Preparation method of electrode material based on high-reflection silver-containing film layer

By using the preparation method of silver-tin composite plating in LED electrode materials, the annealing process is used to drive tin atoms into the silver layer and form a tin oxide film to isolate the chemical reaction between sulfur ions and silver ions, and the low photoelectric conversion efficiency and silver reflection of LED are solved. The problem of poor film stability achieves high reflectivity and high temperature resistance.

CN118943264APending Publication Date: 2024-11-12FANGBO TECHNOLOGY (CHANGZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410878028.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The photoelectric conversion efficiency of existing LEDs is low. The silver reflective film is prone to react with sulfur in the environment to form sulfide during use, resulting in a decrease in reflectivity and affecting the light output efficiency and stability of the LED.

Method used

Using the preparation method based on the high reflective silver-containing film electrode material, by methylsulfonic acid, stannous methylsulfonate, polyethylene glycol octylphenyl ether, benzyl acetone, potassium pyrophosphate, potassium carbonate, Niacin, silver nitrate and 5,5-dimethylhydantoin are mixed to form tin plating and silver plating liquid. After tin plating, silver plating and microwave annealing, a silver tin composite plating layer is generated, and the annealing process is driven Tin atoms enter the silver layer, form intermetallic compounds and form tin oxide films to isolate the chemical reaction between sulfur ions and silver ions.

Benefits of technology

The anti-vulcanization effect is achieved, the reflectivity and high temperature resistance of LEDs are improved, the agglomeration behavior of silver ions is reduced, and the energy utilization rate and the stability of electrode materials are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a preparation method of an electrode material based on a high-reflection silver-containing film layer, and relates to the technical field of electrode materials. Tin atoms are driven to enter the silver layer and even reach the top of the surface of the silver layer by utilizing the annealing process and the difference between the free energy of the surfaces of silver and tin, at the moment, the tin atoms and the silver atoms are mutually diffused, an intermetallic compound is generated on the upper layer of the composite film, and the tin atoms on the surface of the composite film react with oxygen in the heat treatment process. According to the preparation method, silver ions and silver ions are combined, a tin oxide film is formed, so that chemical reaction between the sulfur ions and the silver ions in the environment is isolated, the anti-vulcanization effect of a matrix is achieved, meanwhile, when the temperature of a device is increased during LED working, free energy in the whole system is not affected, the agglomeration behavior of the silver ions is reduced, the reflectivity of the matrix is improved, and the high-temperature-resistant effect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrode materials, and in particular to a method for preparing a high-reflective silver-containing film electrode material. Background Art

[0002] Since the 20th century, due to the rapid development of industrial technology, people's exploitation and utilization of natural resources has increased significantly, resulting in a sharp decline in the reserves of non-renewable energy such as coal, crude oil, and natural gas, and the rapid deterioration of the ecological environment on which organisms depend for survival, and various diseases have also followed. Therefore, in this era of increasing energy demand, all countries are vigorously advocating energy conservation, emission reduction, and low-carbon living. Compared with the shortcomings of traditional lighting fixtures such as large energy loss and poor light quality due to their light-emitting mode, light-emitting diodes (LEDs) emit light through electro-optical conversion and excitation of photons. They have the advantages of green environmental protection, small light source size, high reliability in harsh environments, long working time, and low energy loss.

[0003] The photoelectric conversion efficiency of LED can reach 100% in theory, but in actual lighting, it is found that the photoelectric conversion ratio of LED is far lower than the theoretical conversion value, only about 20% of the ideal conversion rate. This not only restricts the development of LED, but also causes the loss of electric energy and waste of energy. Therefore, for the purpose of energy saving, emission reduction and environmental protection, it is necessary to improve the light output efficiency of LED to improve energy utilization; usually, the reflectivity of silver reflective film to visible light is above 97%, and the stability is good, but during the LED assembly process or operation, silver will react with sulfur in the environment to generate sulfide, that is, silver sulfide. The generation of silver sulfide will cause the silver reflective film to lose its metallic luster, causing the reflectivity of the reflective film to drop sharply or even lose its reflective properties; therefore, it is particularly necessary to invent an electrode material based on a high-reflection silver-containing film layer. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a highly reflective silver-containing film electrode material to solve the problems existing in the prior art.

