Low-resistance composite current collector and preparation method and application thereof
By pretreating acetone on metal copper foil and modifying three-dimensional conductive graphene, the problem of poor binding effect of the negative electrode current collector and active substances of lithium-ion batteries is solved, improving the battery's magnification and cycling performance, improving the conductivity and stability .
Patent Information
- Application Number
- CN202411344108.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-12
AI Technical Summary
The interface bonding effect of the negative electrode current collector and active substance of lithium-ion battery is poor, resulting in a decrease in battery magnification and cycling performance.
The metal copper foil was pretreated using acetone and the three-dimensional conductive network graphene was modified on its surface. The three-dimensional conductive nanosheet graphene was generated by plasma-enhanced chemical vapor deposition method to enhance the binding force between the active substance and the current collector and Conductivity.
It significantly reduces the internal resistance of the battery, improves the magnification and cycling performance, and enhances the stability and conductivity of the current collector.
Smart Images

Figure CN118943276A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of chemical energy storage batteries, and in particular to a low-resistance composite current collector, a preparation method thereof and applications thereof. Background Art
[0002] As a new generation of chemical storage batteries, lithium-ion batteries have the advantages of high energy density, long cycle life, low self-discharge rate, green environmental protection and no memory effect. They have been widely used in electronics, electric vehicles, medical equipment, aerospace and other fields.
[0003] In recent years, industries such as artificial intelligence, big data, and electric vehicles have developed rapidly, and the requirements for the electrochemical performance of lithium-ion batteries (such as capacity, rate, and cycle performance) have been increasing. Lithium-ion batteries are mainly composed of positive and negative electrode materials, current collectors, separators, and electrolytes. Among them, the current collector plays the role of carrying active substances and collecting current, and is a very important factor affecting the performance of batteries. In addition to requiring a strong bonding force between the current collector and the active material coating, the current collector is also required to have good electronic conductivity and high chemical stability.
[0004] Metal copper foil has good mechanical strength and ductility, and low internal resistance. It is one of the most commonly used current collectors in the lithium-ion battery industry. However, the negative electrode current collector of lithium-ion batteries is generally a copper foil with a smooth and clean surface. It does not adhere firmly to the active material and has poor interface bonding. During repeated charge and discharge, it is easy to cause the active material to fall off, resulting in a decrease in the battery's rate and cycle.
[0005] Therefore, the present application first uses acetone to pretreat the metal copper foil, and by modifying a layer of three-dimensional conductive network on the surface of the metal copper foil, the interface bonding effect between the active substance and the current collector is improved, the internal resistance of the battery is reduced, and the rate and cycle performance of the battery are improved. Summary of the invention
[0006] The present invention aims to provide a low-resistance composite current collector, a preparation method and an application thereof. Acetone is used to pretreat the metal copper foil, and a three-dimensional conductive network is modified on the surface of the metal copper foil to enhance the interface bonding effect between the active material and the current collector, thereby reducing the internal resistance of the battery and improving the rate and cycle performance of the battery.
[0007] In order to achieve the above object, the present invention provides the following technical solutions: A method for preparing a low-resistance composite current collector comprises the following steps: S1. Soak the smooth copper foil in acetone for 1 to 2 hours for pretreatment, and dry it under vacuum at 60 to 80°C for 24 to 48 hours; S2. Place the treated copper foil in a quartz tube and heat it to 1000-1200°C in an inert gas atmosphere. The flow rate of the inert gas is 80-100 sccm and the heating rate is 25-28°C / min. After the temperature reaches 1000-1200°C, introduce CH4 gas with a flow rate of 20-50 sccm and keep it at this temperature for 15-30 min respectively. S3. After the reaction is completed, the sample is naturally cooled to room temperature under an inert gas atmosphere to obtain a composite copper current collector modified with three-dimensional conductive nanosheet graphene.
