Composite material and preparation method thereof, electrode, secondary battery and electric device

By using a composite material of bridged dielectric material particles and binder in lithium-ion batteries, the lithium desalination and short circuit problems caused by lithium dendrites are solved, the energy density and cycling performance of the battery are improved, and the longer battery is achieved Lifespan and higher charging efficiency.

CN118943342AActive Publication Date: 2024-11-12CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411294608.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-07-11
Publication Date
2024-11-12
Estimated Expiration
2042-07-11

AI Technical Summary

Technical Problem

The formation of lithium dendrites in lithium-ion batteries leads to higher conductivity than the negative electrode sheet, resulting in lithium ions aggregation, causing problems such as lithium-ion excretion, micro-short circuit, self-discharge, leakage current and short circuit, affecting the energy density and cycling performance of the battery.

Method used

A composite material is used, including negative electrode active material, dielectric material particles and binder. The surface of the dielectric material particles is covered with a coupling agent, and the dielectric material particles and binder are bridged through coupling agent to form a composite material. In the negative electrode of the secondary battery, the dielectric material particles can be evenly dispersed in the electrode slurry, reducing the solvation difference between lithium ions at the SEI membrane interface, reducing lithium ion enrichment, reducing electrolyte consumption, and improving fast charging performance.

Benefits of technology

It improves the specific capacity of the secondary battery, the first week of Coulomb efficiency, improves the fast charging cycle life, reduces the charging resistance, and extends the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943342A_ABST
    Figure CN118943342A_ABST
Patent Text Reader

Abstract

The invention provides a composite material. The composite material comprises a negative electrode active material, dielectric material particles and binder resin, at least a part of the surface of the dielectric material particles is coated with a coupling agent, and the coupling agent bridges the dielectric material particles and the binder resin.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent application with application number 202280005932.8, application date July 11, 2022, and invention name “Composite materials and preparation methods thereof, electrodes, secondary batteries and electrical devices”. Technical Field

[0002] The present application relates to the field of battery technology, and in particular to a composite material and a preparation method thereof, an electrode, a secondary battery and an electrical device. Background Art

[0003] In recent years, as the application scope of secondary batteries becomes wider and wider, secondary batteries are widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. As secondary batteries have made great progress, higher requirements have been put forward for their energy density, cycle performance, etc.

[0004] During the operation of lithium-ion batteries, there is a risk of lithium dendrites forming at the negative electrode. Since the conductivity of lithium dendrites is much higher than that of the negative electrode, lithium ions will preferentially gather at the end of lithium dendrites, causing macroscopic lithium deposition. Macroscopic lithium deposition will bypass the diaphragm and form a micro short circuit with the positive electrode, causing problems such as storage, self-discharge, leakage current, and even piercing the diaphragm, leading to serious problems such as short circuit. Summary of the invention

[0005] In view of the above problems, the present application provides a novel composite material and a preparation method thereof, an electrode, a secondary battery and an electrical device, which are described below respectively.

[0006] In a first aspect, the present application provides a composite material, comprising:

[0007] Negative electrode active material;

[0008] Dielectric material particles; and

[0009] Binder;

[0010] Wherein, at least a portion of the surface of the dielectric material particles is covered with a coupling agent, and the coupling agent bridges the dielectric material particles and the binder.

[0011] The dielectric material particles in the composite material of the present application are bridged to the binder resin through a coupling agent, which can bring the following beneficial effects:

[0012] (1) The dielectric material particles are evenly dispersed in the electrode slurry and will not all settle at the bottom of the slurry;

[0013] (2) The dielectric material particles can be bonded to the surface of the negative electrode active material through the binder, and the distance between the dielectric material particles and the surface of the negative electrode active material is relatively close, so as to give full play to the modification effect;

[0014] Taking lithium-ion batteries as an example, during the rapid charging process, the negative electrode active materials of lithium-ion batteries are embedded with lithium ions, and the difference in the desolvation rate of solvated lithium at the SEI membrane interface will lead to a wide concentration gradient distribution. The lithium ion enrichment at the interface between the SEI membrane and the negative electrode will lead to excessive local lithium content. When the lithium ion enrichment exceeds the lithium ion embedding amount, the lithium ions will combine with electrons to cause lithium dendrites in the local negative electrode. Since the conductivity of lithium dendrites is much higher than that of the negative electrode sheet, the subsequent lithium ions will preferentially gather at the end of the lithium dendrite, and then cause macroscopic lithium precipitation. These lithium precipitations will bypass the diaphragm and form a micro short circuit with the positive electrode, causing problems such as storage, self-discharge, leakage current, and even pierce the diaphragm, leading to serious problems such as short circuit. High dielectric constant materials have a dielectric constant similar to that of the electrolyte, which is beneficial to reducing the desolvation barrier, improving the desolvation level of lithium, and improving fast charging performance. This material is affected by the electric field and will produce a reverse electric field. The thin SEI film produced at the three-phase interface of the dielectric constant material, graphite or silicon, and solvent reduces the loss of active lithium and shortens the migration path of lithium ions in the SEI film, thereby improving fast charging performance and reducing electrolyte consumption.

[0015] The composite material of the present application is used for the negative electrode of a secondary battery, and the secondary battery can exhibit one or more of the following improved properties: improved specific capacity, improved first-cycle coulomb efficiency, and improved fast-charging cycle life.

[0016] (3) The volume of the negative electrode active material will expand / contract during the charge and discharge process. During this process, since the dielectric material particles are bridged on the binder resin, the dielectric material particles will not fall off as the negative electrode active material expands / contracts, and will not lose contact with the negative electrode active material. The dielectric material particles can maintain stable contact with the negative electrode active material during the operation of the battery, and can thus stably play a modifying role.

