Negative electrode active material, secondary battery, and electronic device

By forming an outer layer structure of conductive agent and nitrile polymer on the surface of silicon-based materials, the energy density and safety problems of graphite and elemental silicon in secondary batteries are solved, the circulation and high-temperature performance of secondary batteries are improved, and the Higher energy density and stability.

CN118943327AActive Publication Date: 2024-11-12NINGDE AMPEREX TECHNOLOGY LTD

Patent Information

Application Number
CN202410994289.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

The low energy density and safety risks of graphite as the negative electrode active material in existing secondary batteries limit their application. Due to volume expansion and low conductivity, single silicon is difficult to apply on a large scale. Existing improved methods such as silicon nano-solution and porous silicon or Silicon-carbon composites cannot completely solve these problems.

Method used

By forming an outer layer material composed of conductive agent and nitrile polymer on the surface of the silicon-based material, a highly flexible and closely interwoven outer layer structure is formed, which improves electrical conductivity and promotes the formation of a stable solid electrolyte interface film (SEI film) and buffers Volume expansion and stress optimize the circulation and high temperature performance of secondary batteries.

Benefits of technology

It significantly improves the first Coulomb efficiency, cycle stability and high-temperature storage performance of secondary batteries, reduces structural damage and electrolyte decomposition, and enhances the interface stability and energy density of the negative electrode active material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943327A_ABST
    Figure CN118943327A_ABST
Patent Text Reader

Abstract

The invention provides a negative electrode active material, a secondary battery and electronic equipment, and belongs to the technical field of batteries. The negative electrode active material provided by the invention comprises a silicon-based material and an outer layer material, the outer layer material comprises a conductive agent and a nitrile polymer; the infrared spectrum of the negative electrode active material comprises infrared characteristic peaks of cyano groups; the negative electrode active material comprises a nitrogen element and a silicon element; based on the mass of the negative electrode active material, the mass content of the nitrogen element is D1%, the mass content of the silicon element is G%, and D1 / G is larger than or equal to 0.02 and smaller than or equal to 0.5. According to the present invention, the outer layer material comprising the conductive agent and the nitrile polymer is formed on the surface of the silicon-based material, such that the conductivity and the stability of the negative electrode active material can be improved, the secondary battery has the excellent cycle capacity retention rate and the excellent expansion inhibition performance, and the high-temperature storage performance of the secondary battery can be further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of battery technology, and specifically relates to a negative electrode active material, a secondary battery and an electronic device. Background Art

[0002] With the increasing demand for large-scale storage, electric vehicles, and portable electronic devices, the development of energy storage devices with higher energy density has become a top priority. Secondary batteries are widely used in various fields due to their long cycle life and environmentally friendly characteristics. However, as a traditional negative electrode active material for secondary batteries, graphite is limited in its further application due to its low capacity (372mAh / g) and safety hazards such as active material precipitation. Therefore, the development of negative electrode active materials with high energy density and high safety has become the key to the development of current secondary battery technology.

[0003] Compared with carbon-based materials such as graphite, silicon has a very high theoretical specific capacity (Li 15 Si4, 3579mAh / g) and suitable operating voltage (<0.5V vs.Li / Li + ), is considered to be the most promising negative electrode active material to replace graphite. However, the huge volume expansion and low conductivity of elemental silicon during the alloying / de-alloying process severely restrict its large-scale application in secondary batteries.

[0004] To solve the above problems, the existing technology mainly adopts methods such as nano-sizing silicon, constructing porous silicon or silicon-carbon negative electrode active materials, and introducing transition metal oxides. Although silicon nano-sizing and porous silicon can alleviate the volume expansion problem of elemental silicon to a certain extent, their high specific surface area and low tap density limit their large-scale application. Although silicon-carbon composites and the introduction of transition metal oxides can reduce the volume expansion of silicon, due to the mechanical properties and chemical stability of carbon and metal oxides are not outstanding, they cannot achieve the ideal buffering effect. Summary of the invention

[0005] In order to solve the above problems, the present application provides a negative electrode active material, a secondary battery and an electronic device, which can improve the conductivity of the negative electrode active material and reduce the volume expansion during the charging and discharging process, and improve the first coulombic efficiency, expansion inhibition performance, cycle performance and high-temperature storage performance of the secondary battery.

[0006] In the first aspect, the present application provides a negative electrode active material, including a silicon-based material and an outer layer material; the outer layer material is located on at least part of the surface of the silicon-based material; the outer layer material includes a conductive agent and a nitrile polymer; the infrared spectrum of the negative electrode active material includes an infrared characteristic peak of a cyano group, and the infrared characteristic peak of a cyano group is located at 2250cm -1 Up to 2400cm -1Between; the negative electrode active material includes nitrogen and silicon; based on the mass of the negative electrode active material, the mass content of nitrogen is D1%, and the mass content of silicon is G%, 0.02≤D1 / G≤0.5. The present application utilizes a conductive agent and a cyanide-containing nitrile polymer to form a first shell, and the conductive network formed by the conductive agent on the surface of the silicon-based material can improve the overall conductivity of the negative electrode active material, reduce the negative electrode internal resistance, and improve the first coulomb efficiency of the secondary battery. Among them, when the mass content of nitrogen and silicon in the negative electrode active material is controlled to meet the above range, the conductive agent and the nitrile polymer can form a highly flexible and tightly interwoven outer layer material on the surface of the silicon-based material, and can also promote the formation of a stable solid electrolyte interface film (SEI film) on the surface of the negative electrode active material, which helps to buffer the volume expansion and stress of the silicon-based material under high temperature conditions and during the cycle, improve the interface stability of the negative electrode active material, reduce the structural damage of the negative electrode active material and the decomposition of the electrolyte, improve the expansion problem of the secondary battery containing the silicon system, and improve the high temperature storage performance and cycle stability of the secondary battery.

[0007] In some embodiments, the negative electrode active material satisfies at least one of the following conditions:

[0008] (1) 1.1≤D1≤18.4; Controlling the nitrogen content in the negative electrode active material within this range can improve the quality of the SEI film, reduce the decomposition of the electrolyte and the generation of by-products, and enable the secondary battery to exhibit higher cycle performance and first coulombic efficiency.

[0009] (2) 36.8≤G≤68.3; Controlling the silicon content in the negative electrode active material within this range can make the negative electrode active material have a higher specific capacity, and at the same time, after being combined with the conductive agent and nitrile polymer in the outer layer material, it can significantly improve the expansion inhibition performance and cycle performance of the secondary battery.

[0010] (3) 0.04≤D1 / G≤0.37. Regulating the mass ratio of nitrogen and silicon within this range can further improve the film quality of the SEI film, maintain a high cycle stability of the negative electrode active material, optimize the flexible conductive network structure of the outer layer material, absorb the volume change of the silicon-based material, improve the expansion inhibition performance of the secondary battery, and optimize the cycle performance and high-temperature storage performance of the secondary battery.

[0011] In some more preferred embodiments, the negative electrode active material satisfies at least one of the following conditions:

[0012] (1) 2.3≤D1≤9.2; Nitrile polymers with nitrogen content within this range can further improve the initial coulombic efficiency and cycle performance of secondary batteries.

[0013] (2) 43.2≤G≤51.3; Silicon within this content range can enable the secondary battery to exhibit better expansion suppression performance and cycle performance.

