Graphene-coated V3S4-coated NC material and preparation method and application thereof

By coating V3S4@NC material with graphene, the conductivity and synergistic effect of graphene is used to solve the kinetics and stability of V3S4 materials in sodium ion storage, achieving more efficient electrochemical performance and simplified preparation method .

CN118943325APending Publication Date: 2024-11-12GUANGZHOU MARITIME INST

Patent Information

Application Number
CN202410991224.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing V3S4 materials have slow kinetics and large volume changes in sodium ion storage, resulting in poor high-speed performance and poor cycle stability. The existing composite materials have poor performance and complex preparation methods.

Method used

Graphene-coated V3S4@NC material is used to prepare graphene-coated V3S4@NC nanofiber composite material by electrospinning. It uses graphene conductivity and van der Waals force or π-π stacking to combine it with nitrogen-doped carbon fibers. Reduce the distance and volume changes of sodium ions and improve electrochemical performance.

Benefits of technology

It improves the electrochemical performance of V3S4 composite materials, enhances conductivity and structural stability, simplifies the preparation process, and achieves more efficient sodium ion storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943325A_ABST
    Figure CN118943325A_ABST
Patent Text Reader

Abstract

The invention relates to a graphene-coated V3S4-coated NC material and a preparation method and application thereof, the material is composed of V3S4-coated NC and graphene coating the surface of the V3S4-coated NC, and the V3S4-coated NC is a core-shell structure nanofiber composite material with V3S4 as a core and NC as a shell; the method comprises the following steps: 1, adding powdered sulfur, vanadyl acetylacetonate (VOC (acac) 2), polyacrylonitrile (PAN) and graphene oxide into N-N dimethylformamide (DMF), stirring for 12 hours, and carrying out ultrasonic oscillation to obtain a mixed solution; 2, filling an injector with the mixed solution obtained in the step 1, carrying out electrostatic spinning at the voltage of 18 kV and the flow rate of 0.4 mL / h, and collecting a product to obtain a precursor; 3, placing the collected precursor in a protective atmosphere, and annealing at 800 DEG C for 3 hours to obtain a graphene-coated V3S4-coated NC material; according to the graphene-coated V3S4-coated NC composite material disclosed by the invention, graphene is coated on the basis of the V3S4-coated NC composite material, and the transportation distance of sodium ions is reduced through the synergistic effect between V3S4-coated NC and graphene, so that the electrochemical performance of the graphene-coated V3S4-coated NC material disclosed by the invention is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of battery electrode composite materials, and in particular to a graphene-coated V3S4@NC material and a preparation method and application thereof. Background Art

[0002] To date, many new anode materials such as Sb2S3, ZnS, Co2GeO4, P, CuCo2S4 and V3S4 have attracted great interest in sodium ion storage. Among these negative electrode materials, monoclinic structured V3S4 is considered to be the most advanced sodium ion storage electrode due to its large interlayer space and high theoretical capacity. However, pure V3S4 material has slow kinetics and large volume change, resulting in poor high-speed performance and poor cycle stability. In this context, many strategies have been adopted to address these shortcomings, including constructing special nanostructures and making carbon composites.

[0003] The paper “V3S4 nanoparticles anchored on three-dimensional porous graphenegel for superior lithium storage, Electrochim. Acta 261 (2018) 35–41” discloses V3S4 nanocrystals anchored on conductive graphene sheets. The results show that graphene provides a continuous electron network for electrons and suppresses volume changes during discharge / charge processes.

[0004] The paper "Insights into the storage mechanism of 3D nanoflower-like V3S4anode in sodium-ion batteries, Chem. Eng. J. 427 (2022), 130936" discloses the preparation of three-dimensional nanoflower-like V3S4 material by a solvothermal method. The obtained anode has good sodium storage performance and a discharge capacity of up to 299 mAh / g under 5A / g conditions.

[0005] Although the above papers all use V3S4 to produce corresponding battery electrode composite materials, the performance of the above composite materials is still not very ideal, and the preparation method is relatively complicated and the synthesis environment is relatively harsh. Summary of the invention

[0006] In order to solve the problems existing in the above-mentioned prior art, the purpose of the present disclosure is to provide a graphene-coated V3S4@NC material and a preparation method and application thereof, so as to improve the electrical properties of the V3S4 composite material and provide a relatively simple preparation method.

