Multistage buffer boron-doped silicon-carbon composite material and preparation method thereof
By using multi-stage buffered boron doped silicon-carbon composite materials in the negative electrode material of lithium-ion battery, nano-silicon is coated with 4-aminophenylboric acid and nitrogen-doped carbon to form a core-shell structure, the volume change and preparation process of silicon material are solved. Complex problems achieve efficient cycle stability and simple preparation process.
Patent Information
- Application Number
- CN202310529747.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-11
AI Technical Summary
The cyclic stability of existing lithium-ion battery negative electrode materials is poor and the preparation process is complex. In particular, the volume changes in silicon materials during charging and discharging, resulting in material powdering and current collector falling off, limiting its application potential.
Using multi-stage buffered boron doped silicon-carbon composite material, a core structure is formed on the nano-silicon surface through 4-aminophenylboric acid as a coating agent, combined with nitrogen-doped carbon and amorphous carbon to form a multi-stage buffer structure to improve silicon-carbon The conductivity and cyclic stability of the composite material are obtained by simplifying the process by ball milling and baking in one step.
It improves the first week of Coulomb efficiency and cycle stability of lithium-ion batteries, simplifies the preparation process, reduces costs, and is suitable for industrial production.
Smart Images

Figure CN118943311A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of negative electrode materials for lithium-ion batteries, and in particular relates to a multi-stage buffered boron-doped silicon-carbon composite material and a preparation method thereof. Background Art
[0002] Since Sony successfully launched the first commercial lithium-ion battery in 1991, it has successfully replaced nickel-metal hydride batteries and nickel-cadmium batteries with its advantages of high power density, high energy density, high voltage, and long cycle life, and has been used in 3C products such as laptops, mobile phones, cameras, and electric vehicles. However, the theoretical specific capacity of graphite negative electrode is 372mAhg -1 , while the current commercial graphite anode capacity exceeds 360mAhg -1 , which is close to the theoretical limit, limiting the further development of single carbon material negative electrode. In this context, silicon material has the potential to replace traditional graphite negative electrode and become the next generation negative electrode material due to its advantages such as high theoretical specific capacity, suitable lithium insertion and extraction potential, and low cost. However, silicon has low electrical conductivity and drastic volume changes during charging and discharging, which leads to material pulverization and even falling off from the current collector, ultimately resulting in reduced cycle stability.
[0003] In order to solve the above problems, silicon materials are usually compounded with carbon materials, and carbon materials are used to inhibit the volume expansion of silicon and improve the conductivity of the material. However, the surface of nano-silicon lacks a coating layer, and the effect of inhibiting the volume change of silicon during charging and discharging is poor. In addition, there is a lack of modification of silicon itself. Some methods also have the defects of complex process and difficulty in industrialization. Patent CN 113666354 A discloses a method for preparing a silicon-carbon composite material, including the following steps: mixing a silicon source and carbon black evenly to obtain a silicon source mixture, then mixing the silicon source mixture with porous carbon powder, ultrasonically dispersing, ball milling, heating, introducing a reducing agent, isothermal reduction reaction, and finally removing hybridization with a hydrochloric acid solution, drying, and obtaining a silicon-carbon composite material, but does not involve modification of silicon itself. Patent CN 111799460A discloses a method for preparing a boron-doped nano-metal / porous silicon-carbon composite negative electrode based on cut silicon waste, wherein the cut silicon waste is treated with metal-assisted etching to obtain a nano-metal / porous silicon composite material, the nano-metal / porous silicon composite material is mixed with a boron source and then subjected to high-temperature treatment to allow boron to form substitutional doping on silicon, and then compounded with a carbon material to obtain a boron-doped nano-metal / porous silicon-carbon composite negative electrode. Although the metal particles are physically combined with silicon on the surface of the silicon matrix and the chemical doping of silicon by boron at the atomic scale synergistically improves the intrinsic conductivity of silicon, the volume expansion of silicon is insufficiently constrained. Patent CN 116072839 A discloses a silicon-carbon negative electrode material and its preparation method and application, wherein the silicon-carbon negative electrode material includes a core and a coating layer coated on the surface of the core, the material forming the core includes silicon powder, the material forming the coating layer is carbon nitride and carbon nanotubes, and at least one end of a portion of the carbon nanotubes is embedded in the core, but the preparation process is complicated and difficult to expand production. Summary of the invention
[0004] The purpose of the present invention is to overcome the problems of poor battery cycle stability and complex negative electrode material preparation process in the prior art, and to provide a multi-stage buffered boron-doped silicon-carbon composite material and a preparation method thereof.