[0014] (3) 0.06≤D1 / G≤0.19. Controlling the mass ratio of nitrogen and silicon in the negative electrode active material to meet this range can further improve the expansion suppression performance, cycle performance and high-temperature storage performance of the secondary battery.

[0015] In some embodiments, the sphericity of the negative electrode active material is S, 0.8≤S≤1.0; when the sphericity of the negative electrode active material is regulated to meet this condition, it is combined with an outer layer material including a conductive agent and a nitrile polymer to release the stress of the negative electrode active material more evenly under high temperature conditions or during cycling, buffer the volume expansion and reduce the structural damage of the negative electrode active material, thereby improving the expansion inhibition performance, cycle performance and high temperature storage performance of the secondary battery.

[0016] In some embodiments, in the negative electrode active material, the thickness of the outer layer material is T nm, 0.5≤T≤200.0. The present application regulates the thickness of the outer layer material to meet this range, which can make the negative electrode active material have a higher gram capacity, improve the conductivity of the negative electrode active material, and also help to improve the interface stability of the negative electrode active material, optimize the expansion inhibition performance, cycle performance and high temperature storage performance of the secondary battery.

[0017] In some embodiments, the negative electrode active material satisfies at least one of the following conditions:

[0018] (1) 0.9≤S≤1.0; when the sphericity of the secondary battery is further adjusted to meet this range, the secondary battery can have higher expansion inhibition performance, cycle performance and high-temperature storage performance.

[0019] (2) 0.5≤T≤100.0; By adjusting the thickness T of the outer layer material to meet this range, the expansion suppression performance, cycle performance and high-temperature storage performance of the secondary battery can be more significantly improved.

[0020] (3) 0.5≤S×T≤90.0; preferably, 10.4≤S×T≤67.8; controlling the value of S×T to meet this range can promote the close coordination of the components in the negative electrode active material, uniformly release the stress in the negative electrode active material, and improve the initial coulombic efficiency, expansion inhibition performance, high temperature storage performance and cycle performance of the secondary battery.

[0021] (4) The average particle size of the negative electrode active material is Rμm; 5.6≤R≤10.3. Controlling the average particle size of the negative electrode active material within this range can enable the negative electrode active material to achieve a suitable specific surface area, reduce the consumption of electrolyte, and also help to increase the compaction density of the negative electrode active material, so that the secondary battery has a higher energy density and cycle performance.

[0022] In some embodiments, the negative electrode active material satisfies at least one of the following conditions:

[0023] (1) The conductive agent includes single-walled carbon nanotubes and / or multi-walled carbon nanotubes; the present application uses these carbon nanotubes as conductive agents to achieve long-range conductivity, further improve the conductivity of the negative electrode active material, and when combined with the nitrile polymer of the present application, the secondary battery can exhibit higher first coulombic efficiency and cycle performance.

[0024] (2) The nitrile polymer includes at least one of polyacrylonitrile, polycyanoacrylate, and polycyanobenzene; these nitrile polymers can promote the improvement of the stability of the interface during the cycle, thereby improving the cycle performance and anti-expansion performance of the secondary battery. Among them, the nitrile polymer is preferably polyacrylonitrile. The use of polyacrylonitrile can rivet the outer layer material on the silicon-carbon material, form a good coating on the silicon-based material, improve the interface stability of the negative electrode active material and reduce the generation of interface byproducts, thereby improving the cycle stability, high temperature storage performance and anti-expansion performance of the secondary battery.

[0025] (3) The silicon-based material includes a porous carbon skeleton and a silicon material; the silicon material is located on the surface and / or inside the porous carbon skeleton. This type of silicon-based material can better cooperate with the outer layer material to improve the cycle performance, high temperature storage performance and expansion inhibition performance of the secondary battery.

[0026] In a second aspect, the present application provides a secondary battery comprising a positive electrode, a negative electrode and an electrolyte; the negative electrode comprises a negative electrode collector and a negative electrode mixture layer arranged on at least a portion of the surface of the negative electrode collector, and the negative electrode mixture layer comprises any one of the negative electrode active materials provided in the first aspect of the present application.

[0027] In some embodiments, the negative electrode mixture layer includes sodium element, based on the mass of the negative electrode mixture layer, the mass content of nitrogen element is D2%, and the mass content of sodium element is N%; the negative electrode mixture layer satisfies at least one of the following conditions:

[0028] (1) 0.58≤N≤1.74; preferably, 0.81≤N≤1.04; by regulating the content of the sodium element in the negative electrode mixture layer within the above range, the dispersant can be combined with the negative electrode active material of the present application to fully exert the effect of improving the first coulombic efficiency of the secondary battery.

[0029] (2) 1.6≤D2≤8.1; preferably, 5.0≤D2≤7.8; By controlling the mass content of nitrogen in the negative electrode mixture layer to meet the above range, the gram capacity and conductivity of the secondary battery can be increased, and its cycle performance and expansion inhibition performance can be improved.

[0030] (3) 2.35≤D2 / N≤11.74; preferably, 4.81≤D2 / N≤9.63; controlling the mass ratio of nitrogen and sodium in the negative electrode mixture layer to meet the above range can increase the energy density of the secondary battery and improve the initial coulombic efficiency, cycle performance and expansion inhibition performance of the secondary battery.

[0031] (4) The sodium element comes from at least one of sodium alginate, sodium carboxymethyl cellulose, sodium hydroxymethyl cellulose or sodium hydroxyethyl carboxymethyl cellulose.

[0032] In some embodiments, the electrolyte includes at least one of fluorobenzene or fluoroethylene carbonate; based on the mass of the electrolyte, the electrolyte satisfies at least one of the following conditions:

[0033] (1) The mass content of fluorobenzene is F1%, 0.9≤F1≤5.2; preferably, 2.1≤F1≤3.1; when the electrolyte of the secondary battery contains fluorobenzene and the mass content of fluorobenzene in the electrolyte is regulated to meet the above range, the high-temperature storage performance of the secondary battery can be further optimized, and its first coulombic efficiency, cycle performance and expansion inhibition performance can be improved.

[0034] (2) The mass content of fluoroethylene carbonate is F2%, 3.8≤F2≤7.4. Regulating the mass content of fluoroethylene carbonate (FEC) in the electrolyte to meet the above range can enable the secondary battery to achieve better high-temperature storage performance, cycle performance and expansion inhibition performance.

[0035] In a third aspect, the present application provides an electronic device, comprising the secondary battery provided in the second aspect of the present application.

[0036] Based on the above-mentioned negative electrode active materials, secondary batteries and electronic devices of the present application, by forming an outer layer material including a conductive agent and a nitrile polymer on the surface of the silicon-based material, the conductivity of the negative electrode active material, as well as the stability of the interface and structure can be improved at the same time, so that the secondary battery can have excellent cycle capacity retention and expansion inhibition performance at high energy density. In addition, it can promote the formation of a more stable SEI film, further improving the cycle performance and high-temperature storage performance of the secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is an infrared spectrum of the negative electrode active material provided in Example 1-1 of the present application;

[0038] Figure 2 This is a partially enlarged view of the infrared spectrum of the negative electrode active material provided in Example 1-1 of the present application. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical solution and advantages of the present application more clear, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described here are only used to explain the present application and are not used to limit the present application.

