Lithium molybdate coated silicon negative electrode material as well as preparation method and application thereof

By coating silicon material with lithium molybdate, the problem of poor magnification and circulation performance of silicon in sulfide solid lithium batteries is solved, and more efficient lithium ion transmission and more stable battery performance is achieved, which promotes the business of sulfide solid battery. .

CN118943319AInactive Publication Date: 2024-11-12GAO NENG SHI DAI (SHEN ZHEN) XIN NENG YUAN KE JI YOU XIAN GONG SI

Patent Information

Application Number
CN202410920757.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Silicon has poor rate performance and cycling performance in sulfide solid lithium batteries, mainly due to poor electron and ion transmission caused by volume expansion.

Method used

The silicon negative electrode material is coated with lithium molybdate, and a uniformly dispersed lithium molybdate shell is generated through the neutralization reaction between lithium molybdate and silicon material, which improves the interface contact between silicon and sulfide solid electrolyte, reduces internal resistance, and inhibits volume expansion. Improve cycle stability and rate performance.

Benefits of technology

The transmission rate of lithium ions is improved, the polarization of the silicon negative electrode is reduced, and the rate performance and cycle stability of sulfide solid-state batteries are significantly improved, making the application of silicon materials in sulfide solid-state batteries more reliable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943319A_ABST
    Figure CN118943319A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of batteries, and discloses a lithium molybdate coated silicon negative electrode material as well as a preparation method and application thereof. The lithium molybdate coated silicon negative electrode material has a core-shell structure, the core comprises silicon powder, and the shell comprises lithium molybdate. According to the lithium molybdate coated silicon negative electrode material provided by the invention, the interface problem of silicon and sulfide solid electrolyte can be improved, the conductivity is improved, the internal resistance is reduced, the rate capability is improved, and the volume expansion of silicon can be inhibited to a certain extent by a lithium molybdate shell; the damage of the volume change of the active material in the lithiation lithium removal process to the contact property of the active material and the sulfide solid electrolyte is reduced, and the cycling stability and the rate capability of the material are improved, so that the silicon material can be better applied to the sulfide solid-state battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of batteries, and in particular relates to a lithium molybdate-coated silicon negative electrode material and a preparation method and application thereof. Background Art

[0002] In recent years, with the development of new energy vehicles, electronic communication equipment and large-scale energy storage grids, portable electronic products and electric vehicles are in urgent need of lithium-ion batteries with high capacity, long life, high stability and fast charge and discharge performance. In order to further expand the market, such as stationary energy storage of renewable energy and large vehicles other than automobiles, batteries must have higher energy density and safety performance than the current ones. Given that the current lithium-ion batteries using liquid electrolytes cannot meet the greatly increased demand for energy density and safety, it is of great significance to develop a new generation of batteries. Sulfide all-solid-state lithium batteries are based on non-flammable sulfide solid electrolytes and are expected to improve energy density and alleviate safety issues through a unique bipolar stacking method. However, batteries based on traditional LiCoO2 positive electrodes and graphite negative electrodes have reached the theoretical limit of energy density. The use of high-capacity electrode materials is an urgent need for the development of high-energy sulfide all-solid-state lithium batteries.

[0003] Silicon is the most promising negative electrode material for improving the weight energy density of the next generation of lithium-ion batteries. Silicon has been explored as a negative electrode material or negative electrode component for sulfide solid-state batteries, but its rate performance and cycle performance in sulfide solid-state batteries are poor. Its poor rate performance is due to the interface problem between silicon and sulfide solid electrolyte: during the cycle, the sulfide solid electrolyte will be reduced on the low-potential silicon surface to generate Li2S, LiP, etc. with low ionic conductivity, which will be coated on the Si surface, reducing the ionic conductivity of the silicon negative electrode, increasing the internal resistance of the battery, and reducing the rate performance; and the poor cycle performance is due to the volume expansion of about 300% during the lithium insertion and delithiation process of silicon. The excessive volume expansion causes the gap between silicon and sulfide solid electrolyte to continue to expand, and the contact between the two continues to deteriorate, which makes the electron and ion transmission between the two continue to deteriorate, resulting in rapid decay of cycle performance. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a lithium molybdate-coated silicon negative electrode material and a preparation method and application thereof, wherein the lithium molybdate-coated silicon negative electrode material can achieve excellent contact with a sulfide solid electrolyte, improve the interface problem between silicon and the sulfide solid electrolyte, increase the ion transmission rate of the material, realize rapid transmission of lithium ions, reduce the polarization of the silicon negative electrode, and improve the rate performance and cycle stability of the sulfide solid-state battery.