[0007] The graphene-coated V3S4@NC material disclosed in the present invention is composed of V3S4@NC and graphene coated on the surface of V3S4@NC. The V3S4@NC is a core-shell structure nanofiber composite material with V3S4 as a core and NC as a shell.

[0008] Preferably, the crystal structure of V3S4 is a monoclinic crystal structure.

[0009] The present disclosure also provides a method for preparing the graphene-coated V3S4@NC material, comprising the following steps:

[0010] Step 1: sulfur powder, vanadium acetylacetonate (VO(acac)2), polyacrylonitrile (PAN) and graphene oxide are added to N-N-dimethylformamide (DMF), stirred for 12 hours, and subjected to ultrasonic oscillation to obtain a mixed solution;

[0011] Step 2: Fill the mixed solution obtained in step 1 into a syringe, perform electrospinning at a flow rate of 0.4 mL / h at a voltage of 18 kV, collect the product, and obtain a precursor;

[0012] Step 3: Place the collected precursor in a protective atmosphere and anneal at 800°C for 3h to obtain graphene-coated V3S4@NC material.

[0013] Preferably, the average particle size of the sulfur powder is 400-800 mesh, the average particle size of the vanadium acetylacetonate powder is 600-1000 mesh, the purity of the sulfur powder and the vanadium acetylacetonate powder are both analytically pure, the average molecular weight of the polyacrylonitrile powder is 50,000-200,000, and the number of graphene oxide layers is 15-20.

[0014] Preferably, the protective atmosphere is an inert atmosphere.

[0015] Preferably, the inert atmosphere is a mixed gas of argon and hydrogen, and the volume ratio of the argon to the hydrogen is 95:5.

[0016] The present disclosure also provides a sodium ion battery anode, comprising the above-mentioned graphene-coated V3S4@NC material, conductive carbon black and polyvinylidene fluoride (PVDF), wherein the mass ratio between the graphene-coated V3S4@NC material, conductive carbon black and polyvinylidene fluoride (PVDF) is 80:10:10.

[0017] The present invention also provides an application of the graphene-coated V3S4@NC material, which is used as an anode of a sodium ion battery.

[0018] The graphene-coated V3S4@NC material disclosed in the present invention has the following advantages:

[0019] Graphene is coated on the basis of V3S4@NC composite material. The synergistic effect between V3S4@NC and graphene reduces the transport distance of sodium ions and improves the conductivity of the material. Since V3S4@NC is a core-shell structure nanofiber composite material with V3S4 as the core and NC as the shell, it has a large specific surface area, which is conducive to the dispersion and coating of V3S4@NC on the graphene material;

[0020] At the same time, graphene may bind to nitrogen-doped carbon fibers through strong capillary forces via van der Waals forces or π-π stacking interactions, which helps anchor graphene flakes, alleviates the agglomeration effect of graphene, and also helps the dispersion and coating of graphene on V3S4@NC materials;

[0021] Since graphene is well dispersed on the V3S4@NC material and well coated on the V3S4@NC material, based on the conductive properties of graphene and the electrochemical properties of the V3S4@NC material itself, the two work together to improve the electrochemical properties of the graphene-coated V3S4@NC material described in the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 are the SEM and TEM images of V3S4@NC anode materials;

[0023] a~c are SEM images of V3S4@NC anode materials, d~f are TEM images of V3S4@NC composites;

[0024] Figure 2 These are the XRD pattern, Raman spectrum and XPS spectrum of V3S4@NC anode material;

[0025] a is the XRD pattern of V3S4@NC anode material; b is the Raman spectrum of V3S4@NC anode material; c~f are the XPS spectra of V3S4@NC anode material;

[0026] Figure 3 are the cyclic voltammetry (CV) and electrochemical impedance spectroscopy (EIS) measurement results of V3S4@NC anode material, and the charge and discharge curves of V3S4@NC anode material at 0.1A·g-1;

[0027] a is the charge-discharge curve of V3S4@NC electrode at 0.1A·g-1; b is the rate characteristics of V3S4@NC electrode at different current densities; c is the long-term cycle stability of V3S4@NC electrode at 10A·g-1; d is the electrochemical impedance spectroscopy (EIS) curve of V3S4@NC electrode; e is the cyclic voltammetry curve of V3S4@NC electrode. . DETAILED DESCRIPTION

[0028] The graphene-coated V3S4@NC material disclosed in the present invention is composed of V3S4@NC and graphene coated on the surface of V3S4@NC. The V3S4@NC is a core-shell structure nanofiber composite material with V3S4 as a core and NC as a shell.