[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for preparing a highly reflective silver-containing film electrode material, comprising the following preparation steps: 1. A method for preparing a highly reflective silver-containing film electrode material, comprising the following steps: (1) Mix methanesulfonic acid with half of the total mass of deionized water, stir at 60 rpm until the solution cools to room temperature, add stannous methanesulfonate, polyethylene glycol octylphenyl ether, benzyl acetone, resorcinol and the remaining deionized water, mix well, and obtain a tin plating solution; (2) Mix potassium pyrophosphate, potassium carbonate, nicotinic acid, silver nitrate, 5,5-dimethylhydantoin, 0.1wt% 2,2'-bipyridine aqueous solution, and deionized water, stir at 100 rpm until completely dissolved, and add ammonia water to obtain a silver plating solution; (3) placing the cathode in a tin plating solution for tin plating, then rinsing with deionized water, and drying with cold air, placing the cathode in a silver plating solution for silver plating, and rinsing with deionized water again, and drying with cold air to obtain a silver-tin composite coating; (4) The silver-tin composite coating is annealed under microwave assistance to obtain a highly reflective silver-containing film electrode material.

[0006] Furthermore, in step (1), the mass ratio of methanesulfonic acid, stannous methanesulfonate, polyethylene glycol octylphenyl ether, benzyl acetone, resorcinol, and deionized water is 1.4:5:0.6:0.1:0.5:65.

[0007] Furthermore, in step (2), the mass ratio of potassium pyrophosphate, potassium carbonate, nicotinic acid, silver nitrate, 5,5-dimethylhydantoin, 0.1wt% 2,2'-bipyridine aqueous solution, deionized water, and ammonia water is 4.5:7:10:4:6:0.5:64:3.2.

[0008] Furthermore, the cathode in step (3) is made of copper.

[0009] Furthermore, the flushing time in step (3) is 10 to 15 seconds.

[0010] Furthermore, the drying temperature in step (3) is 10-20° C. and the drying time is 1-3 h.

[0011] Furthermore, the temperature of the plating solution in step (3) is 25-45°C.

[0012] Furthermore, the current density of the tin plating in step (3) is 1.5A / dm 2 , the current density of silver plating is 0.5A / dm 2 .

[0013] Furthermore, in step (3), the tin plating time is 8 minutes and the silver plating time is 4 minutes.

[0014] Furthermore, in step (4), the microwave power is 100-200 W, the annealing temperature is 150° C., and the time is 20-35 min.

[0015] Compared with the prior art, the beneficial effects achieved by the present invention are: The present invention utilizes the difference in free energy between the annealing process and the surface of silver and tin to drive tin atoms into the silver layer, and even to drive them to reach the top of the silver layer surface. At this time, mutual diffusion occurs between the tin atoms and the silver atoms, and intermetallic compounds are generated in the upper layer of the composite film. During the heat treatment process, the tin atoms on the surface of the composite film react with oxygen to form a tin oxide film, thereby isolating the chemical reaction between the sulfur ions and the silver ions in the environment, so that the substrate achieves an anti-sulfurization effect. At the same time, when the temperature of the device is increased during the operation of the LED, the free energy in the entire system is not affected, thereby reducing the agglomeration behavior of the silver ions, improving the reflectivity of the substrate, and achieving a high temperature resistance effect. DETAILED DESCRIPTION

[0016] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0017] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the high-reflection silver-containing film electrode material prepared in the following examples are as follows: Anti-sulfurization property: Take the embodiment and comparative example of the same size, soak them in a 5wt% sodium sulfide aqueous solution for 12 hours, then take them out and observe whether the samples change color, and perform a reflectivity test at a wavelength of 650nm.

[0018] High temperature resistance: The embodiment and the comparative example of the same size were placed at 300°C for 1000 hours, and then the reflectivity was tested at a wavelength of 650nm.