[0017] In some embodiments, the binder binds the dielectric material particles to the negative electrode active material.

[0018] In some embodiments, the relative dielectric constant of the dielectric material particles is 80 to 200. Based on this solution, the relative dielectric constants of the dielectric material particles and the electrolyte are relatively close, and the fast charging performance is better.

[0019] In some embodiments, the dielectric material is selected from one or more of the following: barium titanate, lead titanate, lithium niobate, lead zirconate titanate, lead metaniobate, and lithium barium lead niobate.

[0020] In some embodiments, the binder is an organic binder.

[0021] In some embodiments, the binder is selected from one or more of the following: polyacrylic acid (PAA), styrene-butadiene rubber (SBR), polyamide-imide (PAI), polyvinyl alcohol (PVA), polyethyleneimine (PEI), polyimide binder (PI), polytert-butyl acrylate-triethoxyvinyl silane (TBATEVS).

[0022] In some embodiments, the coupling agent is selected from one or more of the following: a silane coupling agent, a titanate coupling agent.

[0023] In some embodiments, the coupling agent is selected from one or more of silane coupling agent KH590, silane coupling agent KH550, silane coupling agent KH560, silane coupling agent KH570, silane coupling agent KH792, silane coupling agent DL602, silane coupling agent DL171, chelate 100 type titanate coupling agent, and chelate 200 type titanate coupling agent.

[0024] In some embodiments, the coupling agent is connected to the dielectric material via a first terminal functional group, and the first terminal functional group includes -O-.

[0025] In some embodiments, the coupling agent is connected to the binder via a second terminal functional group, and the second terminal functional group includes -S-.

[0026] In some embodiments, the coupling agent is connected to the dielectric material via a first terminal functional group, and the first terminal functional group includes -Si-O-.

[0027] In some embodiments, the coupling agent is connected to the binder via a second terminal functional group, and the second terminal functional group includes -CS-.

[0028] In some embodiments, the binder has a number average molecular weight of 1 million to 2 million.

[0029] In some embodiments, the dielectric material particles are zero-dimensional particles.

[0030] In some embodiments, the dielectric material particles are tetragonal barium titanate particles.

[0031] In some embodiments, the volume median particle size of the dielectric material particles is 50 nm to 200 nm. Based on this, the dielectric material particles can be well combined with the negative electrode active material, and the dielectric material particles are not easy to fall off from the surface of the negative electrode active material.

[0032] In some embodiments, the volume median particle size of the negative electrode active material is 4-10 μm. Based on this, the dielectric material can be well attached to the surface of the negative electrode active material and is not easy to fall off.

[0033] In some embodiments, the ratio of the volume median particle size of the negative electrode active material to the volume median particle size of the dielectric material particles is 200: 1 to 20: 1. Based on this, the dielectric material is easily attached to the surface of the negative electrode active material and is not easy to fall off.

[0034] In some embodiments, the mass ratio of the dielectric material to the binder is 0.1:100 to 1:100.

[0035] In a second aspect, the present application provides a method for preparing a composite material, wherein the composite material is the composite material described in any one of the above items;

[0036] The preparation method comprises:

[0037] (1) performing a hydroxylation treatment on the dielectric material particles to obtain hydroxylated dielectric material particles;

[0038] (2) grafting a coupling agent onto the hydroxylated dielectric material particles to obtain dielectric material particles grafted with the coupling agent;

[0039] (3) connecting the coupling agent grafted on the dielectric material particles with the binder through a condensation reaction;

[0040] (4) Mix the product from the previous step with the negative electrode active material.

[0041] In some embodiments, in step (3), the coupling agent on the dielectric material particles contains a thiol terminal group, the binder contains an alkenyl terminal group, and the coupling agent and the binder are connected via a thiol-alkenyl click chemistry reaction.

[0042] In some embodiments, the thiol-alkenyl click chemistry reaction is carried out under the action of a photoinitiator and ultraviolet light.

[0043] In a third aspect, an electrode is provided, comprising any of the composite materials described above.

[0044] In a fourth aspect, the present application provides a secondary battery comprising any of the electrodes described above.

[0045] In a fifth aspect, the present application provides an electrical device, comprising the above-mentioned secondary battery.

[0046] Beneficial Effects

[0047] One or more embodiments of the present application have one or more of the following beneficial effects:

[0048] (1) The composite material is used for secondary battery electrodes, and the secondary battery exhibits improved negative electrode capacity;

[0049] (2) The composite material is used for secondary battery electrodes, and the secondary battery exhibits improved first-cycle coulombic efficiency;

[0050] (3) The composite material is used for secondary battery electrodes, and the secondary battery exhibits reduced charging resistance;

[0051] (4) The composite material is used for secondary battery electrodes, and the secondary battery exhibits a longer cycle life. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 It is a schematic diagram of a styrene-butadiene rubber-barium titanate particle composite according to one embodiment of the present application.

[0053] Figure 2 It is an infrared spectrum diagram of the styrene-butadiene rubber-barium titanate particle composite, styrene-butadiene rubber, and barium titanate particles according to one embodiment of the present application.

[0054] Figure 3 is a schematic diagram of a composite material according to one embodiment of the present application.

[0055] Figure 4 It is a schematic diagram of an adhesion test according to an embodiment of the present application.

[0056] Figure 5 is a schematic diagram of a secondary battery according to one embodiment of the present application.

[0057] Figure 6 yes Figure 5 An exploded view of a secondary battery according to an embodiment of the present application is shown.

[0058] Figure 7 is a schematic diagram of a battery module according to an embodiment of the present application.

[0059] Figure 8 It is a schematic diagram of a battery pack according to one embodiment of the present application.

[0060] Fig. 9 yes Figure 8 An exploded view of a battery pack according to an embodiment of the present application is shown.