[0040] In the first aspect, the present application provides a negative electrode active material, including a silicon-based material and an outer layer material; the outer layer material is located on at least part of the surface of the silicon-based material; the outer layer material includes a conductive agent and a nitrile polymer; the infrared spectrum of the negative electrode active material includes an infrared characteristic peak of a cyano group, and the infrared characteristic peak of a cyano group is located at 2250cm -1 Up to 2400cm -1 Between; the negative electrode active material includes nitrogen and silicon; based on the mass of the negative electrode active material, the mass content of nitrogen is D1%, the mass content of silicon is G%, and 0.02≤D1 / G≤0.5. The present application forms an outer layer material including a conductive agent and a nitrile polymer on the surface of the silicon-based material, which enables the conductive agent to form a conductive network structure on the surface of the negative electrode active material, improve the conductivity of the negative electrode active material, and improve the electronic conductivity. The combination with the silicon-based material can improve the energy density of the secondary battery, and at the same time promote the ion transfer rate of the secondary battery during the charging and discharging process, and improve the first coulomb efficiency. On this basis, the mass proportion of silicon and nitrogen in the negative electrode active material is controlled to meet the above relationship, which can improve the flexibility and structural stability of the outer layer material, and promote the formation of a stable SEI film on the surface of the negative electrode active material, which helps to buffer the volume expansion and stress of the silicon-based material under high temperature conditions and during the cycle, reduce the structural damage of the negative electrode active material and the decomposition of the electrolyte, and improve the expansion inhibition performance, high temperature storage performance and cycle stability of the secondary battery.

[0041] In the present application, the mass content of silicon and nitrogen in the negative electrode active material satisfies 0.02≤D1 / G≤0.5, preferably 0.04≤D1 / G≤0.37, and more preferably 0.06≤D1 / G≤0.19. For example, the value of D1 / G is 0.02, 0.04, 0.06, 0.09, 0.12, 0.14, 0.16, 0.19, 0.20, 0.23, 0.26, 0.30, 0.31, 0.33, 0.36, 0.37, 0.42, 0.43, 0.46, 0.48, 0.5 or a value in the range composed of any two of these values. Controlling the content ratio of silicon and nitrogen in the above range can enhance the coordination effect of nitrile polymers and silicon-based materials, and further improve the cycle performance and high temperature storage performance of secondary batteries during the cycle process.

[0042] In some embodiments, 1.1≤D1≤18.4; preferably 2.3≤D1≤9.2. Exemplarily, D1 is 1.1, 1.3, 2.3, 3.8, 4.6, 6.8, 7.1, 9.2, 11.2, 11.8, 13.6, 14.9, 15.7, 17.3, 18.4 or a value in the range formed by any two of these values. Regulating the content of nitrogen in the negative electrode active material within the above range can improve the stability of the SEI film, reduce the side reaction between the silicon-based material and the electrolyte, and improve the volume stability of the silicon-based material, further improving the high temperature storage performance, cycle performance and expansion inhibition performance of the secondary battery.

[0043] In some embodiments, 36.8≤G≤68.3, preferably 43.2≤G≤51.3, for example, G can be 36.8, 38.8, 40.0, 43.2, 44.3, 47.0, 49.2, 51.3, 53.4, 55.4, 58.1, 59.8, 62.5, 65.2, 67.1, 68.3 or a value in the range formed by any two of these values. After controlling the content of silicon in the negative electrode active material within the above range and combining it with the nitrile polymer, the gram capacity of the negative electrode active material can be increased, the volume expansion effect can be reduced, and the volume stability of the negative electrode active material during the cycle process can be improved, thereby improving the expansion inhibition performance and cycle performance of the secondary battery.

[0044] In the present application, there is no particular restriction on the method for regulating the mass content of silicon and nitrogen in the negative electrode active material, as long as the purpose of the present application can be achieved. For example, the mass content of silicon can be regulated by controlling the silicon content in the silicon-based material, or by changing the addition ratio of the silicon-based material, and the mass content of nitrogen can be regulated by controlling the addition ratio of the nitrile compound.

[0045] The element content (silicon, nitrogen, etc.) of the negative electrode active material in the present application can be tested by methods known in the art. For example, the element content of the negative electrode active material sample can be quantitatively tested using a Shimadzu / Kratos X-ray photoelectron spectrometer AXIS SUPRA+.

[0046] In some embodiments, the sphericity of the negative electrode active material is S, 0.8≤S≤1.0; preferably 0.9≤S≤1.0; for example, S is 0.8, 0.81, 0.82, 0.84, 0.85, 0.87, 0.89, 0.91, 0.92, 0.93, 0.94, 0.96, 0.97, 0.99, 1.0 or a value in the range formed by any two of these values. The sphericity of the negative electrode active material is regulated to meet the above range, and in combination with the outer layer material including the conductive agent and the nitrile polymer, the stress of the negative electrode active material can be released more uniformly under high temperature conditions or during the cycle process, the volume expansion can be buffered, and the structural damage of the negative electrode active material can be reduced, thereby improving the expansion inhibition performance, cycle performance and high temperature storage performance of the secondary battery.

[0047] In the present application, the sphericity S of the negative electrode active material can be tested by methods known in the art, for example, the sphericity of the negative electrode active material can be tested by the equivalent diameter method, and the testing method includes: using a ZEISS-SEM (sigma-02-33) scanning electron microscope to observe the particle sample of the negative electrode active material, randomly selecting 20 negative electrode active material particles, and calculating the circumference equivalent diameter and area equivalent diameter of each; or, cutting the negative electrode sheet to obtain the test surface, performing argon ion polishing on the test surface to obtain the test sample, and then using a scanning electron microscope to observe the negative electrode active material in the test sample, randomly selecting 20 negative electrode active material particles, and calculating the circumference equivalent diameter and area equivalent diameter of the negative electrode active material particles. The sphericity of each negative electrode active material particle = circumference equivalent diameter / area equivalent diameter, and calculating the arithmetic mean of the sphericity of the 20 negative electrode active material particles to obtain the sphericity of the negative electrode active material.

[0048] In some embodiments, in the negative electrode active material, the thickness of the outer layer material is T nm, 0.5≤T≤200.0; preferably 0.5≤T≤100.0. Exemplarily, T is 0.5, 4.7, 17.6, 27.2, 37.5, 50.5, 54.4, 67.9, 76.2, 92.5, 100.0, 104.7, 111.3, 125.7, 129.8, 143.3, 150.1, 160.9, 171.7, 185.6, 189.9, 200 or a value in the range composed of any two of these values. The present application regulates the thickness of the outer layer material to meet the above range, so that the negative electrode active material has a higher gram capacity, improves the conductivity of the negative electrode active material, and is also beneficial to improve the interface stability of the negative electrode active material, and optimizes the expansion inhibition performance, cycle performance and high temperature storage performance of the secondary battery.

[0049] The present application does not impose any special restrictions on the test method for the thickness of the outer layer material of the negative electrode active material, and the test can be performed using methods known in the art. For example, 20 negative electrode active materials can be randomly selected to prepare 20 cross-sectional samples of the negative electrode active materials, and a scanning electron microscope is used to observe and count the maximum and minimum thickness values ​​of the outer layer material on the cross-section of each negative electrode active material, and the arithmetic mean of the maximum and minimum thickness values ​​is calculated as the thickness of the outer layer material in a single negative electrode active material, and then the arithmetic mean of the 20 negative electrode active materials is calculated and recorded as the thickness T nm of the outer layer material.