[0005] To achieve the above object, the technical solution of the present invention is:
[0006] First, a silicon-carbon composite material is provided, characterized in that the silicon-carbon composite material has a composite structure, including an inner core and an outer layer, wherein the inner core of the silicon-carbon composite material is graphite, and the outer layer is a coating layer composed of amorphous carbon and nano-silicon; the nano-silicon has a core-shell structure, including a nitrogen-doped carbon coating layer and a boron-doped nano-silicon inner core.
[0007] The nitrogen-doped carbon coating layer and the boron-doped nano-silicon are both produced by pyrolysis of organic small molecules, wherein the organic small molecule is 4-aminophenylboronic acid.
[0008] The thickness of the nitrogen-doped carbon coating layer is 1-5 nm.
[0009] The median particle size of the graphite is 5-20 μm, and the median particle size of the nano-silicon is 50-150 nm.
[0010] Taking the total mass of the negative electrode material as 100%, the mass percentage of the nano-silicon is 5-10%.
[0011] The carbon of the amorphous carbon layer is composed of pitch cracked carbon and Super P.
[0012] The method comprises the following steps:
[0013] (1) mixing a micron silicon dispersion with 4-aminophenylboric acid, and ball milling to obtain 4-aminophenylboric acid-coated nano silicon;
[0014] (2) mixing the nano-silicon dispersion obtained in step 1 with asphalt and Super P by ball milling, and then mixing the obtained slurry with graphite by ball milling to obtain a silicon-carbon composite material precursor;
[0015] (3) Sintering the precursor obtained in step 2 at 800-1000° C. for 2-4 h under an inert atmosphere to obtain a silicon-carbon composite material.
[0016] Preferably, the mass ratio of the micron silicon to 4-aminophenylboronic acid in step (1) is 1:0.1-1:0.5, and the mass ratio of the micron silicon to ethanol is 1:10.
[0017] Preferably, the ball milling conditions in step (1) are argon protection, a ball-to-material ratio of 50:1, a ball milling speed of 600 rpm, and a ball milling time of 6-8 h.
[0018] Preferably, the nano-silicon dispersion described in step (2) is mixed with asphalt and Super P by ball milling under argon protection, the mass ratio of nano-silicon to asphalt is 1:1, the mass ratio of nano-silicon to Super P is 1:0.2, the ball-to-material ratio is 10:1, the ball milling speed is 450rpm, and the ball milling time is 1h; the slurry is mixed with graphite by ball milling under argon protection, the mass ratio of nano-silicon to graphite is 1:10-1:5, the ball-to-material ratio is 5:1, the ball milling speed is 200rpm, and the ball milling time is 1h.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] (1) The present invention uses 4-aminophenylboric acid as an additive in the ball milling process, which can form a coating layer on the surface of nano-silicon in situ during the ball milling of micron silicon, thereby reducing oxidation during the ball milling process;
[0021] (2) The present invention uses 4-aminophenylboronic acid as the coating layer of nano-silicon, which can form substitutional boron doping on silicon during the subsequent calcination process, thereby improving the first-cycle coulomb efficiency, and the nitrogen-doped cracked carbon coating layer can form a multi-level buffer structure with graphite and amorphous carbon, thereby improving the cycle stability of the silicon-carbon composite material;
[0022] (3) The multi-stage buffered boron-doped silicon-carbon composite material of the present invention only requires one step of ball milling to obtain a precursor, and one calcination to obtain a finished material. The process is simple, the operation is simple, and the process cost is low, which is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the prior art descriptions. Obviously, the drawings described below are only embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on the provided drawings without creative work.
