, thereby reducing total reflection and improving the light-emitting efficiency of the chip. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 is a schematic diagram of the structure obtained in step (4) of the present invention;
[0036] Figure 2 is a schematic diagram of the structure obtained in step (5) of the present invention;
[0037] Figure 3 is a schematic diagram of the structure obtained in step (6) of the present invention;
[0038] Figure 4 is a schematic diagram of the structure obtained in step (7) of the present invention;
[0039] Figure 5 is a schematic diagram of the structure obtained in step (8) of the present invention;
[0040] Figure 6 is a schematic diagram of the structure obtained in step (9) of the present invention;
[0041] Figure 7 It is a schematic diagram of the structure obtained in step (10) of the present invention. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in further detail below.
[0043] The present invention provides a method for preparing a flip-chip LED chip, comprising the following steps:
[0044] (1) Figure 1 As shown, an epitaxial wafer is provided, which includes a substrate 10 and a first semiconductor layer 11, a multi-quantum well layer 12 and a second semiconductor layer 13 sequentially deposited on the substrate 10.
[0045] The substrate may be a sapphire substrate, a SiC substrate, a ZnO substrate, or a Si substrate, but is not limited thereto.
[0046] The first semiconductor layer, the multi-quantum well layer, and the second semiconductor layer are deposited on the substrate by MOCVD. The material of the first semiconductor layer can be GaN or AlGaN, but is not limited thereto. In one embodiment, the first semiconductor layer is a Si-doped N-type GaN layer with a thickness of 3 μm to 8 μm and a Si doping concentration of 5×10 18 cm -3 ~1×10 19 cm -3 The material of the second semiconductor layer may be GaN or AlGaN, but is not limited thereto. In one embodiment, the second semiconductor layer is a Mg-doped P-type GaN layer with a thickness of 200 nm to 300 nm and a Mg doping concentration of 5×10 17 cm -3 ~1×10 20 cm -3 The multi-quantum well layer may be an InGaN / GaN multi-quantum well layer, an InGaN / AlGaN multi-quantum well layer, or an AlGaN / AlGaN multi-quantum well layer, but is not limited thereto. The thickness of the multi-quantum well layer is 50 nm to 300 nm. In one embodiment, the multi-quantum well layer is an InGaN / GaN multi-quantum well layer.
[0047] (2) Etching the epitaxial wafer to obtain a MESA step exposing the first semiconductor layer.
[0048] (3) A first electrode 15a is formed on the MESA step, and a current spreading layer 14 and a second electrode 15b are formed on the second semiconductor layer.
[0049] The material of the current spreading layer is ITO, ZnO, AZO, FTO, but not limited thereto. In one embodiment, the material of the current spreading layer is ITO, and the thickness is 10nm to 150nm.
[0050] The first electrode and the second electrode are generally a combined stacked structure of metals such as Cr, Ti, Ni, Pt, Au, Al, and Cu.
[0051] (4) Depositing a reflective layer and opening holes to expose the first electrode and the second electrode, forming a first solder pad 17a and a second solder pad 17b on the first electrode and the second electrode respectively, to obtain an LED chip.
[0052] The material of the reflective layer can be Al 2 O 3 、SiO 2 、Si 3 N 4 MgF 2、TiO 2 、Ti 2 O 5 In one embodiment, the reflective layer is SiO 2 and TiO 2 The periodic overlapping structure has a period number of 30 to 60. The reflective layer is formed by evaporation, sputtering or coating.
[0053] (5) Figure 2 As shown, a first bonding layer 18 is prepared on the surface of the LED chip and a hole is opened to expose the first pad and the second pad.
[0054] The material of the first bonding layer may be an insulating material such as high-strength adhesive, silicon oxide, etc., but is not limited thereto.
[0055] The holes are opened to leave holes above the first pad and the second pad, so as to absorb bubbles in the bonding layer and thus improve the bonding strength.
[0056] (6) Figure 3 As shown, a substrate 20 with a second bonding layer 21 is provided, and the substrate is bonded to the LED chip through the first bonding layer and the second bonding layer.