[0050] In some embodiments, 0.5≤S×T≤90.0; preferably, 10.4≤S×T≤67.8. Exemplarily, the value of S×T is 0.5, 2.0, 6.7, 12.6, 14.9, 22.0, 24.9, 33.1, 34.9, 40.3, 45.2, 48.0, 56.6, 60.4, 65.7, 69.6, 75.2, 77.4, 82.8, 88.6, 90.0 or a value in the range formed by any two of these values. Controlling the value of S×T to meet the above range can promote the close cooperation of the components in the negative electrode active material, uniformly release the stress in the negative electrode active material, and improve the first coulombic efficiency, expansion inhibition performance, high temperature storage performance and cycle performance of the secondary battery.

[0051] In some embodiments, the average particle size of the negative electrode active material is Rμm, 5.6≤R≤10.3. For example, R can be 5.6, 5.9, 6.2, 6.6, 7.0, 7.1, 7.7, 8.1, 8.3, 8.7, 8.9, 9.3, 9.8, 10.0, 10.3 or a value within the range formed by any two of these values. On the basis of controlling the element content of the above-mentioned negative electrode active material, the present application further regulates the average particle size of the negative electrode active material within the above-mentioned range, so that the negative electrode active material has a suitable specific surface area, which is beneficial to improve the synergistic effect between the elements, reduce the occurrence of side reactions during the cycle and the consumption of the electrolyte, and also help to improve the compaction density of the negative electrode active material, which is beneficial to improve the conductivity of the negative electrode active material, and improve the cycle performance and the first coulomb efficiency of the secondary battery.

[0052] The average particle size of the negative electrode active material in the present application can be tested by a method known in the art, for example, it can be tested by a method comprising the following steps: selecting a sample area on the negative electrode plate, taking a SEM photo of the sample area by a scanning electron microscope, and then using image analysis software to randomly select 10 particles of the negative electrode active material from the SEM photo as samples, and calculate the area of ​​each of these negative electrode active material samples. Then, assuming that the negative electrode active material samples are spherical, the particle size R0 (diameter) of each of these negative electrode active material samples is calculated by the following formula: R0 = 2×(S / π) 1 / 2 ; Wherein, S is the area of ​​the negative electrode active material sample. The three SEM images are processed to obtain the particle size R0 of the negative electrode active material sample, and the particle sizes of the obtained 30 (10×3) negative electrode active material samples are arithmetic averaged to obtain the average particle size R of the negative electrode active material to be tested.

[0053] In some embodiments, the conductive agent includes single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The use of single-walled carbon nanotubes or multi-walled carbon nanotubes can further improve the conductivity of the negative electrode active material, and when combined with the nitrile polymer of the present application, it can optimize the structural stability of the outer layer material, further improve the cycle stability of the negative electrode active material, and enable the secondary battery to exhibit higher first coulomb efficiency, cycle performance, and expansion inhibition performance.

[0054] In some embodiments, nitrile polymers include polyacrylonitrile. When polyacrylonitrile is combined with the conductive agent and silicon-based material of the present application, it can further promote the improvement of interface stability during the cycle process, thereby improving the cycle stability, high-temperature storage performance and expansion inhibition performance of the secondary battery.

[0055] In the present application, the silicon-based material may adopt materials known in the art, such as silicon-carbon materials, silicon-oxygen materials and silicon. In some preferred embodiments, the silicon-based material includes a porous carbon skeleton and a silicon material; the silicon material is located on the surface and / or inside the porous carbon skeleton. This type of silicon-carbon material can better cooperate with the outer layer material, and the porous carbon skeleton and the outer layer material can cooperate to multiple fixation and support of silicon, which can further limit the expansion effect during the silicon alloying process, improve the expansion inhibition performance and cycle stability of the secondary battery, and also help to improve the overall conductivity of the negative electrode active material, promote the embedding and removal of active substances, and improve the energy density and first coulomb efficiency of the secondary battery.

[0056] The silicon-carbon material used in the present application can be prepared by methods known in the art, and the present application does not impose any particular limitation thereto, as long as the purpose of the present application can be achieved. For example, the silicon-carbon material can be prepared by chemical vapor deposition of a silicon source and a carbon source.

[0057] In some embodiments, the negative electrode active material is prepared by a method comprising the following steps:

[0058] S1: Provide silicon-carbon material; the silicon-based material includes a porous carbon skeleton and a silicon material; the silicon material is located on the surface and inside of the porous carbon skeleton.

[0059] S2: performing a first dispersion treatment on the conductive agent and the nitrile polymer in a solvent to obtain a dispersion system; wherein the solvent comprises at least one of water, ethanol, propanol, butanol, ethylene glycol, propylene glycol, dimethyl carbinol, dimethyl sulfoxide, and ethyl acetate;

[0060] S3: adding the silicon-carbon material in S1 to the dispersion system in S2 for a second dispersion treatment, and then drying the same to obtain the negative electrode active material of the present application.

[0061] The present application does not impose any particular restrictions on the specific parameters of the first dispersion treatment, the second dispersion treatment and the drying treatment in the preparation method of the negative electrode active material, as long as the purpose of the present application can be achieved. During the first dispersion treatment, there is no particular restriction on the order of adding the conductive agent and the nitrile polymer, as long as the purpose of the present application can be achieved. For example, the order of adding the conductive agent and the nitrile polymer can be adjusted so that the two have different first dispersion treatment times, and the area proportion of the conductive agent and the nitrile polymer in the outer layer material can be regulated.

[0062] In a second aspect, the present application provides a secondary battery comprising a positive electrode, a negative electrode and an electrolyte; the negative electrode comprises a negative electrode collector and a negative electrode mixture layer arranged on at least a portion of the surface of the negative electrode collector, and the negative electrode mixture layer comprises any one of the negative electrode active materials provided in the first aspect of the present application.

[0063] The secondary battery of the present application is not particularly limited, and may include, but is not limited to, lithium ion secondary batteries (lithium ion batteries) and sodium ion batteries.

[0064] In some embodiments, the negative electrode mixture layer includes sodium, based on the mass of the negative electrode mixture layer, the mass content of nitrogen is D2%, and the mass content of sodium is N%; 2.35≤D2 / N≤11.74; preferably, 4.81≤D2 / N≤9.63; for example, the value of D2 / N is 2.35, 2.95, 3.61, 4.41, 4.81, 4.93, 5.31, 6.26, 7.09, 7.82, 8.76, 9.14, 9.63, 10.07, 11.00, 11.74 or a value in the range of any two of these values. Controlling the mass ratio of nitrogen and sodium in the negative electrode mixture layer to meet the above range can increase the energy density of the secondary battery, and improve the first coulomb efficiency, cycle performance and expansion inhibition performance of the secondary battery.

[0065] In some embodiments, 0.58≤N≤1.74; preferably, 0.81≤N≤1.04; for example, N is 0.58, 0.61, 0.70, 0.76, 0.81, 0.86, 0.99, 1.04, 1.15, 1.25, 1.37, 1.40, 1.53, 1.57, 1.70, 1.74 or a value in the range formed by any two of these values. Regulating the content of the sodium element in the negative electrode mixture layer within the above range enables the dispersant to cooperate with the negative electrode active material of the present application, giving full play to the improvement of the first coulomb efficiency of the secondary battery, and is beneficial to the cycle performance and high temperature storage performance of the secondary battery.