[0061] Fig.10 FIG. 1 is a schematic diagram of an electric device using a secondary battery according to an embodiment of the present application as a power source.

[0062] Description of reference numerals:

[0063] 1 battery pack; 2 upper box; 3 lower box; 4 battery module; 5 secondary battery; 51 shell; 52 electrode assembly; 53 top cover assembly; 100 negative electrode active material; 101 dielectric material particles; 103 binder; 510 steel plate; 520 double-sided adhesive; 530 pole piece to be tested DETAILED DESCRIPTION

[0064] Below, the negative electrode active material and its manufacturing method, positive electrode sheet, negative electrode sheet, secondary battery, battery module, battery pack and embodiment of the device of the present application are specifically disclosed with appropriate reference to the drawings. However, there are cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0065] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0066] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0067] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0068] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0069] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0070] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0071] [Secondary battery]

[0072] Secondary batteries, also known as rechargeable batteries or storage batteries, refer to batteries that can continue to be used by recharging the active materials after the battery is discharged.

[0073] Normally, a secondary battery includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. During the battery charging and discharging process, active ions (such as lithium ions) are embedded and removed back and forth between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing active ions to pass through. The electrolyte is between the positive electrode sheet and the negative electrode sheet, mainly to conduct active ions.

[0074] [Composite Materials]

[0075] In a first aspect, the present application provides a composite material, comprising:

[0076] Negative electrode active material;

[0077] Dielectric material particles; and

[0078] Binder;

[0079] Wherein, at least a portion of the surface of the dielectric material particles is covered with a coupling agent, and the coupling agent bridges the dielectric material particles and the binder.

[0080] The dielectric material particles in the composite material of the present application are bridged to the binder resin through a coupling agent, which can bring the following beneficial effects:

[0081] (1) The dielectric material particles are evenly dispersed in the electrode slurry and will not all settle at the bottom of the slurry;

[0082] (2) The dielectric material particles can be bonded to the surface of the negative electrode active material through the binder, and the distance between the dielectric material particles and the surface of the negative electrode active material is relatively close, so as to give full play to the modification effect;

[0083] (3) The volume of the negative electrode active material will expand / contract during the charge and discharge process. During this process, since the dielectric material particles are bridged on the binder resin, the dielectric material particles will not fall off as the negative electrode active material expands / contracts, and will not lose contact with the negative electrode active material. The dielectric material particles can maintain stable contact with the negative electrode active material during the operation of the battery, and can thus stably play a modifying role.

[0084] In some embodiments, the term "bridging" means that one end of the coupling agent is connected to the dielectric material particle, and the other end is connected to the binder through a chemical bond.

[0085] In some embodiments, the term "linked" refers to linked by a chemical bond, such as an ionic bond or a covalent bond.

[0086] In some embodiments, the coupling agent is bonded to the dielectric material particles via chemical bonds.

[0087] In some embodiments, the coupling agent is bonded to the binder via a chemical bond.

[0088] The term "coupling agent" refers to a substance that can be connected to both dielectric materials and binders. A "coupling agent" can have two functional groups of different properties, such as one that is an inorganic-philic functional group that is easy to chemically react with the surface of inorganic substances; and the other that is an organic-philic agent that can chemically react, physically entangle, or form hydrogen bonds with synthetic resins or other polymers and dissolve therein.

[0089] In some embodiments, the binder binds the dielectric material particles to the negative electrode active material.

[0090] In some embodiments, the dielectric material particles have a relative dielectric constant of 80 to 200 (eg, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, or 200).

[0091] In some embodiments, the dielectric material is selected from one or more of the following: barium titanate, lead titanate, lithium niobate, lead zirconate titanate, lead metaniobate, and lithium barium lead niobate.

[0092] In some embodiments, the chemical formula of lead zirconate titanate is Pb x Zr 1-x TiO3, 0<x<1.

[0093] In some embodiments, the chemical formula of lead barium lithium niobate is (Pb x Ba 1-x )4Li2Nb 10 O 30 , 0<x<1.

[0094] In some embodiments, the binder is an organic binder.

[0095] In some embodiments, the binder has one or more (e.g., one, two, or three) monomer units selected from Formula 1, Formula 2, and Formula 3;

[0096]

[0097]

[0098] In some embodiments, the binder is selected from one or more of the following: polyacrylic acid (PAA), styrene-butadiene rubber (SBR), polyamide-imide (PAI), polyvinyl alcohol (PVA), polyethyleneimine (PEI), polyimide binder (PI), polytert-butyl acrylate-triethoxyvinyl silane (TBATEVS).

[0099] In some embodiments, the coupling agent is selected from one or more of the following: a silane coupling agent, a titanate coupling agent.

[0100] In some embodiments, the coupling agent is selected from one or more of silane coupling agent KH590, silane coupling agent KH550, silane coupling agent KH560, silane coupling agent KH570, silane coupling agent KH792, silane coupling agent DL602, silane coupling agent DL171, chelate 100 type titanate coupling agent, and chelate 200 type titanate coupling agent.

[0101] In some embodiments, the coupling agent is a silane coupling agent of the general formula RSiX3, wherein R represents amino, thiol, vinyl, epoxy, cyano and methacryloxy groups, and these groups have strong reactivity with different base resins, and X represents an alkoxy group (such as methoxy, ethoxy, etc.) that can be hydrolyzed. The silane coupling agent is one or more of KH550, KH560, KH590, KH570, KH792, DL602, and DL171.