[0057] The material of the second bonding layer can be an insulating material such as high-strength adhesive, silicon oxide, etc., but is not limited thereto. The second bonding layer can be made of the same or different material as the first bonding layer, and the second bonding layer is closely connected to the first bonding layer to complete the bonding between the substrate and the LED chip. The material of the substrate can be Si or glass, but is not limited thereto. Accordingly, the bonding method between the LED chip and the substrate can be direct bonding or adhesive bonding, but is not limited thereto. The transfer substrate is conducive to the subsequent peeling of the substrate and the thinning of the first semiconductor layer.
[0058] (7) Figure 4 As shown, the substrate is peeled off and the first semiconductor layer is thinned.
[0059] The substrate stripping method may be mechanical grinding, dry etching, or wet etching, but is not limited thereto.
[0060] The thinning method of the first semiconductor layer can be mechanical grinding, dry etching, wet etching, but not limited to this. The thickness of the thinned first semiconductor layer is 1μm to 3μm. If the thickness is less than 1μm, it is easy to damage the epitaxial structure of the multi-quantum well layer, resulting in a significant reduction in luminous efficiency; if the thickness is greater than 3μm, the brightness of the LED chip will not be significantly improved. Exemplary examples are 1.5μm, 1.8μm, 2μm, 2.5μm or 2.8μm, but not limited to this.
[0061] Compared with the thinning and stripping of the substrate, the thinning of the first semiconductor layer has more stringent quality requirements. Dry etching and wet etching will cause damage such as increased film defects and increased ohmic contact resistance, affecting the performance of the device; low-damage etching technology has the problem of slow etching speed, resulting in extended process and increased costs.
[0062] In one embodiment, in step (7), the first semiconductor layer is thinned by mechanical grinding and chemical mechanical polishing.
[0063] The grinding pressure of the mechanical grinding is 1kPa to 5kPa, the grinding disc speed is 40r / min to 80r / min, the average particle size of the abrasive in the grinding liquid is 1μm to 10μm, and after mechanical grinding, the surface roughness of the first semiconductor layer is 0.1μm to 5μm. The first semiconductor layer is thinned by mechanical grinding, and the average grinding rate can be increased to 18μm / h to 25μm / h by controlling the pressure, speed and abrasive particle size of the mechanical grinding.
[0064] The polishing pressure of the chemical mechanical polishing is 5kPa to 12kPa, the polishing disc speed is 60r / min to 120r / min, the pH of the polishing liquid is 9 to 12, the average particle size of the abrasive in the polishing liquid is 50nm to 70nm, and after chemical mechanical polishing, the surface roughness of the first semiconductor layer is 0.5nm to 5nm. After mechanical grinding, there will be scratches on the surface of the first semiconductor layer, and the surface roughness is further reduced by chemical mechanical polishing. Since the surface roughness is controlled at 0.1μm to 5μm after mechanical grinding, the time of chemical mechanical polishing can be shortened. Combined with the pressure, speed, pH of the polishing liquid and the abrasive particle size of the chemical mechanical polishing, the average polishing rate can be increased to 240nm / h to 280nm / h.
[0065] Preferably, the mechanical grinding includes a first mechanical grinding and a second mechanical grinding, so as to further improve the grinding efficiency.
[0066] Specifically, the grinding pressure of the first mechanical grinding is 1 kPa to 5 kPa, the grinding disc speed is 40 r / min to 80 r / min, the average particle size of the abrasive in the grinding liquid is 5 μm to 10 μm, and after mechanical grinding, the thickness of the first semiconductor layer is reduced by 30% to 50%, and the surface roughness is 1 μm to 5 μm;
[0067] The grinding pressure of the second mechanical grinding is 1kPa-5kPa, the grinding disc speed is 40r / min-80r / min, the average particle size of the abrasive in the grinding liquid is 1μm-5μm, and after mechanical grinding, the surface roughness of the first semiconductor layer is 0.1μm-1μm.
[0068] In one embodiment, after the first semiconductor layer is thinned, the first semiconductor layer is cleaned to remove abrasive particles. Specifically, the first semiconductor layer can be cleaned with deionized water, and then ultrasonically cleaned in acetone and isopropanol for 2 minutes to 5 minutes.