[0008] Working principle and beneficial effects of the present invention: This scheme first uses acetone to pretreat the smooth metal copper foil to remove the oxide layer and adsorbed impurities on the surface of the copper foil, which is convenient for improving the bonding strength between graphene and copper foil and improving the stability and conductivity of the current collector. Then, a layer of three-dimensional conductive network graphene is modified on the surface of the smooth metal copper foil by plasma enhanced chemical vapor deposition. This method is to generate three-dimensional conductive nanosheet graphene by pyrolysis of CH4 at high temperature, and directly grow on the surface of smooth metal copper foil. There is good bonding strength between graphene and copper current collector, and the addition of graphene improves the conductivity of the material, effectively improving the rate and cycle performance of lithium-ion batteries.
[0009] Preferably, the inert gas is Ar or N2.
[0010] Preferably, S1, immerse the smooth metal copper foil in acetone for 1 h for pretreatment, and dry it at 60°C under vacuum for 24 h; S2, place the treated metal copper foil in a quartz tube, heat it to 1000°C in an inert gas atmosphere, the inert gas flow rate is 80 sccm, the heating rate is 25°C / min, after the temperature reaches 1000°C, introduce CH4 gas, the CH4 flow rate is 20 sccm, and keep it at this temperature for 15 min respectively; S3, after the reaction is completed, cool the sample naturally to room temperature in an inert gas atmosphere to obtain a three-dimensional conductive nanosheet graphene modified composite copper current collector.
[0011] Preferably, S1, immerse the smooth metal copper foil in acetone for 2 h for pretreatment, and dry it under vacuum at 80°C for 48 h; S2, place the treated metal copper foil in a quartz tube, heat it to 1200°C in an inert gas atmosphere, the inert gas flow rate is 100 sccm, the heating rate is 28°C / min, after the temperature reaches 1200°C, introduce CH4 gas with a CH4 flow rate of 50 sccm, and keep it at this temperature for 30 min respectively; S3, after the reaction is completed, naturally cool the sample to room temperature in an inert gas atmosphere to obtain a three-dimensional conductive nanosheet graphene-modified composite copper current collector.
[0012] Preferably, S1, immerse the smooth metal copper foil in acetone for 1.5 h for pretreatment, and dry it under vacuum at 70°C for 36 h; S2, place the treated metal copper foil in a quartz tube, heat it to 1100°C in an inert gas atmosphere, the inert gas flow rate is 90 sccm, the heating rate is 26°C / min, after the temperature reaches 1100°C, introduce CH4 gas, the CH4 flow rate is 35 sccm, and maintain this temperature for 25 min respectively; S3, after the reaction is completed, cool the sample naturally to room temperature in an inert gas atmosphere to obtain a three-dimensional conductive nanosheet graphene modified composite copper current collector.
[0013] A composite copper current collector prepared by a method for preparing a low-resistance composite current collector.
[0014] The invention discloses an application of a composite copper current collector in a chemical energy storage battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a SEM image of the surface of the composite copper current collector modified with three-dimensional conductive nanosheet graphene; Figure 2 The comparative example and application example of the present invention are 0.1 C First charge and discharge curve; Figure 3 It is the EIS graph of the comparative example and the application example of the present invention; Figure 4 It is a magnification diagram of the comparative example and the application example of the present invention; Figure 5 It is a cycle comparison diagram of the comparative example and the application example of the present invention. DETAILED DESCRIPTION
[0016] The following is further described in detail through specific implementation methods: Embodiment 1: A method for preparing a low-resistance composite current collector, comprising the following steps: First, the smooth copper foil was pretreated by soaking it in acetone for 1 h and drying it under vacuum at 60°C for 24 h. After drying, the treated copper foil was placed in a quartz tube, and Ar was introduced. It was heated to 1000°C in an Ar atmosphere, with a gas flow rate of 80 sccm and a heating rate of 25°C min −1 After the temperature reached 1000°C, CH4 gas was introduced with a CH4 flow rate of 20 sccm, and the temperature was maintained for 15 min. After the reaction was completed, the sample was naturally cooled to room temperature under an Ar atmosphere to obtain a three-dimensional conductive nanosheet graphene-modified composite copper current collector, as shown in the SEM image. Figure 1 shown.