[0005] In a first aspect, the present invention provides a lithium molybdate-coated silicon negative electrode material, wherein the lithium molybdate-coated silicon negative electrode material has a core-shell structure, wherein the core comprises silicon powder and the shell comprises lithium molybdate.

[0006] Specifically, lithium molybdate is a material with excellent ionic conductivity. The present invention uses it as a coating material to coat the surface of a silicon material, thereby improving the interface problem between silicon and a sulfide solid electrolyte, enhancing the electrical conductivity, reducing the internal resistance, and improving the rate performance. In addition, the lithium molybdate shell can also inhibit the volume expansion of silicon to a certain extent, reduce the damage to the contact between the active material and the sulfide solid electrolyte caused by the volume change during the lithiation and delithiation process of the active material, improve the cycle stability and rate performance of the material, and enable the silicon material to be better applied to sulfide solid-state batteries.

[0007] In some embodiments of the present invention, the mass of the silicon powder accounts for 80-95% of the mass of the lithium molybdate-coated silicon negative electrode material, for example, it can be any point value among 80%, 82%, 84%, 86%, 88%, 90%, 92%, 95%, or a range value between two arbitrary point values.

[0008] In some embodiments of the present invention, the D50 particle size of the silicon powder is less than 100 μm, preferably 30 nm to 50 μm, for example, it can be any point value among 30 nm, 50 nm, 100 nm, 1 μm, 50 μm, or a range value between two arbitrary point values. The present invention can achieve smaller porosity control by selecting a suitable particle size.

[0009] In some embodiments of the present invention, the thickness of the shell is 5 to 100 nm, for example, it can be any point value among 5 nm, 15 nm, 25 nm, 35 nm, 45 nm, 55 nm, 65 nm, 75 nm, 85 nm, 100 nm, or a range value between two arbitrary point values.

[0010] The second aspect of the present invention provides a method for preparing the lithium molybdate-coated silicon negative electrode material according to the first aspect of the present invention, comprising the following steps:

[0011] S1, mixing silicon powder and solvent, and ultrasonically stirring to obtain a dispersion;

[0012] S2, mixing lithium hydroxide, molybdic acid and the dispersion, and ultrasonically stirring to obtain a mixed solution;

[0013] S3, drying and calcining the mixed solution to obtain the lithium molybdate-coated silicon negative electrode material.

[0014] Specifically, the present invention utilizes molybdic acid and lithium hydroxide to undergo a neutralization reaction in a dispersion of silicon material, so that the generated lithium molybdate is evenly dispersed on the surface of the silicon material, and then the solvent is removed, and the lithium molybdate-coated silicon negative electrode material is obtained by high-temperature calcination. The evenly coated lithium molybdate can avoid the contact between silicon and the sulfide solid electrolyte, and its higher lithium conductivity can improve the lithium conductivity of the silicon material, reduce the interface resistance, and improve the interface problems between the silicon material and the sulfide solid electrolyte, reduce side reactions, and thus improve the rate performance of the silicon negative electrode in the sulfide solid battery; secondly, the hard shell formed by lithium molybdate can alleviate the volume expansion and contraction during the silicon lithiation and delithiation process, inhibit the contact failure between silicon and the sulfide solid electrolyte, and effectively improve the cycle stability of the silicon negative electrode material in the sulfide solid battery. The present invention uses lithium molybdate to evenly coat the surface of the silicon material, improves many shortcomings of the silicon negative electrode in the sulfide solid battery, and is of great significance to the commercialization of sulfide solid batteries.

[0015] In some embodiments of the present invention, the process of step S2 includes: adding lithium hydroxide to the dispersion, ultrasonically stirring, and then adding molybdic acid, ultrasonically stirring, to obtain a mixed solution.

[0016] In some embodiments of the present invention, the process of step S2 includes: adding molybdic acid to the dispersion, ultrasonically stirring, and then adding lithium hydroxide, ultrasonically stirring to obtain a mixed solution.