[0069] (8) Figure 5 As shown, a light emitting layer is deposited on the thinned first semiconductor layer.
[0070] The material of the light-emitting layer includes Al 2 O 3 、SiO 2 、Si 3 N 4 MgF 2 、TiO 2 and Ti 2 O 5 One or more of the above. The thickness of the light emitting layer is 50nm to 1200nm. The light emitting layer is formed by evaporation, sputtering or coating. The light emitting layer protects the GaN epitaxial structure from being damaged by air on the one hand, and can expand the light emitting angle on the other hand.
[0071] Preferably, the light-emitting layer comprises Al 2 O 3 Layer 31 and SiO 2 Layer 32, Al 2 O 3 The thickness of the layer is 30nm~500nm, SiO 2 The thickness of the layer is 30nm to 500nm. GaN, Al 2 O 3 and SiO 2 The refractive indices of the three materials decrease successively, which is beneficial to further increase the light output angle and reduce the interface reflected light.
[0072] (9) Figure 6 As shown, the substrate is thinned and a hole is opened to expose the first pad and the second pad.
[0073] Before opening holes in the substrate, the surface of the substrate may be subjected to surface treatment, wherein the surface treatment includes oxidation treatment and / or evaporation of an insulating layer, so that the surface of the substrate exposed to air has higher insulation properties.
[0074] (10) Figure 7 As shown, solder paste 41 is filled into the hole on the surface of the substrate, and forms an ohmic contact with the first solder pad and the second solder pad to obtain a flip-chip LED chip.
[0075] The solder paste and the first soldering pad and the second soldering pad are tightly combined through a reflow soldering process to obtain good ohmic contact.
[0076] The present invention also provides a flip-chip LED chip, which is prepared by the above-mentioned method for preparing the flip-chip LED chip. The flip-chip LED chip has high luminous efficiency.
[0077] The present invention will be further described below with specific embodiments:
[0078] Example 1
[0079] This embodiment provides a method for preparing a flip-chip LED chip, comprising the following steps:
[0080] (1) An epitaxial wafer is provided, wherein the epitaxial wafer includes a sapphire substrate and a Si-doped N-type GaN layer, an InGaN / GaN multi-quantum well layer and a Mg-doped P-type GaN layer sequentially deposited on the sapphire substrate.
[0081] The thickness of the Si-doped N-type GaN layer is 6 μm, and the Si doping concentration is 5×10 18 cm -3 The thickness of the Mg-doped P-type GaN layer is 200 nm, and the Mg doping concentration is 5×10 19 cm -3 The thickness of the InGaN / GaN multi-quantum well layer is 240nm.
[0082] (2) Etching the epitaxial wafer to obtain a MESA step that exposes the first semiconductor layer.
[0083] (3) A first electrode is formed on the MESA step, and an ITO current spreading layer and a second electrode are formed on the second semiconductor layer.
[0084] The thickness of the ITO current spreading layer is 80 nm.
[0085] (4) depositing a reflective layer and opening holes to expose the first electrode and the second electrode, and forming a first soldering pad and a second soldering pad on the first electrode and the second electrode, respectively, to obtain an LED chip.
[0086] The reflective layer is SiO 2 and TiO 2 Periodic overlapping structure with 40 periods.
[0087] (5) Prepare a first bonding layer on the surface of the LED chip and open a hole to expose the first pad and the second pad.
[0088] The material of the first bonding layer is SiO 2 .
[0089] (6) Providing a substrate with a second bonding layer, and bonding the substrate to the LED chip via the first bonding layer and the second bonding layer.
[0090] The material of the second bonding layer is SiO2 , the material of the substrate is Si. The LED chip is directly bonded to the substrate.
[0091] (7) The substrate is peeled off and the first semiconductor layer is thinned.
[0092] The first semiconductor layer is thinned by mechanical grinding and chemical mechanical polishing.