[0024] Figure 1 This is a scanning electron microscope image of the silicon-carbon composite material provided in Example 1 of the present invention.
[0025] Figure 2 This is a high-resolution transmission electron microscopy image of carbon-coated nano-silicon cracked by 4-aminophenylboronic acid in the silicon-carbon composite material provided in Example 1 of the present invention.
[0026] Figure 3 This is an X-ray photoelectron spectrum of carbon-coated nano-silicon cracked by 4-aminophenylboronic acid in the silicon-carbon composite material provided in Example 1 of the present invention.
[0027] Figure 4 This is a charge and discharge curve diagram of the first week of a lithium-ion battery assembled using the silicon-carbon composite material provided in Example 1 of the present invention.
[0028] Figure 5 This is a cycle curve diagram of a lithium-ion battery assembled using the silicon-carbon composite material provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0029] The specific implementation modes of the present invention are further described below in conjunction with examples. It should be noted that the specific implementation modes described herein are only for illustrating and explaining the present invention and are not limited to the present invention.
[0030] Example 1: Weigh 0.5g of micron silicon and 0.15g of 4-aminophenylboronic acid into a ball mill, add zirconium oxide beads and anhydrous ethanol, and perform ball milling under argon protection. Among them, the mass ratio of ethanol to micron silicon is 10:1, the mass ratio of zirconium oxide beads to micron silicon is 50:1, the ball milling speed is 600rpm, and the ball milling time is 6h. After adding 0.5g of asphalt and 0.1g of Super P to the slurry, place it in a ball mill again, add zirconium oxide beads, and perform ball milling under argon protection. Among them, the mass ratio of zirconium oxide beads to the solid matter in the slurry is 10:1, the ball milling speed is 450rpm, and the ball milling time is 1h. After adding 5g of graphite to the slurry, place it in a ball mill again, add zirconium oxide beads, and perform ball milling under argon protection. Among them, the mass ratio of zirconium oxide beads to the solid matter in the slurry is 5:1, the ball milling speed is 450rpm, and the ball milling time is 1h. After the ball milling, the slurry was centrifuged to obtain a silicon-carbon composite material precursor. The precursor was transferred to a tube furnace, calcined at 900°C for 3 hours under an argon atmosphere, naturally cooled to room temperature, and ground through a 400-mesh screen to obtain a multi-stage buffered boron-doped silicon-carbon composite material.
[0031] Embodiment 1 is further described: Figure 1 The scanning electron microscope image shows that the particle size of the multi-level buffered boron-doped silicon-carbon composite material is between 5-20 μm; Figure 2 The high-resolution transmission electron microscopy image shows that there is an amorphous carbon coating layer with a thickness of about 2-3 nm on the surface of the 4-aminophenylboronic acid cracked carbon-coated nano-silicon in the multi-stage buffered boron-doped silicon-carbon composite material; Figure 3 The X-ray photoelectron spectrum shows that Figure 3 The presence of B-Si bond peaks in (2) indicates that boron has formed substitutional doping on silicon. Figure 3 The presence of pyridine nitrogen peaks in (3) indicates that 4-aminophenylboronic acid cleaves the carbon coating layer on the surface of carbon-coated nano-silicon to form nitrogen doping; Figure 4 The first week charge and discharge curve of Example 1 shows that the first week discharge capacity of the material provided by Example 1 is 605.7 mAhg -1 The first week charging capacity is 544.3mAhg -1 , the first week Coulomb efficiency is 89.9%; Figure 5 The cycle curve of Example 1 shows that the 100-cycle capacity retention rate of the material provided in Example 1 is 89.7%.