[0102] In some embodiments, the coupling agent is a chelated titanate coupling agent. Specifically, it can be one or more of chelated 100 type and 200 type. Chelated 100 type is a titanate coupling agent containing an oxyacetic acid chelate group, and chelated 200 type is a titanate coupling agent containing an ethylene glycol chelate. Chelated 100 type titanate coupling agent is, for example, di(octyl pyrophosphate)hydroxyacetic acid titanate CTDPP-138S (KR-138S). Chelated 200 type titanate coupling agent is, for example, di(dioctyl phosphate)ethylene glycol titanate ETDOP-212S (KR-212S).

[0103] In some embodiments, the coupling agent is selected from one or more of silane coupling agent KH590, silane coupling agent KH550, silane coupling agent KH560, silane coupling agent KH570, silane coupling agent KH792, silane coupling agent DL602, silane coupling agent DL171, chelate 100 type titanate coupling agent, and chelate 200 type titanate coupling agent.

[0104] In some embodiments, the coupling agent is connected to the dielectric material via a first terminal functional group, and the first terminal functional group includes -O-.

[0105] In some embodiments, the coupling agent is connected to the binder via a second terminal functional group, and the second terminal functional group includes -S-.

[0106] In some embodiments, the coupling agent is connected to the dielectric material via a first terminal functional group, and the first terminal functional group includes -Si-O-.

[0107] In some embodiments, the coupling agent is connected to the binder via a second terminal functional group, and the second terminal functional group includes -CS-.

[0108] In some embodiments, the binder has a number average molecular weight of 1 million to 2 million, such as 1.3 million to 1.7 million, such as 1.5 million.

[0109] In some embodiments, the term "number average molecular weight" refers to the common arithmetic mean of the molecular weights of the individual polymers.

[0110] In some embodiments, the dielectric material particles are zero-dimensional particles. Zero-dimensional materials refer to point-shaped materials that are in the nanoscale range (1-100 nm, such as 1-50 nm, such as 1-10 nm) in three dimensions.

[0111] In some embodiments, the dielectric material particles are tetragonal barium titanate particles.

[0112] In some embodiments, the volume median particle size of the dielectric material particles is 50nm-200nm, such as 50nm-100nm, 100nm-150nm, 150nm-200nm. The advantage of the volume median particle size of the dielectric material particles being in the above range is that they are easily mixed with negative electrode active materials such as graphite and are not easily detached from the graphite surface.

[0113] In some embodiments, the term "volume median particle size" Dv50 refers to the particle size corresponding to 50% of the volume in terms of the cumulative particle distribution sorted from the smallest size to the largest size. The "volume median particle size" can be observed and measured using a scanning electron microscope, or can be measured using a laser diffraction method.

[0114] In some embodiments, the volume median particle size of the negative electrode active material is 4 to 10 μm.

[0115] In some embodiments, the ratio of the volume median particle size of the negative electrode active material to the dielectric material particles is 200: 1 to 20: 1, for example, 200: 1 to 150: 1, 150: 1 to 100: 1, 100: 1 to 50: 1, 50: 1 to 20: 1. The advantage of the ratio of the volume median particle size of the negative electrode active material to the dielectric material particles being within the above range is that the dielectric material is easily attached to the graphite surface and is not easy to fall off.

[0116] In some embodiments, the mass ratio of the dielectric material to the binder is 0.1:100 to 1:100 (e.g., 0.1:100-0.2:100, 0.2:100-0.3:100, 0.3:100-0.4:100, 0.4:100-0.5:100, 0.5:100-0.6:100, 0.6:100-0.7:100, 0.7:100-0.8:100, 0.8:100-0.9:100, 0.9:100-1:100).

[0117] In some embodiments, the term "zero-dimensional" refers to a particle state in which the particle size is extremely small and substantially has no length, such as a particle in a nanoparticle state. Compared to the term "zero-dimensional", the term "three-dimensional" refers to a large-volume state with volume, the term "two-dimensional" refers to a thin-film state, and the term "one-dimensional" refers to a nanotube state.

[0118] In some embodiments, the term "zero dimensional" may refer to particles having a diameter of 1 nm to about 100 nm (1-10 nm, 10-20 nm, 20-30 nm, 30-40 nm, 40-50 nm, 50-60 nm, 60-70 nm, 70-80 nm, 80-90 nm, 90-100 nm).

[0119] In some embodiments, the term "tetragonal" refers to a crystal structure having a unit cell comprising three axes, wherein two axes are the same length and are at right angles to each other, and the third axis is perpendicular to the other two axes.

[0120] In some embodiments, the term "relative dielectric constant" refers to the relative dielectric constant (ε r ), which is the relative permittivity of the material divided by the relative permittivity of a vacuum (ε0).

[0121] In some embodiments, the dielectric constant refers to the dielectric constant at room temperature (25±5°C), which has a well-known meaning in the art and can be tested using instruments and methods known in the art. For example, the ferroelectric material can be prepared into a circular sample, and the capacitance C can be tested using an LCR tester and calculated according to the formula: dielectric constant ε = (C×d) / (ε0×A). C represents capacitance, in farads (F); d represents sample thickness, in cm; A represents sample area, in cm 2 ; ε0 represents the vacuum dielectric constant, ε0 = 8.854×10-14F / cm. In this application, the test conditions may be 1KHz, 1.0V, 25±5°C. The test standard may be based on GB / T 11297.11-2015. When preparing the sample, reference may be made to Chinese patent application CN114217139A.

[0122] In some embodiments, the relative dielectric constant of the present application can be measured by a relative dielectric constant tester, specifically referring to GB / T5594.4-1985, and the instrument can be the ZJD-C relative dielectric constant tester of Beijing AVIC Times Instrument Equipment Co., Ltd.