[0029] Specifically, the crystal structure of V3S4 is a monoclinic crystal structure.

[0030] As we all know, graphene has excellent chemical / physical properties, such as a large theoretical specific surface area (≈2630m2g-1), high electronic conductivity, and high mechanical strength. In addition, the doping of heteroatoms (such as N, B, S, and P) can further improve the conductivity and electrochemical sodium ion storage. It can not only be used as a skeleton for the growth of other active materials, but also contribute to sodium ion storage. In this context, the construction of graphene-based composite electrodes can effectively improve the electronic / ionic conductivity of the entire electrode and increase the active sodium ion storage sites. At the same time, the synergistic effect of graphene with other active materials can enhance the charge and discharge platform, accelerate the transfer of ions / electrons at the working interface, and enhance the structural stability. In addition, the introduction of graphene can well accommodate volume expansion and prevent the aggregation of active materials, resulting in excellent electrochemical performance.

[0031] However, when graphene is compounded with other materials, it is easy to produce agglomeration effect, which makes the graphene dispersed unevenly and the coating effect is poor. Under this premise, the inventor unexpectedly found that graphene can be well dispersed and coated with V3S4@NC material, and the obtained graphene-coated V3S4@NC material has excellent electrochemical properties. The following is the preparation method of the above material:

[0032] Step 1: sulfur powder, vanadium acetylacetonate (VO(acac)2), polyacrylonitrile (PAN) and graphene oxide are added to N-N-dimethylformamide (DMF), stirred for 12 hours, and subjected to ultrasonic oscillation to obtain a mixed solution;

[0033] Step 2: Fill the mixed solution obtained in step 1 into a syringe, perform electrospinning at a flow rate of 0.4 mL / h at a voltage of 18 kV, collect the product, and obtain a precursor;

[0034] Step 3: Place the collected precursor in a protective atmosphere and anneal at 800°C for 3h to obtain graphene-coated V3S4@NC material.

[0035] Specifically, the average particle size of the sulfur powder is 400-800 meshes, the average particle size of the vanadium acetylacetonate powder is 600-1000 meshes, the purity of the sulfur powder and the vanadium acetylacetonate powder are both analytically pure, the average molecular weight of the polyacrylonitrile powder is 50,000-200,000, the number of layers of graphene oxide is 15-20 layers, and the protective atmosphere is an inert atmosphere;

[0036] More specifically, sulfur powder, vanadyl acetylacetonate (VO(acac)2), polyacrylonitrile (PAN) and graphene oxide are added to N-N dimethylformamide (DMF) in a mass ratio of 1:4:5:2, stirred for 12 hours and ultrasonically oscillated for 12 hours to obtain a mixed solution; the protective atmosphere is an inert atmosphere of a mixed gas of argon and hydrogen, and the volume ratio of the argon to the hydrogen is 95:5.

[0037] The sulfur powder and vanadyl acetylacetonate in the mixed solution obtained in step 1 are reacted to obtain a mixed solution of V3S4 particles and unreacted polyacrylonitrile and graphene oxide; in step 2, the mixed solution is spun by an electrostatic spinning method at a voltage of 18 kV and a flow rate of 0.4 mL / h to obtain a precursor, which includes V3S4 silk, polyacrylonitrile precursor and graphene; the precursor is placed in a protective atmosphere, and annealed at 800° C. by a solid-state annealing method, and the polyacrylonitrile precursor is annealed at 800° C. During annealing, nitrogen-doped carbon (NC) fibers are formed and coated on the V3S4 filaments, forming a core-shell structure with the V3S4 filaments, namely V3S4@NC. Graphene oxide is reduced to graphene during the annealing process. Since there is a strong capillary force between the V3S4@NC fibers and the graphene, it helps to anchor the graphene flakes, reduce the agglomeration effect, and help the graphene sheets to be better dispersed, so that the graphene is coated on the outer surface of the V3S4@NC fiber, which is the graphene-coated V3S4@NC material described in the present disclosure.