[0066] In some embodiments, 1.6≤D2≤8.1; preferably, 5.0≤D2≤7.8; for example, D2 is 1.6, 2.0, 2.5, 2.8, 3.4, 3.7, 4.4, 5.0, 5.2, 5.6, 6.4, 6.7, 7.2, 7.8, 8.1 or a value in the range formed by any two of these values. By controlling the mass content of nitrogen in the negative electrode mixture layer to meet the above range, the gram capacity and conductivity of the secondary battery can be increased, and its cycle performance, high temperature storage performance and expansion inhibition performance can be improved.

[0067] In some embodiments, the sodium element is from at least one of sodium alginate, sodium carboxymethyl cellulose, sodium hydroxymethyl cellulose or sodium hydroxyethyl carboxymethyl cellulose. The above dispersant can better cooperate with the negative electrode active material of the present application to improve the first coulombic efficiency, cycle performance, high temperature storage performance and expansion inhibition performance of the secondary battery.

[0068] In the present application, the negative electrode active material is included in the negative electrode mixture layer of the negative electrode plate. The negative electrode plate of the present application also includes a negative electrode current collector. In the present application, the negative electrode mixture layer can be arranged on the surface on one side in the thickness direction of the negative electrode current collector, or on the surfaces on both sides in the thickness direction of the negative electrode current collector. It should be noted that the "surface" here can be the entire area of ​​the negative electrode current collector, or it can be a partial area of ​​the negative electrode current collector. This application has no special restrictions, as long as the purpose of this application can be achieved. This application has no special restrictions on the thickness of the negative electrode mixture layer, as long as the purpose of this application can be achieved. For example, the thickness of a single-sided negative electrode mixture layer can be 30μm to 160μm.

[0069] The present application has no particular restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the negative electrode current collector may include copper foil, aluminum foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, composite current collector (such as carbon copper composite current collector, nickel copper composite current collector, titanium copper composite current collector), polymer substrate coated with conductive metal or any combination thereof. The present application has no particular restrictions on the thickness of the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the thickness of the negative electrode current collector is 4μm to 10μm.

[0070] In the present application, the negative electrode mixture layer may also include a negative electrode binder, which may include but is not limited to at least one of polyvinyl alcohol, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyacrylic acid, styrene-butadiene rubber, acrylic (ester) styrene-butadiene rubber, epoxy resin or nylon.

[0071] In the present application, the negative electrode mixture layer may also include a conductive agent. The present application has no particular restrictions on the type of conductive agent in the negative electrode mixture layer, as long as the purpose of the present application can be achieved. For example, the conductive agent may include but is not limited to carbon-based materials, metal-based materials, conductive polymers and mixtures thereof. In some embodiments, the carbon-based material is selected from natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber or any combination thereof. In some embodiments, the metal-based material is selected from metal powder, metal fiber, copper, nickel, aluminum or silver. In some embodiments, the conductive polymer is a polyphenylene derivative. The present application has no particular restrictions on the mass ratio of the negative electrode active material, the conductive agent and the negative electrode binder in the negative electrode mixture layer, as long as the purpose of the present application can be achieved. For example, the loading amount of the negative electrode active material in the negative electrode sheet is 1.0 mg / cm 2 Up to 1.5 mg / cm 2 .

[0072] In some embodiments, the electrolyte includes at least one of fluorobenzene or fluoroethylene carbonate; based on the mass of the electrolyte, the mass content of fluorobenzene is F1%, 0.9≤F1≤5.2; preferably, 2.1≤F1≤3.1; for example, F1 is 0.9, 1.0, 1.2, 1.5, 1.7, 2.0, 2.1, 2.5, 2.7, 2.9, 2.9, 3.3, 3.5, 3.8, 4.0, 4.2, 4.4, 4.6, 4.9, 5.0, 5.2 or a value within the range of any two of these values. When the electrolyte of the secondary battery is controlled to contain fluorobenzene, and the mass content of fluorobenzene in the electrolyte is regulated to meet the above range, the high temperature storage performance of the secondary battery can be further optimized, and its first coulombic efficiency, cycle performance and expansion inhibition performance can be improved.

[0073] In some embodiments, based on the mass of the electrolyte, the mass content of fluoroethylene carbonate is F2%, 3.8≤F2≤7.4, for example, F2 is 3.8, 4.0, 4.2, 4.3, 4.4, 4.6, 4.9, 5.0, 5.3, 5.4, 5.5, 5.7, 6.0, 6.1, 6.4, 6.6, 6.7, 6.8, 7.2, 7.3, 7.4 or a value within the range of any two of these values. By regulating the mass content of fluoroethylene carbonate (FEC) in the electrolyte to meet the above range, the secondary battery can achieve more excellent high temperature storage performance, cycle performance and expansion inhibition performance.

[0074] According to some embodiments of the present application, the electrolyte further includes a lithium salt and a non-aqueous solvent. The lithium salt may include, but is not limited to, lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium difluorophosphate (LiPO2F2), lithium bis(trifluoromethanesulfonyl)imide LiN(CF3SO2)2(LiTFSI), lithium bis(fluorosulfonyl)imide Li(N(SO2F)2)(LiFSI), lithium bis(oxalate borate) LiB(C2O4)2(LiBOB), lithium difluorooxalate borate LiBF2(C2O4)(LiDFOB), LiNO3, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiC(SO2CF3)3, Li2SiF6, lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) or at least one of lithium difluoroborate. The present application does not limit the content of the lithium salt in the electrolyte, as long as the purpose of the present application can be achieved. The application has no particular restrictions on non-aqueous solvents, as long as the purpose of the application can be achieved. For example, non-aqueous solvents may include but are not limited to at least one of carbonate compounds, carboxylate compounds, ether compounds or other organic solvents. The above-mentioned carbonate compounds may include but are not limited to at least one of linear carbonate compounds, cyclic carbonate compounds or fluorocarbonate compounds. The above-mentioned linear carbonate compounds may include but are not limited to at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate or ethyl methyl carbonate (EMC). The above-mentioned cyclic carbonate may include but are not limited to at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate or vinyl ethylene carbonate. The fluorinated carbonate compound may include, but is not limited to, at least one of 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, or trifluoromethylethylene carbonate. The above-mentioned carboxylate compound may include, but is not limited to, at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decalactone, valerolactone, or caprolactone. The above-mentioned ether compound may include but is not limited to at least one of 1,3-dioxolane (DOL), ethylene glycol dimethyl ether (1,2-dimethoxyethane, DME), dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran.The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate or trioctyl phosphate.

[0075] The present application has no special restrictions on the positive electrode, as long as the purpose of the present application can be achieved. For example, the positive electrode comprises a positive electrode current collector and a positive electrode mixture layer located on at least one surface of the positive electrode current collector. The above-mentioned "positive electrode mixture layer located on at least one surface of the positive electrode current collector" means that the positive electrode mixture layer can be located on one surface of the positive electrode current collector along its own thickness direction, or on two surfaces of the positive electrode current collector along its own thickness direction. It should be noted that the "surface" here can be the entire area of ​​the surface of the positive electrode current collector, or it can be a partial area of ​​the surface of the positive electrode current collector. The present application has no special restrictions, as long as the purpose of the present application can be achieved.

[0076] The present application has no particular restrictions on the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the positive electrode current collector may include aluminum foil, aluminum alloy foil or a composite current collector (such as an aluminum-carbon composite current collector). The composite current collector can be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate.