[0123] In a second aspect, the present application provides a method for preparing a composite material, wherein the composite material is the composite material described in any one of the above items;

[0124] The preparation method comprises:

[0125] (1) performing a hydroxylation treatment on the dielectric material particles to obtain hydroxylated dielectric material particles;

[0126] (2) grafting a coupling agent onto the hydroxylated dielectric material particles to obtain dielectric material particles grafted with the coupling agent;

[0127] (3) connecting the coupling agent grafted on the dielectric material particles with the binder through a condensation reaction;

[0128] (4) Mix the product from the previous step with the negative electrode active material.

[0129] In some embodiments, in step (3), the coupling agent on the dielectric material particles contains a thiol terminal group, the binder contains an alkenyl terminal group, and the coupling agent and the binder are connected via a thiol-alkenyl click chemistry reaction.

[0130] In some embodiments, the thiol-alkenyl click chemistry reaction is carried out under the action of a photoinitiator and ultraviolet light.

[0131] In a third aspect, an electrode is provided, comprising any of the composite materials described above.

[0132] In a fourth aspect, the present application provides a secondary battery comprising any of the electrodes described above.

[0133] In a fifth aspect, the present application provides an electrical device, comprising the above-mentioned secondary battery.

[0134] [Negative electrode]

[0135] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material, and the negative electrode active material adopts any negative electrode active material of the present application.

[0136] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0137] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0138] In some embodiments, the negative electrode active material may adopt the negative electrode active material for the battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0139] In some embodiments, the negative electrode film layer may further include a binder. As an example, the binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).

[0140] In some embodiments, the negative electrode film layer may further include a conductive agent. As an example, the conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0141] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0142] In some embodiments, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0143] [Positive electrode]

[0144] In some embodiments, the positive electrode sheet generally includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, and the positive electrode film layer includes a positive electrode active material.

[0145] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.

[0146] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0147] In some embodiments, the positive electrode active material may adopt a positive electrode active material for a battery that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: a lithium-containing phosphate with an olivine structure, a lithium transition metal oxide, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 5 n 1 / 3 O2 (also referred to as NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 )、LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05O2) and its modified compounds, etc. Examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0148] In some embodiments, the positive electrode film layer may also optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.

[0149] In some embodiments, the positive electrode film layer may further include a conductive agent, for example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0150] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0151] [Electrolytes]

[0152] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be liquid, gel or all-solid.

[0153] In some embodiments, the electrolyte is liquid and includes an electrolyte salt and a solvent.

[0154] In some embodiments, the electrolyte salt can be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0155] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0156] In some embodiments, the electrolyte may further include additives. As examples, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.

[0157] [Isolation film]

[0158] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.

[0159] In some embodiments, the material of the isolation membrane can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0160] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.

[0161] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.

[0162] In some embodiments, the outer packaging of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0163] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 5 The secondary battery 5 is a square structure as an example.

[0164] In some embodiments, reference Figure 6, the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0165] In some embodiments, secondary batteries may be assembled into a battery module. The number of secondary batteries contained in the battery module may be one or more, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery module.

[0166] Figure 7 4 is an example of a battery module. Figure 7 In the battery module 4, the plurality of secondary batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of secondary batteries 5 may be fixed by fasteners.

[0167] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0168] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery pack.

[0169] Figure 8 and Fig. 9 1 is a battery pack 1 as an example. Figure 8 and Fig. 9 The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.

[0170] In addition, the present application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0171] As the electrical device, a secondary battery, a battery module or a battery pack may be selected according to its usage requirements.

[0172] Fig.10 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for the secondary battery, a battery pack or a battery module can be used.

[0173] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0174] Embodiment 1:

[0175] Take 100g of dielectric material particles (barium titanate particles, tetragonal crystal) and add them to 1L of H2O2 solution (H2O2 concentration is 3%), then add 50ml of ammonium chloride solution, heat and stir at 90°C reflux temperature for 3 hours to obtain hydroxyl-modified barium titanate particles.

[0176] Take 100g of hydroxyl-modified barium titanate particles and immerse them in an ethanol aqueous solution (the volume ratio of ethanol to water is 8:1), add 10ml of a coupling agent (γ-mercaptopropyltrimethoxysilane), heat to 50°C, react for 4h, and obtain barium titanate particles grafted with a coupling agent.

[0177] 200g of the binder (styrene-butadiene rubber, number average molecular weight 1.5 million) copolymer was dissolved in 1L of DMF, ultrasonically stirred, 10g of barium titanate particles grafted with a coupling agent were added, and then 9g of benzoin dimethyl ether were added to obtain a mixture. The above mixture was irradiated under an ultraviolet lamp with a wavelength of 360nm for 30min, and then heated at 30°C until the DMF volatilized to obtain a styrene-butadiene rubber-barium titanate particle composite.

[0178] In the styrene-butadiene rubber-barium titanate particle composite (SBR-BTO for short), at least a portion of the surface of the barium titanate particle is covered with γ-mercaptopropyltrimethoxysilane, and the γ-mercaptopropyltrimethoxysilane bridges the barium titanate particle and the styrene-butadiene rubber.

[0179] Figure 1 A schematic diagram of a styrene-butadiene rubber-barium titanate particle composite is shown. As shown in the figure, at least a portion of the surface of the dielectric material particle 101 is covered with a coupling agent 102 , and the coupling agent 102 bridges the dielectric material particle 101 and the binder 103 .

[0180] Figure 2 The infrared spectrum of barium titanate particles grafted with styrene-butadiene rubber (BTO-SBR) is shown. It can be seen from the figure that at wave numbers of 1200 and 1100 cm -1 The absorption peaks of Si-C and Si-O were observed at , which proved that γ-mercaptopropyltrimethoxysilane bridged the barium titanate particles and styrene-butadiene rubber together.