[0032] Example 2: Weigh 0.5g of micron silicon and 0.05g of 4-aminophenylboronic acid into a ball mill, add zirconium oxide beads and anhydrous ethanol, and perform ball milling under argon protection. Among them, the mass ratio of ethanol to micron silicon is 10:1, the mass ratio of zirconium oxide beads to micron silicon is 50:1, the ball milling speed is 600rpm, and the ball milling time is 7h. After adding 0.5g of asphalt and 0.1g of Super P to the slurry, it is placed in a ball mill again, and zirconium oxide beads are added, and ball milling is performed under argon protection. Among them, the mass ratio of zirconium oxide beads to the solid matter in the slurry is 10:1, the ball milling speed is 450rpm, and the ball milling time is 1h. After adding 5g of graphite to the slurry, it is placed in a ball mill again, and zirconium oxide beads are added, and ball milling is performed under argon protection. Among them, the mass ratio of zirconium oxide beads to the solid matter in the slurry is 5:1, the ball milling speed is 450rpm, and the ball milling time is 1h. After the ball milling is completed, the slurry is centrifuged to obtain a silicon-carbon composite material precursor. The precursor is transferred into a tube furnace, calcined at 800°C for 4 hours under an argon atmosphere, naturally cooled to room temperature, and ground through a 400-mesh screen to obtain a multi-stage buffered boron-doped silicon-carbon composite material.
[0033] Example 3: Weigh 0.5g of micron silicon and 0.25g of 4-aminophenylboronic acid into a ball mill, add zirconium oxide beads and anhydrous ethanol, and perform ball milling under argon protection. Among them, the mass ratio of ethanol to micron silicon is 10:1, the mass ratio of zirconium oxide beads to micron silicon is 50:1, the ball milling speed is 600rpm, and the ball milling time is 6h. After adding 0.5g of asphalt and 0.1g of Super P to the slurry, it is placed in a ball mill again, and zirconium oxide beads are added, and ball milling is performed under argon protection. Among them, the mass ratio of zirconium oxide beads to the solid matter in the slurry is 10:1, the ball milling speed is 450rpm, and the ball milling time is 1h. After adding 5g of graphite to the slurry, it is placed in a ball mill again, zirconium oxide beads are added, and ball milling is performed under argon protection. Among them, the mass ratio of zirconium oxide beads to the solid matter in the slurry is 5:1, the ball milling speed is 450rpm, and the ball milling time is 1h. After the ball milling, the slurry was centrifuged to obtain a silicon-carbon composite material precursor. The precursor was transferred into a tube furnace, calcined at 1000°C for 3 hours under an argon atmosphere, naturally cooled to room temperature, and ground through a 400-mesh screen to obtain a multi-stage buffered boron-doped silicon-carbon composite material.
[0034] Example 4: Weigh 0.5g of micron silicon and 0.15g of 4-aminophenylboronic acid into a ball mill, add zirconium oxide beads and anhydrous ethanol, and perform ball milling under argon protection. Among them, the mass ratio of ethanol to micron silicon is 10:1, the mass ratio of zirconium oxide beads to micron silicon is 50:1, the ball milling speed is 600rpm, and the ball milling time is 6h. After adding 0.5g of asphalt and 0.1g of Super P to the slurry, it is placed in a ball mill again, and zirconium oxide beads are added, and ball milling is performed under argon protection. Among them, the mass ratio of zirconium oxide beads to the solid matter in the slurry is 10:1, the ball milling speed is 450rpm, and the ball milling time is 1h. After adding 5g of graphite to the slurry, it is placed in a ball mill again, zirconium oxide beads are added, and ball milling is performed under argon protection. Among them, the mass ratio of zirconium oxide beads to the solid matter in the slurry is 5:1, the ball milling speed is 450rpm, and the ball milling time is 1h. After the ball milling, the slurry was centrifuged to obtain a silicon-carbon composite material precursor. The precursor was transferred into a tube furnace, calcined at 1000°C for 2 hours under an argon atmosphere, naturally cooled to room temperature, and ground through a 400-mesh screen to obtain a multi-stage buffered boron-doped silicon-carbon composite material.