[0017] Embodiment 2: A method for preparing a low-resistance composite current collector, comprising the following steps: First, the smooth copper foil was pretreated by soaking it in acetone for 1 h and drying it under vacuum at 60°C for 24 h. After drying, the treated copper foil was placed in a quartz tube, N2 was introduced, and heated to 1000°C in a N2 atmosphere, with a gas flow rate of 80 sccm and a heating rate of 25°C min −1 After the temperature reaches 1000°C, CH4 gas is introduced with a CH4 flow rate of 50 sccm, and the temperature is maintained for 15 min. After the reaction is completed, the sample is naturally cooled to room temperature under a N2 atmosphere to obtain a three-dimensional conductive nanosheet graphene-modified composite copper current collector.
[0018] Example 3: First, the smooth metal copper foil was dried at 60°C under vacuum for 24 h. After drying, the treated metal copper foil was placed in a quartz tube, and Ar was introduced. The foil was heated to 1000°C in an Ar atmosphere, where the gas flow rate was 80 sccm and the heating rate was 25°C min −1 After the temperature reaches 1000°C, CH4 gas is introduced with a CH4 flow rate of 20 sccm, and the temperature is maintained for 15 min. After the reaction is completed, the sample is naturally cooled to room temperature in an Ar atmosphere to obtain a three-dimensional conductive nanosheet graphene-modified composite copper current collector.
[0019] Comparative Example: Ordinary copper foil without modification of three-dimensional conductive nanosheet graphene was used as the negative electrode current collector, commercial graphite was used as the active material, SP was used as the conductive agent, and PVDF was used as the binder. The weight ratio of graphite, SP and PVDF was 94.0:3.7:2.3. NMP was used as the solvent, and a uniformly mixed slurry was prepared by a planetary disperser, and then the slurry was evenly coated on the ordinary copper foil to obtain a negative electrode sheet. The electrode sheet was cut into an electrode disc with a diameter of 12 mm and used as a positive electrode for standby. A metal lithium sheet with a diameter of 14 mm was used as the counter electrode and reference electrode, a ceramic diaphragm with a model of CF15D and a diameter of 16 mm was used as the diaphragm, and 10 μL 1 mol / L LiPF6 / EC+DMC+DEC (volume ratio 1:1:1) was used as the electrolyte. In an argon-protected glove box, a 2016-type button half-cell was assembled, and the capacity, EIS, rate and cycle performance were tested.
[0020] Application Example 1: The three-dimensional conductive nanosheet graphene-modified composite copper foil prepared in Example 1 is used as the negative electrode current collector, commercial graphite is used as the active material, conductive carbon black (SP) is used as the conductive agent, and polyvinylidene fluoride (PVDF) is used as the binder. The graphite, SP and PVDF are weighed in a mass ratio of 94.0:3.7:2.3. N-methylpyrrolidine copper (NMP) is used as the solvent, and a uniformly mixed slurry is prepared by a planetary disperser, and then the slurry is evenly coated on the composite copper current collector to obtain a negative electrode sheet. The electrode sheet is cut into an electrode disc with a diameter of 12 mm and used as a positive electrode for standby use. Metal lithium sheets with a diameter of 14 mm were used as counter and reference electrodes, ceramic diaphragms with a model number of CF15D and a diameter of 16 mm were used as diaphragms, and 10 μL of 1 mol / L LiPF6 / EC+DMC+DEC (volume ratio of 1:1:1) were used as electrolytes. 2016-type button half-cells were assembled in an argon-protected glove box, and the capacity, electrochemical impedance spectroscopy (EIS), rate, and cycle performance were tested.