[0181] The negative electrode active material (artificial graphite), the conductive agent (acetylene black), the barium titanate particles grafted with styrene-butadiene rubber (referred to as SBR-BTO) and the dispersant (sodium carboxymethyl cellulose, referred to as CMC) were mixed in a weight ratio of 97:1:1:1 to obtain the composite material of Example 1. The composite material was subsequently used to prepare the negative electrode slurry of the lithium-ion battery. The ratio of the volume median particle size of the negative electrode active material to the dielectric material particles was controlled to be 50:1, that is, the volume average particle size of the negative electrode active material in Example 1 was 2.5 μm.

[0182] Figure 3 Schematic diagram of a composite material is shown, as shown in the figure, the composite material includes a negative electrode active material 100, dielectric material particles 101 and a binder 103, and the binder 103 binds the dielectric material particles 101 to the negative electrode active material 100. Figure 3 As shown, the above scheme of the present application prepares a composite material with a "chain ball structure". By connecting the binder 103 and the dielectric material particles 101 through the thiol group, the hydroxyl groups on the surface of the binder 103 can be connected to the surface of the negative electrode active material 100 through hydrogen bonds, so that the dielectric material particles 101 can be evenly distributed on the surface of the negative electrode active material 100. At the same time, this composite material is connected point to surface at the negative end, which improves the utilization rate of high dielectric constant materials, can give full play to its desolvation effect and the performance of thin SEI, and will not block the migration channel of lithium ions. It should be particularly noted that Figure 3 The diagram shown is only for the convenience of presenting the connection relationship. Figure 3 The dimensional relationships shown in the drawings do not represent actual dimensional relationships.

[0183] Example 1 The ratio of the raw material components (artificial graphite, acetylene black, SBR-BTO, CMC) for preparing the composite material, the ratio of SBR to BTO in SBR-BTO, the volume median particle size Dv50 and relative dielectric constant of barium titanate, and the number average molecular weight of SBR are shown in Table 1.

[0184] Embodiments 2 to 15

[0185] The difference between Examples 2 to 15 and Example 1 is that the raw material parameters or process parameters for preparing the composite material are different. The specific parameter differences are shown in Table 1.

[0186] In Example 11, lead titanate (PTO) is used to replace the barium titanate (BTO) in Example 1.

[0187] In Example 12, lithium niobate (PPLN) is used to replace the barium titanate (BTO) in Example 1.

[0188] Example 13 uses lead zirconate titanate (PZT) to replace the barium titanate (BTO) in Example 1.

[0189] In Example 14, a chelate 100 type titanate coupling agent (CTDPP-138S) is used to bridge the dielectric material particles and the binder to replace the γ-mercaptopropyltrimethoxysilane in Example 1.

[0190] In Example 15, a chelated 200 type titanate coupling agent (ETDOP-212S) is used to bridge the dielectric material particles and the binder to replace the γ-mercaptopropyltrimethoxysilane in Example 1.

[0191] Comparative Example 1

[0192] The difference between Comparative Example 1 and Example 1 is that the composite material formula is different. The composite material of Comparative Example 1 does not contain dielectric material particles BTO. The formula of the composite material of Comparative Example 1 is as follows: negative electrode active material (artificial graphite), conductive agent (acetylene black), styrene-butadiene rubber and dispersant (sodium carboxymethyl cellulose) are mixed in a weight ratio of 97:1:1:1.

[0193] Comparative Example 2

[0194] The difference between Comparative Example 2 and Example 1 is that the composite material formula is different. The composite material of Comparative Example 2 does not contain dielectric material particles BTO. The composite material formula of Comparative Example 2 is as follows: negative electrode active material (artificial graphite), conductive agent (acetylene black), styrene-butadiene rubber, dielectric material particles (barium titanate particles) and dispersant (sodium carboxymethyl cellulose) are mixed according to a weight ratio of 97:1:0.95::0.05:1.

[0195] Preparation of full battery

[0196] (1) Preparation of negative electrode sheet: The composite materials of the above-mentioned embodiment and comparative example were added to deionized water respectively, stirred and mixed to prepare negative electrode slurry. The negative electrode slurry was coated on a 7μm negative electrode current collector copper foil, and then dried, cold pressed and cut to obtain a negative electrode sheet with a negative electrode film layer. The surface density of the negative electrode film layer was 9.7mg / cm 2 .

[0197] (2) Preparation of positive electrode sheet: positive electrode active material lithium nickel cobalt manganese oxide (NCM523, i.e. LiNi 0.5 Co 0.2 Mn 0.3 O2), polyvinylidene fluoride PVDF, and conductive agent acetylene black SP were mixed in a weight ratio of 98:1:1, N-methylpyrrolidone (NMP) was added as a solvent, and the slurry was stirred in a vacuum state until it was uniform. The obtained slurry was coated on a 13μm aluminum foil with a scraper, then dried at 140°C, cold pressed, and cut to obtain a positive electrode sheet with a positive electrode film layer. The surface density of the positive electrode film layer was 13.7mg / cm 2 .

[0198] (3) Electrolyte: In an argon atmosphere glove box (H2O<0.1ppm, O2<0.1ppm), organic solvents ethylene carbonate (EC) / ethyl methyl carbonate (EMC) were mixed in a volume ratio of 3:7, 12.5 wt% (based on the total weight of the ethylene carbonate / ethyl methyl carbonate solvent) of LiPF6 was added and dissolved in the organic solvent, and stirred to obtain an electrolyte. The relative dielectric constant of the electrolyte was 90.

[0199] (4) Isolation membrane: A commercially available PP-PE copolymer microporous film with a thickness of 20 μm and an average pore size of 80 nm (from Zhuogao Electronic Technology Co., Ltd., model 20) was used.

[0200] (5) Stack the positive electrode sheet, the separator, and the negative electrode sheet in order, so that the separator is between the positive and negative electrodes to play a role of isolation, and wind them to obtain a bare cell. Place the bare cell in an outer package, inject the above-mentioned electrolyte and package it to obtain a secondary battery.