[0093] The grinding pressure of mechanical grinding is 4 kPa, the grinding disc rotation speed is 50 r / min, the average particle size of the abrasive in the grinding liquid is 5 μm, and after mechanical grinding, the surface roughness of the first semiconductor layer is 2.3 μm.
[0094] The polishing pressure of chemical mechanical polishing is 6 kPa, the rotation speed of the polishing disc is 100 r / min, the pH of the polishing liquid is 11, the average particle size of the abrasive in the polishing liquid is 60 nm, and after chemical mechanical polishing, the surface roughness of the first semiconductor layer is 1.9 nm.
[0095] The thickness of the first semiconductor layer after thinning is 2 μm.
[0096] (8) Depositing a light emitting layer on the thinned first semiconductor layer.
[0097] The light-emitting layer includes Al 2 O 3 Layer and SiO 2 Layer, Al 2 O 3 The thickness of the SiO layer is 120 nm. 2 The thickness of the layer is 100 nm.
[0098] (9) The substrate is thinned and a hole is opened to expose the first pad and the second pad.
[0099] Before opening holes in the substrate, the surface of the substrate is subjected to oxidation treatment.
[0100] (10) Fill the holes on the surface of the substrate with solder paste, and tightly combine the solder paste, the first solder pad, and the second solder pad through a reflow soldering process to obtain good ohmic contact.
[0101] Example 2
[0102] This embodiment provides a method for preparing a flip-chip LED chip, which is different from Embodiment 1 in that the mechanical grinding includes a first mechanical grinding and a second mechanical grinding.
[0103] The grinding pressure of the first mechanical grinding was 2 kPa, the grinding disc speed was 50 r / min, and the average particle size of the abrasive in the grinding liquid was 10 μm. After mechanical grinding, the thickness of the first semiconductor layer was reduced to 2.2 μm, and the surface roughness was 2.3 μm.
[0104] The grinding pressure of the second mechanical grinding is 4 kPa, the grinding disc speed is 40 r / min, the average particle size of the abrasive in the grinding liquid is 3 μm, and after mechanical grinding, the surface roughness of the first semiconductor layer is 0.6 μm.
[0105] The polishing pressure of chemical mechanical polishing is 6 kPa, the rotation speed of the polishing disc is 100 r / min, the pH of the polishing liquid is 11, the average particle size of the abrasive in the polishing liquid is 60 nm, and after chemical mechanical polishing, the surface roughness of the first semiconductor layer is 0.7 nm.
[0106] The rest are the same as in Example 1.
[0107] Example 3
[0108] This embodiment provides a method for preparing a flip-chip LED chip, which is different from Embodiment 1 in that the mechanical grinding includes a first mechanical grinding and a second mechanical grinding.
[0109] The grinding pressure of the first mechanical grinding was 4 kPa, the grinding disc speed was 50 r / min, and the average particle size of the abrasive in the grinding liquid was 6 μm. After mechanical grinding, the thickness of the first semiconductor layer was reduced to 2.5 μm, and the surface roughness was 2.1 μm.
[0110] The grinding pressure of the second mechanical grinding is 4 kPa, the grinding disc speed is 50 r / min, the average particle size of the abrasive in the grinding liquid is 1 μm, and after mechanical grinding, the surface roughness of the first semiconductor layer is 0.3 μm.
[0111] The polishing pressure of chemical mechanical polishing is 6 kPa, the polishing disc rotation speed is 100 r / min, the pH of the polishing liquid is 11, the average particle size of the abrasive in the polishing liquid is 60 nm, and after chemical mechanical polishing, the surface roughness of the first semiconductor layer is 0.4 nm.
[0112] The rest are the same as in Example 1.
[0113] The photoelectric performance of the flip-chip LED chips obtained in Examples 1 to 3 was tested. Compared with the traditional flip-chip LED chips, the luminous brightness can be improved by 1.5% to 4.7%.