[0035] Example 5: Weigh 1g of micron silicon and 0.3g of 4-aminophenylboronic acid into a ball mill, add zirconium oxide beads and anhydrous ethanol, and perform ball milling under argon protection. Among them, the mass ratio of ethanol to micron silicon is 10:1, the mass ratio of zirconium oxide beads to micron silicon is 50:1, the ball milling speed is 600rpm, and the ball milling time is 6h. After adding 1g of asphalt and 0.2g of Super P to the slurry, it is placed in a ball mill again, and zirconium oxide beads are added, and ball milling is performed under argon protection. Among them, the mass ratio of zirconium oxide beads to the solid matter in the slurry is 10:1, the ball milling speed is 450rpm, and the ball milling time is 1h. After adding 5g of graphite to the slurry, it is placed in a ball mill again, and zirconium oxide beads are added, and ball milling is performed under argon protection. Among them, the mass ratio of zirconium oxide beads to the solid matter in the slurry is 5:1, the ball milling speed is 450rpm, and the ball milling time is 1h. After the ball milling is completed, the slurry is centrifuged to obtain a silicon-carbon composite material precursor. The precursor was transferred into a tube furnace and calcined at 900° C. for 4 h in an argon atmosphere. After naturally cooling to room temperature, the precursor was ground through a 400-mesh sieve to obtain a multi-stage buffered boron-doped silicon-carbon composite material.
[0036] Comparative Example 1: Weigh 0.5g of micron silicon and place it in a ball mill, add zirconium oxide beads and anhydrous ethanol, and perform ball milling under argon protection. Among them, the mass ratio of ethanol to micron silicon is 10:1, the mass ratio of zirconium oxide beads to micron silicon is 50:1, the ball milling speed is 600rpm, and the ball milling time is 6h. After adding 0.5g of asphalt and 0.1g of Super P to the slurry, place it in a ball mill again, add zirconium oxide beads, and perform ball milling under argon protection. Among them, the mass ratio of zirconium oxide beads to the solid matter in the slurry is 10:1, the ball milling speed is 450rpm, and the ball milling time is 1h. After adding 5g of graphite to the slurry, place it in a ball mill again, add zirconium oxide beads, and perform ball milling under argon protection. Among them, the mass ratio of zirconium oxide beads to the solid matter in the slurry is 5:1, the ball milling speed is 450rpm, and the ball milling time is 1h. After the ball milling is completed, the slurry is centrifuged to obtain a silicon-carbon composite material precursor. The precursor was transferred into a tube furnace and calcined at 900° C. for 3 h in an argon atmosphere. After naturally cooling to room temperature, the precursor was ground through a 400-mesh sieve to obtain a multi-stage buffered boron-doped silicon-carbon composite material.
[0037] Comparative Example 2: Weigh 0.5g of micron silicon and 0.25g of boric acid into a ball mill, add zirconium oxide beads and anhydrous ethanol, and perform ball milling under argon protection. Among them, the mass ratio of ethanol to micron silicon is 10:1, the mass ratio of zirconium oxide beads to micron silicon is 50:1, the ball milling speed is 600rpm, and the ball milling time is 6h. After adding 0.5g of asphalt and 0.1g of Super P to the slurry, it is placed in a ball mill again, and zirconium oxide beads are added, and ball milling is performed under argon protection. Among them, the mass ratio of zirconium oxide beads to the solid matter in the slurry is 10:1, the ball milling speed is 450rpm, and the ball milling time is 1h. After adding 5g of graphite to the slurry, it is placed in a ball mill again, zirconium oxide beads are added, and ball milling is performed under argon protection. Among them, the mass ratio of zirconium oxide beads to the solid matter in the slurry is 5:1, the ball milling speed is 450rpm, and the ball milling time is 1h. After the ball milling is completed, the slurry is centrifuged to obtain a silicon-carbon composite material precursor. The precursor was transferred into a tube furnace and calcined at 900° C. for 3 h in an argon atmosphere. After naturally cooling to room temperature, the precursor was ground through a 400-mesh sieve to obtain a multi-stage buffered boron-doped silicon-carbon composite material.