[0077] The positive electrode mixture layer of the present application includes a positive electrode material. The present application has no particular restrictions on the type of positive electrode material, as long as the purpose of the present application can be achieved. For example, the positive electrode material may include lithium nickel cobalt manganese oxide (LiNi 0.90 Co 0.05 Mn 0.05 O2 (NCM955), NCM811, NCM622, NCM523, NCM111), lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium vanadium phosphate, lithium cobalt phosphate, lithium manganese phosphate, lithium manganese iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide (LiCoO2), lithium iron silicate, lithium vanadium silicate, lithium cobalt silicate, lithium manganese silicate, spinel lithium manganese oxide, spinel lithium nickel manganese oxide and lithium titanate. In the present application, the positive electrode material may also contain non-metallic elements, for example, the non-metallic elements include at least one of fluorine, phosphorus, boron, chlorine, silicon or sulfur. In the present application, there is no particular restriction on the thickness of the positive current collector and the positive electrode mixture layer, as long as the purpose of the present application can be achieved. For example, the thickness of the positive current collector is 5μm to 20μm, and the thickness of the single-sided positive electrode mixture layer is 30μm to 120μm.

[0078] In the present application, the positive electrode mixture layer may further include a positive electrode binder and a conductive agent. The present application does not particularly limit the type of positive electrode binder in the positive electrode mixture layer, as long as the purpose of the present application can be achieved. For example, the positive electrode binder may include but is not limited to polyvinylidene fluoride, polytetrafluoroethylene, polyolefins, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, modified polyvinylidene fluoride, modified styrene-butadiene rubber (SBR) or at least one of polyurethane. In some embodiments, the polyolefin binder includes at least one of polyethylene, polypropylene, polyolefin ester, polyolefin alcohol or polyacrylic acid.

[0079] The present application has no particular restrictions on the type of conductive agent in the positive electrode mixture layer, as long as the purpose of the present application can be achieved. For example, the conductive agent can be the same type as the conductive agent in the above-mentioned negative electrode mixture layer. In some embodiments, the conductive agent includes carbon-based materials, such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black or carbon fiber; metal-based materials, such as metal powders or metal fibers of copper, nickel, aluminum, silver, etc.; conductive polymers, such as polyphenylene derivatives; or mixtures thereof. The present application has no particular restrictions on the mass ratio of the positive electrode material, conductive agent, and positive electrode binder in the positive electrode mixture layer. Those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved. For example, the loading amount of the positive electrode material in the positive electrode sheet is 4.0 mg / cm 2 Up to 10.0mg / cm 2 .

[0080] The secondary battery of the present application also includes a separator. The material and shape of the separator used in the secondary battery of the present application are not particularly limited, and it can be any technology disclosed in the prior art. In some embodiments, the separator includes a polymer or inorganic substance formed of a material that is stable to the electrolyte of the present application.

[0081] For example, the isolation film may include a substrate layer and a surface treatment layer. The substrate layer is a non-woven fabric, a film or a composite film having a porous structure, and the material of the substrate layer is selected from at least one of polyethylene, polypropylene, polyethylene terephthalate and polyimide. Specifically, a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite film may be selected.

[0082] A surface treatment layer is provided on at least one surface of the substrate layer, and the surface treatment layer can be a polymer layer or an inorganic layer, or a layer formed by a mixed polymer and an inorganic substance. The inorganic layer includes inorganic particles and a binder, and the inorganic particles are selected from at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide and barium sulfate. The binder is selected from at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride-hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyethylene alkoxy, polymethyl methacrylate, polytetrafluoroethylene and polyhexafluoropropylene. The polymer layer contains a polymer, and the material of the polymer is selected from at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyethylene alkoxy, polyvinylidene fluoride and poly (vinylidene fluoride-hexafluoropropylene).

[0083] The secondary battery of the present application also includes a packaging bag for containing a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, as well as other components known in the art in the secondary battery, and the present application does not limit the above other components. The present application does not specifically limit the packaging bag, and it can be a packaging bag known in the art, as long as it can achieve the purpose of the present application.

[0084] The preparation process of the secondary battery of the present application is well known to those skilled in the art, and the present application has no special restrictions. For example, it may include but is not limited to the following steps: stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and winding, folding and other operations as needed to obtain an electrode assembly of a winding structure, placing the electrode assembly in a packaging bag, injecting the electrolyte into the packaging bag and sealing it to obtain a secondary battery; or stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and then fixing the four corners of the entire stacked structure with tape to obtain an electrode assembly of a stacked structure, placing the electrode assembly in a packaging bag, injecting the electrolyte into the packaging bag and sealing it to obtain a secondary battery. In addition, overcurrent protection elements, guide plates, etc. may also be placed in the packaging bag as needed to prevent the pressure inside the secondary battery from rising and overcharging and discharging.

[0085] In a third aspect, the present application provides an electronic device, comprising the secondary battery provided in the second aspect of the present application.

[0086] The electronic device of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. For example, the electronic device can include but is not limited to a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, a liquid crystal television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery, and a lithium-ion capacitor.

[0087] The scheme of the present application is described below in conjunction with the following specific examples. Unless otherwise specified, the raw materials used in the following examples are all from common commercial products, and the devices or equipment used are all purchased from conventional market sales channels. Various tests and evaluations are carried out according to the following methods. In addition, unless otherwise specified, "parts" and "%" are mass references.

[0088] Example 1-1

[0089] This embodiment provides a negative electrode active material, including a silicon-based material and an outer layer material; the outer layer material is located on at least a portion of the surface of the silicon-based material; the outer layer material includes multi-walled carbon nanotubes (conductive agent) and polyacrylonitrile (nitrile polymer).

[0090] Reference Figure 1 In the infrared spectrum of Example 1 shown in FIG. 1 , the infrared spectrum of the negative electrode active material includes the infrared characteristic peak of cyano group. Figure 2 From the local enlarged image, we can see that the infrared characteristic peak of cyano is located at 2340cm -1 Up to 2300cm -1 Between; the negative electrode active material includes nitrogen and silicon; based on the mass of the negative electrode active material, the mass content of the nitrogen element D1% is 1.11%, the mass content of the silicon element G% is 54.2%, wherein D1 / G=0.02.

[0091] In the negative electrode active material, the sphericity S=0.85, the thickness T nm of the outer layer material is 0.5 nm, and the average particle size R μm of the negative electrode active material is 5.3 μm.

[0092] The negative electrode active material of this embodiment is prepared by a method comprising the following steps:

[0093] S1: Provide silicon-carbon material; the silicon-based material includes a porous carbon skeleton and a silicon material; the silicon material is located on the surface and inside of the porous carbon skeleton.

[0094] S2: performing a first dispersion treatment on the multi-walled carbon nanotubes and polyacrylonitrile in a solvent for 4 hours to obtain a dispersion system; wherein the solvent comprises ethanol and butanol (in a mass ratio of 1:1).

[0095] S3: adding the silicon-carbon material in S1 to the dispersion system in S2 for a second dispersion treatment for 4 hours, and then drying the mixture at 200° C. for 4 hours to obtain the negative electrode active material of this embodiment.