[0114] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. A method for preparing a flip-chip LED chip, characterized in that: The following steps are involved: (1) providing an epitaxial wafer, the epitaxial wafer comprising a substrate and a first semiconductor layer, a multi-quantum well layer, and a second semiconductor layer sequentially deposited on the substrate; (2) etching the epitaxial wafer to obtain a MESA step exposing the first semiconductor layer; (3) forming a first electrode on the MESA step, and forming a current spreading layer and a second electrode on the second semiconductor layer; (4) depositing a reflective layer and opening a hole to expose the first electrode and the second electrode, and forming a first soldering pad and a second soldering pad on the first electrode and the second electrode, respectively, to obtain an LED chip; (5) preparing a first bonding layer on the surface of the LED chip and opening a hole to expose the first pad and the second pad; (6) providing a substrate with a second bonding layer, and bonding the substrate to the LED chip through the first bonding layer and the second bonding layer; (7) peeling off the substrate and thinning the first semiconductor layer; (8) depositing a light emitting layer on the thinned first semiconductor layer; (9) thinning the substrate and opening a hole to expose the first pad and the second pad; (10) Fill the holes on the surface of the substrate with solder paste and form ohmic contact with the first solder pad and the second solder pad to obtain a flip-chip LED chip.
2. The method for preparing a flip-chip LED chip according to claim 1, characterized in that: The thickness of the thinned first semiconductor layer is 1 μm to 3 μm.
3. The method for preparing a flip-chip LED chip according to claim 1, characterized in that: In step (7), the first semiconductor layer is thinned by mechanical grinding and chemical mechanical polishing; The grinding pressure of the mechanical grinding is 1 kPa to 5 kPa, the grinding disc speed is 40 r / min to 80 r / min, the average particle size of the abrasive in the grinding liquid is 1 μm to 10 μm, and after mechanical grinding, the surface roughness of the first semiconductor layer is 0.1 μm to 5 μm; The polishing pressure of the chemical mechanical polishing is 5kPa~12kPa, the polishing disk rotation speed is 60r / min~120r / min, the pH of the polishing liquid is 9~12, the average particle size of the abrasive in the polishing liquid is 50nm~70nm, and after chemical mechanical polishing, the surface roughness of the first semiconductor layer is 0.5nm~5nm.
4. The method for preparing a flip-chip LED chip according to claim 3, characterized in that: The mechanical grinding includes a first mechanical grinding and a second mechanical grinding; The grinding pressure of the first mechanical grinding is 1 kPa to 5 kPa, the grinding disc speed is 40 r / min to 80 r / min, the average particle size of the abrasive in the grinding liquid is 5 μm to 10 μm, and after the first mechanical grinding, the thickness of the first semiconductor layer is reduced by 30% to 50%, and the surface roughness is 1 μm to 5 μm; The grinding pressure of the second mechanical grinding is 1kPa-5kPa, the grinding disc speed is 40r / min-80r / min, the average particle size of the abrasive in the grinding liquid is 1μm-5μm, and after the second mechanical grinding, the surface roughness of the first semiconductor layer is 0.1μm-1μm.
5. The method for preparing a flip-chip LED chip according to claim 1, characterized in that: After the first semiconductor layer is thinned, the first semiconductor layer is cleaned.
6. The method for preparing a flip-chip LED chip according to claim 1, characterized in that: The material of the light-emitting layer includes one or more of Al2O3, SiO2, Si3N4, MgF2, TiO2 and Ti2O5; The thickness of the light-emitting layer is 50nm-1200nm.
7. The method for preparing a flip-chip LED chip according to claim 6, characterized in that: The light-emitting layer comprises an Al2O3 layer and a SiO2 layer deposited in sequence, and the thickness of the Al2O3 layer and the SiO2 layer are both 30nm to 500nm.
8. The method for preparing a flip-chip LED chip according to claim 1, characterized in that: The method further includes performing surface treatment on the surface of the substrate, wherein the surface treatment includes oxidation treatment and / or evaporation of an insulating layer.
9. The method for preparing a flip-chip LED chip according to claim 1, wherein: The LED chip and the substrate are bonded by direct bonding or adhesive bonding.
10. A flip-chip LED chip, characterized in that: The flip-chip LED is manufactured by the method for manufacturing a flip-chip LED chip according to any one of claims 1 to 9.