[0201] Preparation of half-cell

[0202] It uses the same negative electrode and electrolyte as the full battery, and a lithium sheet as the counter electrode, assembled into a button-type half-cell.

[0203] Analysis and testing

[0204] 1. Pole piece adhesion test

[0205] The adhesion test was carried out using the peel test method. Figure 4 (a) to (d) show the flow chart of the peeling test. Figure 4As shown in (a), first provide a steel plate 510, the steel plate size is 30mm wide × 100mm long. Figure 4 As shown in (b), a double-sided adhesive tape 520 is provided, and the size of the double-sided adhesive tape 520 is 20 mm wide and 30 mm long. The double-sided adhesive tape 520 is attached to the steel plate 510, and one wide side of the double-sided adhesive tape 520 is aligned with one wide side of the steel plate 510. Figure 4 As shown in (c), a piece of electrode piece 530 to be tested is provided, and the size of the electrode piece 530 to be tested is 20 mm wide and 180 mm long. The electrode piece 530 to be tested is covered on the double-sided adhesive tape 520 (aligned on both sides), and the coated surface of the electrode piece 530 faces the double-sided adhesive tape 520. Since the length of the electrode piece 530 to be tested is greater than the length of the double-sided adhesive tape 520, part of the area of ​​the electrode piece 520 to be tested is not bonded to the double-sided adhesive tape. Figure 4 As shown in (d), the steel plate 510 is fixed on the base of the tensile testing machine, and the end of the electrode 530 to be tested that is not bonded to the double-sided tape is clamped with a clamp, and then the clamp is stretched in the direction of the other end (as shown by the arrow), and the direction of the stretching force is perpendicular to the steel plate 510 and there is a certain distance from the surface of the steel plate 510. While the electrode is stretched and peeled off outside the paper, the steel plate moves upward to keep the stretching direction perpendicular to the electrode peeling position. During the stretching process, the stretching causes the electrode 530 to be gradually peeled off from the steel plate. During the stretching process, the stretching speed of the clamp is 50mm / min. During the stretching process, the tension of the clamp is recorded, and after the tension stabilizes, the peeling length of 40mm is continued, and the average tension at the peeling length is taken as the bonding force (unit N).

[0206] 2. Negative electrode capacity (C)

[0207] At 2.5-4.3V, charge the button cell at 0.1C to 4.3V, then charge at 4.3V at a constant voltage until the current is less than or equal to 0.05mA, let stand for 5 minutes, and then discharge at 0.1C to 2.0V. The discharge capacity at this time is the initial gram capacity. Divide the initial gram capacity by the weight of the positive electrode active material to get the positive electrode gram capacity.

[0208] 3. Negative electrode first coulombic efficiency (ICE)

[0209] At 25°C and normal pressure, discharge the button cell at a constant current of 0.1C to a voltage of 0.005V, and then discharge at a constant current of 0.05C to a voltage of 0.005V, and record the discharge specific capacity at this time, which is the first lithium insertion capacity; then charge at a constant current of 0.1C to a voltage of 1.5V, and record the charge specific capacity at this time, which is the first lithium removal capacity. Perform 50 cycles of charge and discharge test on the button cell according to the above method, and record the lithium removal capacity each time.

[0210] First coulombic efficiency (%) = first lithium removal capacity / first lithium insertion capacity × 100%

[0211] 5. Charging resistance test

[0212] In this application, the kinetic performance of the secondary battery is evaluated by the 25°C 4C charging resistance. At 25°C, the lithium-ion batteries prepared in the examples and comparative examples are discharged to 50% capacity, left to stand for 30 minutes, and the voltage value V1 is recorded. The battery is charged for 10 seconds at a current A0 corresponding to a 4C rate, and the voltage value V2 corresponding to the end of charging is recorded. The charging resistance is calculated as follows: R = (V2-V1) / A0

[0213] The experimental results were normalized, with the charging resistor value of Example 2 being the reference value of 100, and the other examples were scaled accordingly.

[0214] 4. Fast charging cycle life / number of cycles

[0215] In this application, the capacity retention performance of the secondary battery is evaluated by the fast charge cycle life / number of cycles. At 25°C, the lithium-ion batteries prepared in the examples and comparative examples are charged at a 2C rate and discharged at a 1C rate, and a continuous cycle test is performed in the range of 3%-97% SOC until the capacity of the lithium-ion battery is less than 80% of the initial capacity, and the number of cycles is recorded.

[0216] 5. Relative dielectric constant test

[0217] In the present application, the relative dielectric constant of the dielectric material particles and the electrolyte can be measured by a dielectric constant tester, and specific reference can be made to GB / T5594.4-1985. The instrument can be the ZJD-C dielectric constant tester of Beijing AVIC Times Instrument Equipment Co., Ltd.

[0218] 6. Volume average particle size

[0219] The volume average particle size Dv50 is well known in the art and can be measured by instruments and methods well known in the art. For example, it can be conveniently measured by a laser particle size analyzer with reference to GB / T 19077-2016 particle size distribution laser diffraction method, such as the Mastersizer 2000E laser particle size analyzer of Malvern Instruments Ltd., UK.

[0220]

[0221]

[0222] From the above experimental data, we can see that:

[0223] The negative electrode slurries of Examples 1 to 16 contain the novel composite material of the present application, which includes: a negative electrode active material (artificial graphite), dielectric material particles (barium titanate particles); and a binder resin (styrene-butadiene rubber); wherein at least a portion of the surface of the dielectric material particles is coated with a coupling agent (γ-mercaptopropyltrimethoxysilane), and the coupling agent bridges the dielectric material particles and the binder resin.