[0096] Preparation of negative electrode: The negative electrode active material prepared above is used as the active material, acetylene black is used as the conductive agent, and sodium alginate is used as the binder. The mass ratio of active material, acetylene black, and sodium alginate is 70:20:10. The active material and acetylene black are fully mixed in proportion and ground evenly, and sodium alginate aqueous solution is added in proportion and stirred for 4 hours to obtain a negative electrode mixture slurry. Finally, the above slurry is evenly coated on the copper foil, and vacuum dried at 70°C for 12 hours. After cold pressing, the negative electrode is obtained, in which the loading amount of the active material is 1.2 mg / cm 2 The mass content of nitrogen in the negative electrode mixture layer is 0.77%, and the mass content of sodium is 1.6%.

[0097] Preparation of positive electrode: super-P is used as the conductive agent and PVDF is used as the binder, wherein the mass ratio of active material (LiFePO4), super-P and PVDF is 70:20:10. The active material and super-P are fully mixed in proportion and ground evenly, and the prepared 10wt.% PVDF solution is added in proportion and stirred for 4 hours to obtain the positive electrode mixture slurry. Finally, the positive electrode mixture slurry is evenly coated on aluminum foil, and vacuum dried at 70℃ for 12 hours, and the positive electrode is obtained after cold pressing. The loading amount of active material is 8mg / cm 2 .

[0098] Preparation of electrolyte: Using ethylene carbonate and dimethyl carbonate (EC and DMC, volume ratio of 1:1) as the base solvent, 1 mol / L LiPF6 was added to the base solvent to obtain the electrolyte.

[0099] Preparation of diaphragm: A 25 μm microporous single-layer polypropylene (PP) membrane was used as the diaphragm.

[0100] Preparation of secondary batteries: The negative electrode was cut into a circular electrode sheet with a diameter of 10 mm, and the lithium metal sheet and the circular electrode sheet were used as the counter electrode to assemble into a button-type half-cell in a glove box.

[0101] Alternatively, the positive electrode, separator, and negative electrode are stacked in order, with the separator placed between the positive electrode and the negative electrode to play an isolating role, and wound to obtain a bare cell. The bare cell is placed in an outer package, injected with electrolyte, packaged, and subjected to formation, degassing, trimming, and other process flows to obtain a lithium-ion battery.

[0102] Test method:

[0103] Gram capacity test of negative electrode active materials

[0104] The button half-cell was placed on a blue electricity tester for testing. The test process was as follows: the first step was to discharge at 0.05C to 0V, the second step was to stand for 5 minutes, the third step was to discharge at 50μA to 0V, the fourth step was to stand for 5 minutes, the fifth step was to discharge at 20μA to 0V, the sixth step was to stand for 5 minutes, the seventh step was to charge at 0.1C to 2V, the eighth step was to stand for 5 minutes, and the first to eighth steps were cycled twice. Then, the voltage was discharged at 1C to 0V, the voltage was stood for 5 minutes, and the voltage was charged at 0.1C to 2V, and the test was completed. The cumulative capacity of the first, third, and fifth steps of the first cycle is the discharge capacity, and the charging capacity is obtained by charging to 2.0V at 0.1C. The gram capacity of the negative electrode active material can be obtained by dividing the charging capacity by the weight of the negative electrode active material, and the first coulomb efficiency can be obtained by dividing the charging capacity by the discharge capacity.

[0105] Cycle capacity retention rate and cycle expansion rate test:

[0106] The lithium-ion battery was placed in a constant temperature box at 25℃±1℃ for 30 minutes, charged to 4.35V at 0.5C constant current, then charged to 0.025C at 4.35V constant voltage, placed for 5 minutes, and then discharged to 3.0V at 0.5C. This is a charge and discharge cycle process. The first cycle discharge capacity C0 and initial thickness H of the lithium-ion battery were recorded. 10 After that, the above cycle process was repeated for 600 cycles. The discharge capacity C1 at the 600th cycle and the thickness H after the cycle were recorded. 11 .

[0107] 600 cycle capacity retention rate = C1 / C0×100%.

[0108] Cycle expansion ratio = (H 11 -H 10 ) / H 10 ×100%.

[0109] High temperature storage expansion rate test:

[0110] The lithium-ion battery was placed in a constant temperature box at 25℃±1℃ for 30 minutes, charged to 4.35V at a constant current of 0.5C, and then charged to 0.025C at a constant voltage of 4.35V. After being placed for 5 minutes, the initial thickness H of the lithium-ion battery was measured. 20 The thickness of the lithium-ion battery was measured after storage at 60°C for 21 days. 21 Storage expansion ratio = (H 21 -H 20) / H 20 ×100%.

[0111] The negative electrode active materials of the following examples and comparative examples differ from those of Example 1-1 only in that the mass content of silicon and / or nitrogen in the negative electrode active materials, sphericity, thickness of the outer layer material and average particle size are adjusted according to Table 1, wherein only the addition amount of the silicon-based material, nitrile polymer and conductive agent is changed accordingly when the element content is adjusted. The addition amount of nitrogen in the negative electrode active material of Comparative Example 1-1 is 0, but the nitrile polymer of medium mass in Example 1-1 is added to the negative electrode mixture slurry to ensure that the mass proportion of the nitrile polymer in the negative electrode sheets of Comparative Example 1-1 and Example 1-1 is the same.

[0112] Table 1

[0113]

[0114] As can be seen from Table 1, the negative electrode active material of the present application forms an outer layer material composed of a conductive agent and a nitrile polymer on the surface of a silicon-based material, wherein the mass content of nitrogen based on the negative electrode active material is D1%, and the mass content of silicon is G%. When 0.02≤D1 / G≤0.5 is controlled, the cycle capacity retention rate, expansion inhibition performance and high-temperature storage performance of the secondary battery can be improved. Preferably, when 0.04≤D1 / G≤0.37 is satisfied, the cycle capacity retention rate, expansion inhibition performance and high-temperature storage performance of the secondary battery can be further improved. More preferably, when 0.06≤D1 / G≤0.19 is satisfied, the secondary battery has a more excellent cycle capacity retention rate, expansion inhibition performance and high-temperature storage performance.

[0115] In particular, when the conditions of 1.1≤D1≤18.4 are satisfied, especially when the conditions of 2.3≤D1≤9.2 are satisfied, the secondary battery exhibits higher cycle performance and high temperature performance. When the conditions of 36.8≤G≤68.3 are satisfied, especially when the conditions of 43.2≤G≤51.3 are satisfied, the silicon element can better cooperate with the nitrogen element to improve the expansion suppression performance and cycle performance of the secondary battery.

[0116] In particular, regulating the sphericity S of the negative electrode active material to meet 0.8≤S≤1.0 can improve the expansion inhibition performance, cycle performance and high-temperature storage performance of the secondary battery. When the sphericity is further increased to 0.9≤S≤1.0, the secondary battery can have higher expansion inhibition performance, cycle performance and high-temperature storage performance. In particular, regulating the thickness T nm of the outer layer material to meet 0.5≤T≤200.0 can optimize the expansion inhibition performance, cycle performance and high-temperature storage performance of the secondary battery. In particular, when the thickness T of the outer layer material is regulated to meet 0.5≤T≤100.0, the expansion inhibition performance, cycle performance and high-temperature storage performance of the secondary battery can be more significantly improved.

[0117] In particular, when the negative electrode active material satisfies 0.5≤S×T≤90.0, the first coulombic efficiency, expansion inhibition performance, high temperature storage performance and cycle performance of the secondary battery can be improved. Preferably, when 10.4≤S×T≤67.8 is satisfied, the expansion inhibition performance, high temperature storage performance and cycle performance of the secondary battery can be further improved. In particular, when the average particle size Rμm of the negative electrode active material is controlled within the range of 5.6≤R≤10.3, the secondary battery can have higher cycle performance, expansion inhibition performance and high temperature storage performance.