[0038] Comparative Example 3: Weigh 0.5g of micron silicon and 0.25g of citric acid into a ball mill, add zirconium oxide beads and anhydrous ethanol, and perform ball milling under argon protection. Among them, the mass ratio of ethanol to micron silicon is 10:1, the mass ratio of zirconium oxide beads to micron silicon is 50:1, the ball milling speed is 600rpm, and the ball milling time is 6h. After adding 0.5g of asphalt and 0.1g of Super P to the slurry, it is placed in a ball mill again, and zirconium oxide beads are added, and ball milling is performed under argon protection. Among them, the mass ratio of zirconium oxide beads to the solid matter in the slurry is 10:1, the ball milling speed is 450rpm, and the ball milling time is 1h. After adding 5g of graphite to the slurry, it is placed in a ball mill again, and zirconium oxide beads are added, and ball milling is performed under argon protection. Among them, the mass ratio of zirconium oxide beads to the solid matter in the slurry is 5:1, the ball milling speed is 450rpm, and the ball milling time is 1h. After the ball milling is completed, the slurry is centrifuged to obtain a silicon-carbon composite material precursor. The precursor was transferred into a tube furnace and calcined at 800° C. for 2 h in an argon atmosphere. After naturally cooling to room temperature, the precursor was ground through a 400-mesh sieve to obtain a multi-stage buffered boron-doped silicon-carbon composite material.
[0039] The silicon-carbon composite negative electrode materials prepared in Examples 1-6 and Comparative Examples 1-3 were made into negative electrode sheets and batteries in the following manner:
[0040] Graphite, silicon-carbon negative electrode material, conductive agent, and binder were prepared into a uniform slurry with a mass ratio of 80:10:10 and coated on copper foil. The conductive agent used was Super P, and the binder was prepared by stirring carboxymethyl cellulose (CMC), 50% styrene-butadiene rubber (SBR), and deionized water in a mass ratio of 1:1:48 for 24 hours. After vacuum drying, rolling, and punching, the negative electrode sheet was prepared. A metal lithium sheet was used as the negative electrode, and 1 mol / L LiPF6 (the solvent was a mixture of ethylene carbonate, diethyl carbonate, ethyl methyl carbonate, and fluoroethylene carbonate) was used as the electrolyte to assemble a button cell in a glove box.
[0041] The charge and discharge test of button cells was carried out on the Wuhan LAND battery test system, with a test voltage range of 0.01 to 1.5 V and a test current density of 0.5 C (1 C = 500 mA / g).
[0042] The test results are shown in Table 1.
[0043] Table 1 Button battery test results of Examples 1-5 and Comparative Examples 1-3
[0044]
[0045] It can be seen from the embodiments and test results that the multi-stage buffered boron-doped silicon-carbon composite material provided by the present invention has a higher first-week reversible capacity, a higher first-week coulomb efficiency and better cycle stability. From the comparison between Example 1 and Comparative Example 1, it can be seen that due to the lack of 4-aminophenylboric acid in the ball milling process, the degree of oxidation of nano-silicon is deepened during the ball milling process, and there is a lack of boron doping and surface carbon coating, the electrochemical properties such as the first-week reversible capacity, the first-week coulomb efficiency and the cycle stability of the silicon-carbon composite material provided in Comparative Example 1 are all reduced; from the comparison between Example 1 and Comparative Example 2, it can be seen that 4-aminophenylboric acid is replaced with boric acid, and the surface carbon coating is lacking, and the cycle stability of the silicon-carbon composite material provided in Comparative Example 2 is reduced; from the comparison between Example 1 and Comparative Example 3, it can be seen that 4-aminophenylboric acid is replaced with citric acid. Since citric acid cannot form an in-situ coating during the ball milling process, the first-week coulomb efficiency and cycle stability of the silicon-carbon composite material provided in Comparative Example 3 are both reduced.