[0224] The dielectric material particles in the composite material of the present application are bridged to the binder resin through a coupling agent, which can bring the following beneficial effects:

[0225] (1) The dielectric material particles are evenly dispersed in the electrode slurry and will not all settle at the bottom of the slurry;

[0226] (2) The dielectric material particles can be bonded to the surface of the negative electrode active material through the binder, and the distance between the dielectric material particles and the surface of the negative electrode active material is relatively close, so as to give full play to the modification effect;

[0227] (3) The volume of the negative electrode active material will expand / contract during the charge and discharge process. During this process, since the dielectric material particles are bridged on the binder resin, the dielectric material particles will not fall off as the negative electrode active material expands / contracts, and will not lose contact with the negative electrode active material. The dielectric material particles can maintain stable contact with the negative electrode active material during the operation of the battery, and can thus stably play a modifying role.

[0228] From the perspective of battery performance, the battery of the present application exhibits one or more of the following properties:

[0229] (1) Improved negative electrode capacity;

[0230] (2) Improved first-cycle Coulombic efficiency;

[0231] (3) Reduced charging resistance;

[0232] (4) Longer cycle life.

[0233] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A composite material comprising Negative electrode active material; Dielectric material particles; and Binder; in, At least a portion of the surface of the dielectric material particles is covered with a coupling agent, the coupling agent bridges the dielectric material particles and the binder, and the binder binds the dielectric material particles to the negative electrode active material.

2. The composite material according to claim 1, wherein The relative dielectric constant of the dielectric material particles is 80-200.

3. The composite material according to any one of claims 1 to 2, wherein The dielectric material is selected from one or more of the following: barium titanate, lead titanate, lithium niobate, lead zirconate titanate, lead metaniobate, and lithium barium lead niobate.

4. The composite material according to any one of claims 1 to 3, wherein The binder is an organic binder.

5. The composite material according to any one of claims 1 to 4, wherein The binder is selected from one or more of the following: polyacrylic acid (PAA), styrene-butadiene rubber (SBR), polyamide-imide (PAI), polyvinyl alcohol (PVA), polyethyleneimine (PEI), polyimide binder (PI), polytert-butyl acrylate-triethoxyvinyl silane (TBATEVS).

6. The composite material according to any one of claims 1 to 5, wherein The coupling agent is selected from one or more of the following: silane coupling agent, titanate coupling agent.

7. The composite material according to any one of claims 1 to 6, wherein The coupling agent is selected from one or more of silane coupling agent KH590, silane coupling agent KH550, silane coupling agent KH560, silane coupling agent KH570, silane coupling agent KH792, silane coupling agent DL602, silane coupling agent DL171, chelate 100 type titanate coupling agent, and chelate 200 type titanate coupling agent.

8. The composite material according to any one of claims 1 to 7, having one or more of the following characteristics (1) The coupling agent is connected to the dielectric material via a first terminal functional group, wherein the first terminal functional group includes -O-; (2) The coupling agent is connected to the binder via a second terminal functional group, and the second terminal functional group includes -S-.

9. The composite material according to any one of claims 1 to 7, having one or more of the following characteristics (1) The coupling agent is connected to the dielectric material via a first terminal functional group, wherein the first terminal functional group includes -Si-O-; (2) The coupling agent is connected to the binder via a second terminal functional group, and the second terminal functional group includes -CS-.

10. The composite material according to any one of claims 1 to 9, wherein The number average molecular weight of the binder is 1 million to 2 million.

11. The composite material according to any one of claims 1 to 10, wherein The dielectric material particles have one or more of the following characteristics: (1) The dielectric material particles are zero-dimensional particles; (2) The dielectric material particles are tetragonal barium titanate particles; (3) The volume median particle size of the dielectric material particles is 50 nm to 200 nm; (4) The volume median particle size of the negative electrode active material is 4 to 10 μm; (5) The ratio of the volume median particle size of the negative electrode active material to the volume median particle size of the dielectric material particles is 200:1 to 20:

1.

12. The composite material according to any one of claims 1 to 11, wherein The mass ratio of the dielectric material to the binder is 0.1:100 to 1:

100.

13. A method for preparing a composite material, wherein the composite material is defined as in any one of claims 1 to 12; The preparation method comprises: (1) performing a hydroxylation treatment on the dielectric material particles to obtain hydroxylated dielectric material particles; (2) grafting a coupling agent onto the hydroxylated dielectric material particles to obtain dielectric material particles grafted with the coupling agent; (3) connecting the coupling agent grafted on the dielectric material particles with the binder through a condensation reaction; (4) Mix the product from the previous step with the negative electrode active material.

14. The method according to claim 13, wherein in step (3), the coupling agent on the dielectric material particles contains a thiol terminal group, the binder contains an alkenyl terminal group, and the coupling agent and the binder are connected via a thiol-alkenyl click chemistry reaction.

15. The method according to claim 14, wherein the thiol-ene click chemistry reaction is carried out under the action of a photoinitiator and ultraviolet light.

16. An electrode comprising the composite material according to any one of claims 1 to 12.

17. A secondary battery comprising the electrode according to claim 16.

18. An electric device comprising the secondary battery according to claim 17.

Citation Information

Patent Citations

  • Coating composition

    CN101490767A

  • Binder for silicon-based negative electrode of lithium ion battery, silicon-based negative electrode of lithium ion battery, preparation method of silicon-based negative electrode, and lithium ion battery

    CN110247017A

  • Electrode, secondary battery, battery pack, and vehicle

    CN110299556A

  • Lithium ion secondary battery and manufacturing method of positive electrode active material for lithium ion secondary battery

    JP2013191539A

  • Negative active material for rechargeable lithium battery and negative electrode and rechargeable lithium battery including same

    US20140050975A1