[0021] Application Example 2: The three-dimensional conductive nanosheet graphene modified composite copper foil prepared in Example 2 is used as the negative electrode current collector, commercial graphite is used as the active material, SP is used as the conductive agent, and PVDF is used as the binder. The graphite, SP and PVDF are weighed according to the mass ratio of 94.0:3.7:2.3. NMP is used as the solvent, and a uniformly mixed slurry is prepared by a planetary disperser, and then the slurry is evenly coated on the composite copper current collector to obtain a negative electrode sheet. The electrode sheet is cut into an electrode disc with a diameter of 12 mm and used as a positive electrode for standby. A metal lithium sheet with a diameter of 14 mm is used as the counter electrode and reference electrode, a ceramic diaphragm with a model of CF15D and a diameter of 16 mm is used as the diaphragm, and 10 μL 1 mol / L LiPF6 / EC+DMC+DEC (volume ratio 1:1:1) is used as the electrolyte. In an argon-protected glove box, a 2016-type button half-cell is assembled, and the capacity, EIS, rate and cycle performance are tested.
[0022] Application Example 3: The three-dimensional conductive nanosheet graphene modified composite copper foil prepared in Example 3 is used as the negative electrode current collector, commercial graphite is used as the active material, SP is used as the conductive agent, and PVDF is used as the binder. The graphite, SP and PVDF are weighed in a mass ratio of 94.0:3.7:2.3. NMP is used as the solvent, and a uniformly mixed slurry is prepared by a planetary disperser, and then the slurry is evenly coated on the composite copper current collector to obtain a negative electrode sheet. The electrode sheet is cut into an electrode disc with a diameter of 12 mm and used as a positive electrode for standby. A metal lithium sheet with a diameter of 14 mm is used as the counter electrode and reference electrode, a ceramic diaphragm with a model of CF15D and a diameter of 16 mm is used as the diaphragm, and 10 μL 1 mol / L LiPF6 / EC+DMC+DEC (volume ratio 1:1:1) is used as the electrolyte. In an argon-protected glove box, a 2016-type button half-cell is assembled, and the capacity, EIS, rate and cycle performance are tested.
[0023] The SEM image of the surface of the composite copper current collector modified with three-dimensional conductive nanosheet graphene prepared in Example 1 is as follows: Figure 1 As shown, it can be seen that the nano-sheet graphene is evenly loaded on the surface of the copper current collector. The addition of nano-graphene improves the conductivity of the electrode, reduces the polarization phenomenon of the battery, and greatly improves the battery's initial charge and discharge capacity, rate, cycle and other performance.
[0024] The 0.1 C first charge and discharge curves of the batteries prepared in Application Example 1, Application Example 2, Application Example 3 and Comparative Example are as follows: Figure 2 As shown, the first charge specific capacity of Application Example 1, Application Example 2 and Application Example 3 is as high as 371.65 mAh / g, and the discharge specific capacity is as high as 437.65 mAh / g.
[0025] The EIS performance of the batteries prepared in Application Example 1, Application Example 2, Application Example 3 and Comparative Example was tested. Figure 3 As shown. Figure 3 It can be seen that the charge transfer resistance and diffusion resistance of the batteries prepared in Application Examples 1 and 2 are both lower than those in Application Example 3, indicating that the current collector after acetone pretreatment has better conductivity. This is because the oxide layer and impurities on the surface of the copper foil are removed, which improves the bonding force between the nanosheet graphene and the copper foil, thereby improving the conductivity of the battery. The charge transfer resistance and diffusion resistance of the batteries prepared in Application Examples 1, 2 and 3 are all lower than those in the comparative example, indicating that the composite copper current collector prepared in this patent improves the conductivity of the pole piece.
[0026] The rate performance of the batteries prepared in Application Example 1, Application Example 2, Application Example 3 and Comparative Example was tested. Figure 4 As shown. Figure 4It can be seen that the rate performance of Application Example 1 and Application Example 2 is higher than that of Application Example 3, indicating that the use of acetone pretreatment helps to improve the growth of nano-sheet graphene on the surface of copper foil and improves the rate performance of the battery. The discharge capacity of the batteries prepared in Application Example 1, Application Example 2 and Application Example 3 is much higher than that in the comparative example, indicating that the composite copper current collector prepared in this patent improves the rate performance of the battery.