[0019] Example 1; (1) Mix methanesulfonic acid with half the total mass of deionized water, stir at 60 rpm until the solution cools to room temperature, add stannous methanesulfonate, polyethylene glycol octylphenyl ether, benzyl acetone, resorcinol and the remaining deionized water, mix well, and obtain a tin plating solution; the mass ratio of methanesulfonic acid, stannous methanesulfonate, polyethylene glycol octylphenyl ether, benzyl acetone, resorcinol and deionized water is 1.4:5:0.6:0.1:0.5:65; (2) Mix potassium pyrophosphate, potassium carbonate, nicotinic acid, silver nitrate, 5,5-dimethylhydantoin, 0.1wt% 2,2'-bipyridine aqueous solution, and deionized water, stir at 100rpm until completely dissolved, and add ammonia water to obtain a silver plating solution; the mass ratio of potassium pyrophosphate, potassium carbonate, nicotinic acid, silver nitrate, 5,5-dimethylhydantoin, 0.1wt% 2,2'-bipyridine aqueous solution, deionized water, and ammonia water is 4.5:7:10:4:6:0.5:64:3.2; (3) Place the copper cathode material in a tinning solution for tinning at 25°C with a current density of 1.5A / dm 2 The time was 8 minutes, followed by rinsing with deionized water for 10 seconds, drying with cold air at 10°C for 1 hour, and silver plating in a silver plating solution with a current density of 0.5A / dm 2 , the time is 4min, rinsed again with deionized water for 10s, and dried with cold air at 10℃ for 1h to obtain a silver-tin composite coating; (4) The silver-tin composite coating is annealed at 150° C. and a microwave power of 100 W for 20 min to obtain a highly reflective silver-containing film electrode material.

[0020] Example 2; (1) Mix methanesulfonic acid with half the total mass of deionized water, stir at 60 rpm until the solution cools to room temperature, add stannous methanesulfonate, polyethylene glycol octylphenyl ether, benzyl acetone, resorcinol and the remaining deionized water, mix well, and obtain a tin plating solution; the mass ratio of methanesulfonic acid, stannous methanesulfonate, polyethylene glycol octylphenyl ether, benzyl acetone, resorcinol and deionized water is 1.4:5:0.6:0.1:0.5:65; (2) Mix potassium pyrophosphate, potassium carbonate, nicotinic acid, silver nitrate, 5,5-dimethylhydantoin, 0.1wt% 2,2'-bipyridine aqueous solution, and deionized water, stir at 100rpm until completely dissolved, and add ammonia water to obtain a silver plating solution; the mass ratio of potassium pyrophosphate, potassium carbonate, nicotinic acid, silver nitrate, 5,5-dimethylhydantoin, 0.1wt% 2,2'-bipyridine aqueous solution, deionized water, and ammonia water is 4.5:7:10:4:6:0.5:64:3.2; (3) Place the copper cathode material in a tinning solution at 35°C for tinning at a current density of 1.5A / dm 2 The time was 8 minutes, followed by rinsing with deionized water for 13 seconds, drying with cold air at 15°C for 2 hours, and silver plating in a silver plating solution with a current density of 0.5A / dm 2 , the time is 4min, and then rinsed with deionized water for 13s, and dried with cold air at 15℃ for 2h to obtain a silver-tin composite coating; (4) The silver-tin composite coating is annealed at 150° C. and a microwave power of 150 W for 30 min to obtain a highly reflective silver-containing film electrode material.

[0021] Example 3; (1) Mix methanesulfonic acid with half the total mass of deionized water, stir at 60 rpm until the solution cools to room temperature, add stannous methanesulfonate, polyethylene glycol octylphenyl ether, benzyl acetone, resorcinol and the remaining deionized water, mix well, and obtain a tin plating solution; the mass ratio of methanesulfonic acid, stannous methanesulfonate, polyethylene glycol octylphenyl ether, benzyl acetone, resorcinol and deionized water is 1.4:5:0.6:0.1:0.5:65; (2) Mix potassium pyrophosphate, potassium carbonate, nicotinic acid, silver nitrate, 5,5-dimethylhydantoin, 0.1wt% 2,2'-bipyridine aqueous solution, and deionized water, stir at 100rpm until completely dissolved, and add ammonia water to obtain a silver plating solution; the mass ratio of potassium pyrophosphate, potassium carbonate, nicotinic acid, silver nitrate, 5,5-dimethylhydantoin, 0.1wt% 2,2'-bipyridine aqueous solution, deionized water, and ammonia water is 4.5:7:10:4:6:0.5:64:3.2; (3) Place the copper cathode material in a tinning solution at 45°C for tinning at a current density of 1.5A / dm 2 The time was 8 minutes, followed by rinsing with deionized water for 15 seconds, drying with cold air at 20°C for 3 hours, and silver plating in a silver plating solution with a current density of 0.5A / dm 2 , the time is 4min, and then rinsed with deionized water for 15s, and dried with cold air at 20℃ for 3h to obtain a silver-tin composite coating; (4) The silver-tin composite coating was annealed at 150° C. for 35 min under the conditions of 150° C. and a microwave power of 200 W to obtain a highly reflective silver-containing film electrode material.