[0017] In some embodiments of the present invention, the rotation speed of the ultrasonic stirring is 500-1000 rpm, preferably 700-800 rpm; the stirring time is 0.1-1 h, preferably 0.5-1 h.

[0018] In some embodiments of the present invention, before the drying, a step of removing solvent from the mixed solution is also included, and the method of removing solvent includes one or more of rotary evaporation, freeze drying, centrifugal washing, preferably rotary evaporation.

[0019] In some embodiments of the present invention, the drying process comprises: drying for 12 to 48 hours, preferably 12 to 24 hours, at a temperature of 60 to 100° C., preferably 80 to 100° C., and a vacuum pressure of -0.04 to -0.1 MPa, preferably -0.1 MPa.

[0020] In some embodiments of the present invention, the calcination process comprises: heating to 300-800° C. at a heating rate of 3-8° C. / min under an inert gas atmosphere, and keeping the temperature for 0.5-10 h.

[0021] In some embodiments of the present invention, the calcination process includes: in an inert gas atmosphere, heating to 300°C at a heating rate of 3 to 8°C / min, keeping warm for 0.5 to 1 hour, then heating to 400 to 800°C at a heating rate of 3 to 8°C / min, and keeping warm for 2 to 4 hours.

[0022] In some embodiments of the present invention, the inert gas includes one or more of argon, helium, and nitrogen.

[0023] In some embodiments of the invention, the solvent comprises water.

[0024] In some embodiments of the present invention, the molybdic acid is molybdic acid monohydrate.

[0025] In some embodiments of the present invention, the mass ratio of lithium hydroxide to silicon powder is (1-10):100, for example, it can be any point value among 1:100, 2:100, 3:100, 4:100, 5:100, 6:100, 7:100, 8:100, 9:100, 10:100, or a range value between two arbitrary point values.

[0026] In some embodiments of the present invention, the molar ratio of lithium hydroxide to molybdic acid is 1:(1-1.1), for example, it can be any point value among 1:1, 1:1.01, 1:1.02, 1:1.03, 1:1.04, 1:1.05, 1:1.06, 1:1.07, 1:1.08, 1:1.09, 1:1.1, or a range value between two arbitrary point values.

[0027] According to a third aspect of the present invention, a solid-state battery is provided, comprising a positive electrode, a negative electrode and a solid electrolyte, wherein the material of the negative electrode comprises the lithium molybdate-coated silicon negative electrode material as described in the first aspect of the present invention.

[0028] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0029] The lithium molybdate-coated silicon negative electrode material provided by the present invention has lithium molybdate uniformly distributed on its surface, which can achieve excellent contact with the sulfide solid electrolyte, improve the interface problem between silicon and the sulfide solid electrolyte, improve the ion transmission rate of the material, achieve rapid transmission of lithium ions, reduce the polarization of the silicon negative electrode, and improve the rate performance of the sulfide solid battery; the lithium molybdate material shell can reduce the influence of the volume expansion of silicon on the electrode structure, inhibit the increase of the porosity in the negative electrode, reduce the contact failure between the negative electrode material and the sulfide solid electrolyte, improve the problem of accelerated capacity decay of the material in the long-term cycle process, so that the silicon material can be better applied to the sulfide solid battery, and the performance of the sulfide solid battery is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The SEM image and the energy spectrum distribution diagram of silicon, oxygen and molybdenum elements of Example 1;

[0031] Figure 2 This is the energy spectrum distribution diagram of silicon and oxygen elements in Comparative Example 4;

[0032] Figure 3 The first cycle charge and discharge curve of the half-cell formed in Example 1;

[0033] Figure 4 This is a graph of the discharge capacity of the half-cell composed of Example 1 at different rates. DETAILED DESCRIPTION

[0034] The present invention is further described in detail below by specific examples. The raw materials, reagents or devices used in the examples can be obtained from conventional commercial sources or by prior art methods unless otherwise specified. Unless otherwise specified, the experiments or test methods are conventional methods in the art.