[0027] The cycle performance of the batteries prepared in Application Example 1, Application Example 2, Application Example 3 and Comparative Example was tested. Figure 5 As shown. Figure 5 It can be seen that the cycle performance of Application Example 1 and Application Example 2 is higher than that of Application Example 3. This may be because the use of acetone to pretreat the copper foil improves the bonding force between the nanosheet graphene and the copper foil, thereby improving the cycle performance of the battery. The cycle performance of the batteries prepared in Application Examples 1, 2, and 3 is much higher than that of the comparative example, indicating that the composite copper current collector prepared in this patent improves the cycle performance of the battery.
Claims
1. A method for preparing a low-resistance composite current collector, characterized in that: The following steps are involved: S1. Soak the smooth copper foil in acetone for 1 to 2 hours for pretreatment, and dry it under vacuum at 60 to 80°C for 24 to 48 hours; S2. Place the treated copper foil in a quartz tube and heat it to 1000-1200°C in an inert gas atmosphere. The flow rate of the inert gas is 80-100 sccm and the heating rate is 25-28°C / min. After the temperature reaches 1000-1200°C, introduce CH4 gas with a flow rate of 20-50 sccm and keep it at this temperature for 15-30 min respectively. S3. After the reaction is completed, the sample is naturally cooled to room temperature under an inert gas atmosphere to obtain a composite copper current collector modified with three-dimensional conductive nanosheet graphene.
2. The method for preparing a low-resistance composite current collector according to claim 1, characterized in that: The inert gas is Ar or N2.
3. The method for preparing a low-resistance composite current collector according to claim 2, characterized in that: S1. Pre-treat the smooth copper foil by soaking it in acetone for 1 h, and then dry it at 60°C under vacuum for 24 h. S2. Place the treated copper foil in a quartz tube, heat it to 1000°C in an inert gas atmosphere with an inert gas flow rate of 80 sccm and a heating rate of 25°C / min. After the temperature reaches 1000°C, introduce CH4 gas with a CH4 flow rate of 20 sccm, and keep it at this temperature for 15 min respectively. S3. After the reaction is completed, cool the sample naturally to room temperature in an inert gas atmosphere to obtain a three-dimensional conductive nanosheet graphene-modified composite copper current collector.
4. The method for preparing a low-resistance composite current collector according to claim 2, characterized in that: S1. Pre-treat the smooth copper foil by soaking it in acetone for 2 h, and then dry it at 80°C under vacuum for 48 h. S2. Place the treated copper foil in a quartz tube, heat it to 1200°C in an inert gas atmosphere with an inert gas flow rate of 100 sccm and a heating rate of 28°C / min. After the temperature reaches 1200°C, introduce CH4 gas with a CH4 flow rate of 50 sccm, and keep it at this temperature for 30 min. S3. After the reaction is completed, cool the sample naturally to room temperature in an inert gas atmosphere to obtain a three-dimensional conductive nanosheet graphene-modified composite copper current collector.
5. The method for preparing a low-resistance composite current collector according to claim 2, characterized in that: S1. Pre-treat the smooth copper foil by soaking it in acetone for 1.5 h, and then dry it at 70°C under vacuum for 36 h. S2. Place the treated copper foil in a quartz tube, heat it to 1100°C in an inert gas atmosphere with an inert gas flow rate of 90 sccm and a heating rate of 26°C / min. After the temperature reaches 1100°C, introduce CH4 gas with a CH4 flow rate of 35 sccm, and keep it at this temperature for 25 min. S3. After the reaction is completed, cool the sample naturally to room temperature in an inert gas atmosphere to obtain a three-dimensional conductive nanosheet graphene-modified composite copper current collector.
6. A composite copper current collector prepared according to the method for preparing a low-resistance composite current collector according to any one of claims 3 to 5.
7. Use of the composite copper current collector according to claim 6 in a chemical energy storage battery.
Citation Information
Patent Citations
Preparation method for copper foil current collector and application
CN103579631A
Copper current collector for lithium-ion battery anodes as well as preparation method and application of copper current collector
CN105186004A