[0022] Effect example Table 1 below shows the performance analysis results of the high-reflective silver-containing film electrode materials according to Examples 1 to 3 of the present invention.

[0023] Table 1

[0024] From the comparison of the experimental results of the embodiments in Table 1, it can be found that the present invention utilizes the difference in the annealing process and the surface free energy of silver and tin to drive the tin atoms into the silver layer, and even to drive them to the top of the silver layer surface. At this time, mutual diffusion occurs between the tin atoms and the silver atoms, and intermetallic compounds are generated in the upper layer of the composite film. During the heat treatment process, the tin atoms on the surface of the composite film react with oxygen to form a tin oxide film, thereby isolating the chemical reaction between the sulfur ions and the silver ions in the environment, so that the matrix can achieve an anti-sulfurization effect. At the same time, when the temperature of the device is increased during the operation of the LED, the free energy in the entire system is not affected, thereby reducing the agglomeration behavior of the silver ions, improving the reflectivity of the matrix, and achieving a high temperature resistance effect.

[0025] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A method for preparing a highly reflective silver-containing film electrode material, characterized in that: The method comprises the following preparation steps: (1) Mix methanesulfonic acid with half of the total mass of deionized water, stir at 60 rpm until the solution cools to room temperature, add stannous methanesulfonate, polyethylene glycol octylphenyl ether, benzyl acetone, resorcinol and the remaining deionized water, mix well, and obtain a tin plating solution; (2) Mix potassium pyrophosphate, potassium carbonate, nicotinic acid, silver nitrate, 5,5-dimethylhydantoin, 0.1wt% 2,2'-bipyridine aqueous solution, and deionized water, stir at 100 rpm until completely dissolved, and add ammonia water to obtain a silver plating solution; (3) placing the cathode in a tin plating solution for tin plating, then rinsing with deionized water, and drying with cold air, placing the cathode in a silver plating solution for silver plating, and rinsing with deionized water again, and drying with cold air to obtain a silver-tin composite coating; (4) The silver-tin composite coating is annealed under microwave assistance to obtain a highly reflective silver-containing film electrode material.

2. The method for preparing a highly reflective silver-containing film electrode material according to claim 1, characterized in that: The mass ratio of the methanesulfonic acid, stannous methanesulfonate, polyethylene glycol octylphenyl ether, benzyl acetone, resorcinol and deionized water in step (1) is 1.4:5:0.6:0.1:0.5:

65.

3. The method for preparing a highly reflective silver-containing film electrode material according to claim 1, characterized in that: In step (2), the mass ratio of potassium pyrophosphate, potassium carbonate, nicotinic acid, silver nitrate, 5,5-dimethylhydantoin, 0.1wt% 2,2'-bipyridine aqueous solution, deionized water, and ammonia water is 4.5:7:10:4:6:0.5:64:3.

2.

4. The method for preparing a highly reflective silver-containing film electrode material according to claim 1, characterized in that: The cathode in step (3) is made of copper.

5. The method for preparing a highly reflective silver-containing film electrode material according to claim 1, characterized in that: The flushing time in step (3) is 10 to 15 seconds.

6. The method for preparing a highly reflective silver-containing film electrode material according to claim 1, characterized in that: The drying temperature in step (3) is 10-20°C and the drying time is 1-3 hours.

7. The method for preparing a highly reflective silver-containing film electrode material according to claim 1, characterized in that: The temperature of the plating solution in step (3) is 25-45°C.

8. The method for preparing a highly reflective silver-containing film electrode material according to claim 1, characterized in that: The current density of the tinning in step (3) is 1.5A / dm 2 , the current density of silver plating is 0.5A / dm 2 .

9. The method for preparing a highly reflective silver-containing film electrode material according to claim 1, characterized in that: The tin plating time in step (3) is 8 minutes and the silver plating time is 4 minutes.

10. The method for preparing a highly reflective silver-containing film electrode material according to claim 1, characterized in that: In step (4), the microwave power is 100-200 W, the annealing temperature is 150° C., and the time is 20-35 min.