[0035] Example 1: Lithium molybdate coated silicon negative electrode material

[0036] A lithium molybdate-coated silicon negative electrode material is prepared by a preparation method comprising the following steps:

[0037] S1. Take 1 g of silicon powder with a D50 particle size of 100 nm, add it to 100 mL of deionized water, and stir it ultrasonically for 30 minutes to obtain a dispersion;

[0038] S2, adding 0.05 g of lithium hydroxide to the above dispersion, ultrasonically stirring for 30 min, and then adding 0.35 g of molybdic acid monohydrate, ultrasonically stirring for 30 min to obtain a mixed solution;

[0039] S3, the mixed solution was rotary evaporated to remove deionized water, and then dried in a vacuum oven at 80° C. and a vacuum pressure of -0.1 MPa for 24 h to obtain a powder;

[0040] S4. The above powder is calcined at high temperature to obtain a lithium molybdate-coated silicon negative electrode material (recorded as silicon@lithium molybdate). The specific high-temperature calcination procedure is: in a nitrogen atmosphere, the temperature is increased to 300°C at a heating rate of 5°C / min, and kept warm for 1 hour, and then the temperature is increased to 600°C at a heating rate of 5°C / min and kept warm for 3 hours.

[0041] The lithium molybdate-coated silicon negative electrode material prepared in Example 1 was tested using a scanning electron microscope (SEM) and an X-ray energy dispersive spectrometer (EDS). The SEM images are shown in FIG. Figure 1 As shown in (a), the resolution is 100nm; the energy spectrum distribution diagrams of silicon, oxygen and molybdenum are as follows: Figure 1As shown in (b), (c) and (d).

[0042] from Figure 1 It can be seen that the silicon@lithium molybdate prepared in Example 1 is composed of a core silicon and an outer shell lithium molybdate. The small lithium molybdate particles are evenly distributed on the surface of the silicon, which firmly coats the silicon, can effectively reduce the contact between the silicon and the sulfide solid electrolyte, and improve the lithium conductivity of the material.

[0043] Example 2: Lithium molybdate coated silicon negative electrode material

[0044] A lithium molybdate-coated silicon negative electrode material is prepared by a preparation method comprising the following steps:

[0045] S1. Take 1 g of silicon powder with a D50 particle size of 100 nm, add it to 100 mL of deionized water, and stir it ultrasonically for 30 minutes to obtain a dispersion;

[0046] S2, adding 0.05 g of lithium hydroxide to the above dispersion, stirring ultrasonically for 30 min, and then adding 0.5 g of molybdic acid monohydrate, stirring ultrasonically for 30 min to obtain a mixed solution;

[0047] S3, the mixed solution was rotary evaporated to remove deionized water, and then dried in a vacuum oven at 80° C. and a vacuum pressure of -0.1 MPa for 24 h to obtain a powder;

[0048] S4. The above powder is calcined at high temperature to obtain a lithium molybdate-coated silicon negative electrode material. The specific high-temperature calcination procedure is: in a nitrogen atmosphere, the temperature is increased to 300°C at a heating rate of 5°C / min, and kept warm for 1 hour, and then the temperature is increased to 600°C at a heating rate of 5°C / min and kept warm for 3 hours.

[0049] Example 3: Lithium molybdate coated silicon negative electrode material

[0050] A lithium molybdate-coated silicon negative electrode material is prepared by a preparation method comprising the following steps:

[0051] S1. Take 1 g of silicon powder with a D50 particle size of 1 μm, add it to 100 mL of deionized water, and stir it ultrasonically for 30 minutes to obtain a dispersion;

[0052] S2, adding 0.05 g of lithium hydroxide to the above dispersion, ultrasonically stirring for 30 min, and then adding 0.35 g of molybdic acid monohydrate, ultrasonically stirring for 30 min to obtain a mixed solution;

[0053] S3, the mixed solution was rotary evaporated to remove deionized water, and then dried in a vacuum oven at 80° C. and a vacuum pressure of -0.1 MPa for 24 h to obtain a powder;

[0054] S4. The above powder is calcined at high temperature to obtain a lithium molybdate-coated silicon negative electrode material. The specific high-temperature calcination procedure is: in a nitrogen atmosphere, the temperature is increased to 300°C at a heating rate of 5°C / min, and kept warm for 1 hour, and then the temperature is increased to 600°C at a heating rate of 5°C / min and kept warm for 3 hours.