[0038] The above material or the graphene-coated V3S4@NC material prepared by the above method is applied to the anode of a sodium ion battery. Specifically, the electrolyte of the sodium ion battery is NaClO4, and the anode material is selected from conductive carbon black (super P), polyvinylidene fluoride (PVDF) and the above material or the graphene-coated V3S4@NC material prepared by the above method. More specifically, the mass ratio of graphene-coated V3S4@NC material, conductive carbon black (super P) and polyvinylidene fluoride (PVDF) is 80:10:10. The above graphene-coated V3S4@NC material, conductive carbon black (super P) and polyvinylidene fluoride (PVDF) are mixed in N-methylpyrrolidone (NMP) at a mass ratio of 80:10:10 to obtain a mixed slurry. The mixed slurry is cast on a clean copper foil and heated at 110°C for 16 hours as a working anode. Metallic sodium is selected as the cathode, 1M NaClO4 is selected as the electrolyte, and Celgard is selected as the 2400 was used as a battery separator and assembled to obtain a coin cell.

[0039] In the description of the present disclosure, it is necessary to understand that the directions or positional relationships indicated by directional words such as "front, back, up, down, left, right", "lateral, vertical, horizontal" and "top, bottom" are usually based on the directions or positional relationships shown in the drawings, and are only for the convenience of describing the present disclosure and simplifying the description. Unless otherwise specified, these directional words do not indicate or imply that the device or element referred to must have a specific orientation or be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the scope of protection of the present disclosure.

[0040] For those skilled in the art, various other corresponding changes and deformations can be made according to the technical solutions and concepts described above, and all of these changes and deformations should fall within the protection scope of the claims of the present disclosure.

Claims

1. A graphene-coated V3S4@NC material, characterized in that: The invention is composed of V3S4@NC and graphene coated on the surface of V3S4@NC. The V3S4@NC is a nanofiber composite material with a core-shell structure, which has V3S4 as a core and NC as a shell.

2. The graphene-coated V3S4@NC material according to claim 1, characterized in that: The crystal structure of the V3S4 is a monoclinic crystal structure.

3. The method for preparing the graphene-coated V3S4@NC material according to claim 1 or 2, characterized in that: The following steps are involved: Step 1: sulfur powder, vanadium acetylacetonate (VO(acac)2), polyacrylonitrile (PAN) and graphene oxide are added to N-N-dimethylformamide (DMF), stirred for 12 hours, and subjected to ultrasonic oscillation to obtain a mixed solution; Step 2: Fill the mixed solution obtained in step 1 into a syringe, perform electrospinning at a flow rate of 0.4 mL / h at a voltage of 18 kV, collect the product, and obtain a precursor; Step 3: Place the collected precursor in a protective atmosphere and anneal at 800°C for 3h to obtain graphene-coated V3S4@NC material.

4. The preparation method according to claim 3, characterized in that: The average particle size of sulfur powder is 400-800 meshes, the average particle size of vanadium acetylacetonate powder is 600-1000 meshes, the purity of sulfur powder and vanadium acetylacetonate powder are both analytically pure, the average molecular weight of polyacrylonitrile powder is 50,000-200,000, and the number of graphene oxide layers is 15-20.

5. The preparation method according to claim 3, characterized in that: The protective atmosphere is an inert atmosphere.

6. The preparation method according to claim 3, characterized in that: The inert atmosphere is a mixed gas of argon and hydrogen, and the volume ratio of the argon to the hydrogen is 95:

5.

7. Use of the graphene-coated V3S4@NC material according to any one of claims 1 to 2 or the graphene-coated V3S4@NC material obtained by the preparation method according to any one of claims 3 to 6, characterized in that: It is used as the anode of sodium-ion batteries.

8. A sodium ion battery, characterized in that: Comprising the sodium ion battery anode as described in claim 7.

Citation Information

Patent Citations

  • Preparation method of high-power aqueous zinc ion battery positive electrode material

    CN110828802A

  • Preparation method and application of transition metal sulfide / nitrogen-sulfur co-doped carbon composite fiber electrode material

    CN112599777A

  • Preparation method and application of V3S4C / G composite electrode material

    CN114843476A

  • Nanometer composite electrode material, magnesium-lithium hybrid battery and preparation method

    CN116314725A

  • Composite positive electrode material, preparation method therefor, and application in zinc ion battery

    US20230343929A1

Cited By

  • Negative pole piece, preparation method thereof and battery

    CN121964525A