[0046] The above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, and the present invention is not limited thereto. Any modification, equivalence, substitution and improvement of the present invention shall fall within the protection scope of the present invention.
Claims
1. A multi-stage buffered boron-doped silicon-carbon composite material, characterized in that: The silicon-carbon composite material has a composite structure, including an inner core and an outer layer, wherein the inner core of the silicon-carbon composite material is graphite, and the outer layer is a coating layer composed of amorphous carbon and nano-silicon; the nano-silicon has a core-shell structure, including a nitrogen-doped carbon coating layer and a boron-doped nano-silicon inner core.
2. The multi-stage buffered boron-doped silicon-carbon composite material according to claim 1, characterized in that: The nitrogen-doped carbon coating layer and the boron-doped nano-silicon are both produced by thermal decomposition of organic small molecules; wherein the organic small molecule is 4-aminophenylboronic acid.
3. The multi-stage buffered boron-doped silicon-carbon composite material according to claim 1, characterized in that: The thickness of the nitrogen-doped carbon coating layer is 1-5 nm.
4. The multi-stage buffered boron-doped silicon-carbon composite material according to claim 1, characterized in that: The median particle size of the graphite is 5-20 μm, and the median particle size of the nano-silicon is 50-150 nm.
5. The multi-stage buffered boron-doped silicon-carbon composite material according to claim 1, characterized in that: Taking the total mass of the negative electrode material as 100%, the mass percentage of the nano-silicon is 5-10%.
6. The multi-stage buffered boron-doped silicon-carbon composite material according to claim 1, characterized in that: The carbon of the amorphous carbon layer is composed of pitch cracked carbon and Super P.
7. A method for preparing the multi-stage buffered boron-doped silicon-carbon composite material according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: (1) mixing an ethanol dispersion of micron silicon with 4-aminophenylboric acid, and ball milling to obtain 4-aminophenylboric acid-coated nanosilicon; (2) mixing the nano-silicon dispersion obtained in step 1 with asphalt and Super P by ball milling, and then mixing the obtained slurry with graphite by ball milling to obtain a silicon-carbon composite material precursor; (3) Sintering the precursor obtained in step 2 at 800-1000° C. for 2-4 h under an inert atmosphere to obtain a silicon-carbon composite material.
8. The preparation method according to claim 7, characterized in that: The mass ratio of the micron silicon to 4-aminophenylboronic acid in step (1) is 1:0.1-1:0.5, and the mass ratio of the micron silicon to ethanol is 1:
10.
9. The preparation method according to claim 7, characterized in that: The ball milling conditions in step (1) are argon protection, a ball-to-material ratio of 50:1, a ball milling speed of 600 rpm, and a ball milling time of 6-8 h.
10. The preparation method according to claim 7, characterized in that: The nano-silicon dispersion in step (2) is mixed with asphalt and Super P by ball milling under argon protection, the mass ratio of nano-silicon to asphalt is 1:1, the mass ratio of nano-silicon to Super P is 1:0.2, the ball-to-material ratio is 10:1, the ball milling speed is 450rpm, and the ball milling time is 1h; the slurry is mixed with graphite by ball milling under argon protection, the mass ratio of nano-silicon to graphite is 1:10-1:5, the ball-to-material ratio is 5:1, the ball milling speed is 200rpm, and the ball milling time is 1h.
Citation Information
Patent Citations
Method for preparing boron-doped nano-metal / porous silicon-carbon composite negative electrode based on cut silicon wastes
CN111799460A
Preparation method of silicon-carbon composite material, silicon negative pole piece and battery
CN113666354A
Silicon-carbon negative electrode material and preparation method and application thereof
CN116072839A
Silicon composite negative electrode material for lithium ion battery, preparation method thereof, and lithium ion battery negative electrode comprising same
CN106784640A
Boron-doped silicon-based negative electrode material used for lithium ion battery
CN107195893A