[0055] Comparative Example 1

[0056] The only difference from Example 1 is that the amount of lithium hydroxide in Comparative Example 1 is adjusted to 0.5 g, and the other conditions are the same as those in Example 1.

[0057] Comparative Example 2

[0058] The only difference from Example 1 is that in Comparative Example 2, molybdic acid monohydrate is replaced by hydrochloric acid, and the other conditions are the same as those in Example 1.

[0059] Comparative Example 3

[0060] The only difference from Example 1 is that in Comparative Example 3, the D50 particle size of the silicon powder is adjusted to 100 μm, and the other conditions are the same as those in Example 1.

[0061] Comparative Example 4

[0062] The only difference from Example 1 is that lithium hydroxide is replaced by lithium chloride in Comparative Example 4, and the other conditions are the same as those in Example 1.

[0063] The sample prepared in Comparative Example 4 was tested by an X-ray energy dispersive spectrometer (EDS), and the energy spectrum distribution diagrams of silicon and oxygen elements were as follows: Figure 2 As shown in (a) and (b).

[0064] from Figure 2 There is no molybdenum element in the silicon, and there is an obvious phenomenon of lithium molybdate not being coated. This is attributed to the fact that lithium chloride and molybdic acid monohydrate are difficult to react to form lithium molybdate, and cannot be evenly attached to the silicon surface to form a lithium molybdate coating layer.

[0065] Comparative Example 5

[0066] A negative electrode material is prepared by the following steps:

[0067] 1 g of silicon powder with a D50 particle size of 100 nm, 0.05 g of lithium hydroxide and 0.35 g of monohydrated molybdic acid were mixed, then ball-milled, and finally the resulting product was calcined at high temperature to obtain the negative electrode material. The specific high-temperature calcination procedure was: in a nitrogen atmosphere, the temperature was increased to 300°C at a heating rate of 5°C / min, kept warm for 1 hour, and then the temperature was increased to 600°C at a heating rate of 5°C / min and kept warm for 3 hours.

[0068] Product electrochemical performance test

[0069] Test method: The samples prepared in Examples 1-3 and Comparative Examples 1-5 were used as active materials, and the active materials were mixed with LiP6S5Cl and polytetrafluoroethylene (PTFE) in a mass ratio of 60:40:1 to form a composite negative electrode, and a negative electrode sheet was obtained by a roller pressing and slicing process;

[0070] The negative electrode sheet was placed in a polyetheretherketone tube with a diameter of 10 mm, and then 100 mg of LiP6S5Cl was weighed and added to the tube. It was pressed into shape at a pressure of 12 MPa and kept in tight contact with the negative electrode sheet. Finally, an indium sheet and a lithium sheet were added to the other side of the solid electrolyte and pressed into shape at a pressure of 360 MPa to prepare a half-cell with a three-layer structure (composite negative electrode / solid electrolyte / Li-In alloy).

[0071] Test conditions: Charge and discharge tests were performed at 60°C with currents of 0.1C, 0.3C, 0.5C, 0.8C and 1C and a cut-off voltage of -0.61-0.2V. The battery was tested under a pressure of 15MPa.

[0072] Test 1: Electrochemical impedance spectroscopy

[0073] The internal resistance of the half-cell was tested by electrochemical impedance spectroscopy (EIS), thereby determining the contact between the obtained negative electrode material and the sulfide solid electrolyte and the lithium conductivity. The internal resistance of the half-cell composed of the negative electrode materials obtained in Examples 1-3 and Comparative Examples 1-5 is shown in Table 1.

[0074] Table 1 Internal resistance of half-cells composed of Examples 1-3 and Comparative Examples 1-5

[0075]

[0076] By comparing the internal resistance of the half-cells composed of Examples 1-3 and Comparative Examples 1-5 in Table 1, it can be found that Example 1 has the best contact with the sulfide solid electrolyte, and the combination of the two achieves better and lowest internal resistance, which is conducive to the transmission of lithium ions in the negative electrode, thereby achieving higher rate performance; the internal resistance of the embodiments of the present invention is significantly lower than that of the comparative example. It can be seen that the embodiments of the present invention well achieve the coating of silicon materials by lithium molybdate, effectively inhibit the contact between silicon and the sulfide solid electrolyte, and at the same time, lithium molybdate can quickly transfer lithium ions as an intermediate layer.