[0118] The secondary batteries of the following embodiments differ from those of Embodiment 1-1 only in that: the mass content of nitrogen and / or sodium in the negative electrode mixture layer is adjusted according to Table 2 (wherein the mass content of nitrogen and sodium in the negative electrode mixture layer is controlled by adjusting the type of negative electrode active material according to Table 2, and by controlling the ratio of the negative electrode active material to sodium alginate, with the remainder being multi-walled carbon nanotubes), and / or the mass content of fluorobenzene and / or fluoroethylene carbonate in the electrolyte is controlled (the control method is to add a corresponding mass of fluorobenzene and / or fluoroethylene carbonate to the base solvent).

[0119] Table 2

[0120]

[0121] As shown in Table 2, controlling the mass content D2% of nitrogen in the negative electrode mixture layer and the mass content N% of sodium to satisfy 2.35≤D2 / N≤11.74 can improve the cycle performance and suppress the expansion performance of the secondary battery. In particular, under the condition of 4.81≤D2 / N≤9.63, the cycle performance and suppress the expansion performance of the secondary battery can be further improved.

[0122] In particular, regulating the content of sodium in the negative electrode mixture layer within the range of 0.58≤N≤1.74 is beneficial to the cycle performance and high-temperature storage performance of the secondary battery. In particular, when 0.81≤N≤1.04, the secondary battery exhibits more excellent cycle performance and high-temperature storage performance. In particular, when the secondary battery satisfies 1.6≤D2≤8.1, its cycle performance and expansion inhibition performance can be improved, especially 5.0≤D2≤7.8, the cycle performance and expansion inhibition performance of the secondary battery are significantly improved.

[0123] In particular, adding fluorobenzene and / or fluoroethylene carbonate to the electrolyte in combination with the negative electrode system of the present application can optimize the high-temperature storage performance of the secondary battery, and can improve its first coulombic efficiency, cycle performance and expansion inhibition performance. Preferably, when the mass content F1% of fluorobenzene in the electrolyte is regulated to meet 0.9≤F1≤5.2, the high-temperature storage performance, cycle performance and expansion inhibition performance of the secondary battery can be further optimized; preferably, when 2.1≤F1≤3.1, the high-temperature storage performance, cycle performance and expansion inhibition performance of the secondary battery can be significantly improved.

[0124] In particular, by adjusting the mass content F2% of fluoroethylene carbonate in the electrolyte to meet 3.8≤F2≤7.4, the secondary battery can achieve more excellent high-temperature storage performance, cycle performance and expansion inhibition performance. In particular, when the electrolyte contains both fluorobenzene and fluoroethylene carbonate and meets the above preferred range, the secondary battery has extremely excellent high-temperature storage performance, cycle performance and expansion inhibition performance.

[0125] The above are only preferred embodiments of the present application and are not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the principles of the present application should be included in the protection scope of the present application.

Claims

1. A negative electrode active material, characterized in that: It comprises a silicon-based material and an outer layer material; the outer layer material is located on at least a portion of the surface of the silicon-based material; the outer layer material comprises a conductive agent and a nitrile polymer; The infrared spectrum of the negative electrode active material includes an infrared characteristic peak of cyano, and the infrared characteristic peak of cyano is located at 2250cm -1 Up to 2400cm -1 between; The negative electrode active material includes nitrogen and silicon. Based on the mass of the negative electrode active material, the mass content of the nitrogen is D1%, the mass content of the silicon is G%, and 0.02≤D1 / G≤0.

5.

2. The negative electrode active material according to claim 1, characterized in that The negative electrode active material satisfies at least one of the following conditions: (1)1.1≤D1≤18.4; (2)36.8≤G≤68.3; (3)0.04≤D1 / G≤0.

37.

3. The negative electrode active material according to claim 2, characterized in that: The negative electrode active material satisfies at least one of the following conditions: (1)2.3≤D1≤9.2; (2)43.2≤G≤51.3; (3)0.06≤D1 / G≤0.

19.

4. The negative electrode active material according to any one of claims 1 to 3, characterized in that The sphericity of the negative electrode active material is S, 0.8≤S≤1.0; and / or, In the negative electrode active material, the thickness of the outer layer material is T nm, 0.5≤T≤200.

0.

5. The negative electrode active material according to claim 4, characterized in that The negative electrode active material satisfies at least one of the following conditions: (1)0.9≤S≤1.0; (2)0.5≤T≤100.0; (3) 0.5≤S×T≤90.0; preferably, 10.4≤S×T≤67.8; (4) The average particle size of the negative electrode active material is R μm; 5.6≤R≤10.3。 6. The negative electrode active material according to any one of claims 1 to 3, characterized in that The negative electrode active material satisfies at least one of the following conditions: (1) The conductive agent comprises single-walled carbon nanotubes and / or multi-walled carbon nanotubes; (2) the nitrile polymer comprises at least one of polyacrylonitrile, polycyanoacrylate and polycyanobenzene; (3) The silicon-based material includes a porous carbon skeleton and a silicon material; the silicon material is located on the surface and / or inside of the porous carbon skeleton.

7. A secondary battery, characterized in that: including a positive electrode, a negative electrode and an electrolyte; The negative electrode comprises a negative electrode current collector and a negative electrode mixture layer disposed on at least a portion of the surface of the negative electrode current collector, wherein the negative electrode mixture layer comprises the negative electrode active material according to any one of claims 1 to 6.

8. The secondary battery according to claim 7, characterized in that: The negative electrode mixture layer includes sodium element, based on the mass of the negative electrode mixture layer, the mass content of the nitrogen element is D2%, and the mass content of the sodium element is N%; The negative electrode mixture layer satisfies at least one of the following conditions: (1) 0.58≤N≤1.74; preferably, 0.81≤N≤1.04; (2) 1.6≤D2≤8.1; preferably, 5.0≤D2≤7.8; (3) 2.35≤D2 / N≤11.74; preferably, 4.81≤D2 / N≤9.63; (4) The sodium element comes from at least one of sodium alginate, sodium carboxymethyl cellulose, sodium hydroxymethyl cellulose or sodium hydroxyethyl carboxymethyl cellulose.

9. The secondary battery according to claim 7, wherein the electrolyte comprises at least one of fluorobenzene or fluoroethylene carbonate; based on the mass of the electrolyte, the electrolyte satisfies at least one of the following conditions: (1) The mass content of fluorobenzene is F1%, 0.9≤F1≤5.2; preferably, 2.1≤F1≤3.1; (2) The mass content of the fluoroethylene carbonate is F2%, 3.8≤F2≤7.

4.

10. An electronic device, characterized in that: A secondary battery comprising the secondary battery according to any one of claims 7 to 9.

Citation Information

Patent Citations

  • Negative electrode active material and secondary battery

    CN112310356A

  • Secondary battery and device

    CN116454393A

  • Negative active material, secondary battery and electronic device

    CN117174888A

  • Negative pole piece, secondary battery and electronic device

    CN117393696A

  • Secondary battery and electronic device

    CN118173860A

Cited By

  • Negative electrode active material, secondary battery, and electronic device

    WO2026020770A1

  • Secondary battery and electronic device

    WO2026156807A1