[0077] Test 2: First Coulombic efficiency test

[0078] The half-cell prepared by the above method was tested for the first coulombic efficiency (first efficiency), and the test results are shown in Table 2 and Figure 3 shown.

[0079] Table 2 First coulombic efficiency of half-cells composed of Examples 1-3 and Comparative Examples 1-5

[0080]

[0081] By comparing the first effects of the half-cells composed of Examples 1-3 and Comparative Examples 1-5 in Table 2, it can be seen that the first effect of Example 1 is the highest, indicating that the lithium molybdate coating on its surface is the most uniform, and the uniformly coated lithium molybdate effectively reduces the contact between silicon and the sulfide solid electrolyte, so the side reaction of silicon and the sulfide solid electrolyte is correspondingly reduced, and the first effect is improved; the first effects of the embodiments of the present invention are all higher than the first effects of the comparative examples.

[0082] Test 3: Rate performance test

[0083] The half-cell composed of Example 1 was tested for rate performance, and the results are as follows: Figure 4 shown.

[0084] from Figure 4 It can be seen that Example 1 exhibits excellent rate performance, and can even maintain a specific capacity of 2880 mAh / g at a rate of 1 C. This fully proves that the lithium molybdate-coated silicon negative electrode material prepared by the present invention has excellent performance and commercial potential.

[0085] The preferred embodiments of the present invention are specifically described above, but the invention is not limited to the embodiments. Those skilled in the art may make various equivalent modifications or substitutions without violating the spirit of the invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.

Claims

1. A lithium molybdate-coated silicon negative electrode material, characterized in that: The lithium molybdate-coated silicon negative electrode material has a core-shell structure, wherein the core comprises silicon powder and the shell comprises lithium molybdate.

2. The lithium molybdate-coated silicon negative electrode material according to claim 1, characterized in that: The mass of the silicon powder accounts for 80-95% of the mass of the lithium molybdate-coated silicon negative electrode material.

3. The lithium molybdate-coated silicon negative electrode material according to claim 1, characterized in that: The D50 particle size of the silicon powder is less than 100 μm.

4. The lithium molybdate-coated silicon negative electrode material according to claim 1, characterized in that: The thickness of the shell is 5-100 nm.

5. The method for preparing the lithium molybdate-coated silicon negative electrode material according to any one of claims 1 to 4, characterized in that: The following steps are involved: The silicon powder and the solvent are mixed and ultrasonically stirred to obtain a dispersion; Mixing lithium hydroxide, molybdic acid and the dispersion, and stirring with ultrasound to obtain a mixed solution; The mixed solution is dried and calcined to obtain the lithium molybdate-coated silicon negative electrode material.

6. The preparation method according to claim 5, characterized in that: The mass ratio of the lithium hydroxide to the silicon powder is (1-10):

100.

7. The preparation method according to claim 5, characterized in that: The molar ratio of the lithium hydroxide to molybdic acid is 1:(1-1.1).

8. The preparation method according to claim 5, characterized in that: The drying process includes: drying for 12 to 48 hours at a temperature of 60 to 100° C. and a vacuum pressure of -0.04 to -0.1 MPa.

9. The preparation method according to claim 5, characterized in that: The calcination process comprises: in an inert gas atmosphere, heating to 300-800° C. at a heating rate of 3-8° C. / min, and keeping the temperature for 0.5-10 hours.

10. A solid-state battery, characterized in that: The solid-state battery comprises a positive electrode, a negative electrode and a solid electrolyte, and the material of the negative electrode comprises the lithium molybdate-coated silicon negative electrode material according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Lithium molybdate coated lithium-rich manganese-based positive electrode material as well as preparation method and application thereof

    CN113078316A

  • Silicon negative electrode material and preparation method and application thereof

    CN115548325A

  • Ternary positive electrode material with surface modified with lithium molybdate, preparation method of ternary positive electrode material and lithium battery

    CN117638022A

  • Surface-modified lithium-rich manganese-based positive electrode material with multi-layer core-shell structure and preparation method of surface-modified lithium-rich manganese-based positive electrode material

    CN118016841A

Cited By

  • Silicon-based solid-state battery and preparation method thereof

    CN119764579A

  • Silicon-based solid-state battery and preparation method thereof

    CN119764579B