Lithium nitride composite material coated by adopting ALD (atomic layer deposition) technology as well as preparation method and application of lithium nitride composite material

By depositing a metal oxide coating layer on the surface of lithium nitride using ALD technology, the problem of active lithium being consumed by the SEI film in lithium-ion batteries is solved, improving the coulombic efficiency and stability of the battery and achieving a highly efficient lithium replenishment effect.

CN118943344APending Publication Date: 2024-11-12XIAOGAN CORNEX NEW ENERGY INNOVATION TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411344792.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing lithium-ion batteries consume active lithium ions during the first charge and discharge process due to the formation of an SEI film caused by electrolyte decomposition, resulting in low coulombic efficiency and capacity reduction. Furthermore, lithium nitride, as a positive electrode lithium replenishment additive, suffers from poor stability and high decomposition potential.

Method used

ALD technology is used to deposit a metal oxide coating layer on the surface of lithium nitride to form a composite material, which is used as a lithium replenishment additive for the positive electrode of lithium-ion batteries. By controlling the thickness and uniformity of the metal oxide layer, the stability and charge/discharge performance of the battery can be improved.

Benefits of technology

It improves the capacity retention and coulombic efficiency of lithium-ion batteries, reduces the decomposition potential, enhances battery stability and safety, and reduces the risk of side reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943344A_ABST
    Figure CN118943344A_ABST
Patent Text Reader

Abstract

The invention provides a lithium nitride composite material coated by adopting an ALD technology and a preparation method and application thereof, and relates to the technical field of lithium ion batteries, the composite material comprises lithium nitride powder and a metal oxide layer coating the outer surface of the lithium nitride powder; and the metal oxide layer is formed by adopting an ALD (Atomic Layer Deposition) technology. The metal oxide coating layer is deposited on the surface of lithium nitride through the ALD technology to obtain the composite material, and the composite material can serve as a lithium ion battery positive electrode lithium supplement additive to be added into a lithium ion battery positive electrode material, so that the capacity retention ratio and coulombic efficiency of the battery can be improved, and the stability and charging and discharging performance of the battery can also be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a lithium nitride composite material coated by ALD technology, and a preparation method and application thereof. Background Art

[0002] During the first charge and discharge process of lithium-ion batteries, the electrolyte will decompose and a solid electrolyte membrane SEI will be formed on the surface of the negative electrode. This process will consume the active lithium ions in the battery and convert them into lithium carbonate, lithium fluoride and alkyl lithium in the SEI components, resulting in low coulombic efficiency and decreased capacity of the first cycle of the whole battery. In response to the above problems, relevant technicians have proposed lithium replenishment technology for lithium-ion batteries. At present, the lithium replenishment technology for lithium-ion batteries is mainly divided into two processes: negative electrode lithium replenishment and positive electrode lithium replenishment. In terms of safety and cost issues, compared with negative electrode lithium replenishment, positive electrode lithium replenishment has received widespread attention, and the application of positive electrode lithium replenishment additives has been proposed. Among the many positive electrode lithium replenishment additives, lithium nitride has an extremely high theoretical specific capacity (2309mAh / g) and a low theoretical decomposition potential (~0.44Vvs.Li + / Li), the decomposition products are lithium ions and nitrogen gas, which has attracted a lot of attention and research.

[0003] Lithium nitride has high self-reactivity, poor stability in air, and its decomposition potential and decomposition rate need to be further improved. Lithium nitride has high chemical activity. The synthetic raw material is metallic lithium. It is very easy to react with air and water to produce lithium carbonate and lithium hydroxide during the synthesis process. The product has a high residual alkali content, which faces great difficulties in the actual production process. The synthesis route of lithium nitride product purity ≥ 98% requires extremely harsh conditions, requiring a highly dry and inert environment. When the purity is lower than 95%, the lithium delithiation potential of lithium nitride is above 4.7V, and the decomposition rate is only about 30%, which does not meet the requirements of industrial application. It is difficult to control the ratio of α-Li3N and β-Li3N generated by sintering, and the active lithium supplement phase is α-Li3N.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The purpose of the present invention is to provide a lithium nitride composite material coated by ALD technology, a preparation method and application thereof. The present invention deposits a metal oxide coating layer on the surface of lithium nitride by ALD technology to obtain a composite material, which can be added to the positive electrode material of a lithium ion battery as a lithium supplement additive for the positive electrode of a lithium ion battery, which can not only improve the capacity retention rate and coulomb efficiency of the battery, but also improve the stability and charging and discharging performance of the battery.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The present invention provides a lithium nitride composite material coated by ALD technology, wherein the composite material comprises lithium nitride powder and a metal oxide layer coated on the outer surface of the lithium nitride powder;

[0008] The metal oxide layer is formed by using ALD technology.

[0009] Further, on the basis of the above technical solution, the metal oxide includes one or more of aluminum oxide, zinc oxide, tungsten oxide, zirconium oxide, iron oxide, titanium oxide, nickel oxide, and manganese oxide;

[0010] And / or, the thickness of the metal oxide layer in the composite material is 2-18 nm.

[0011] The present invention also provides a method for preparing the lithium nitride composite material coated by ALD technology as described above, comprising the following steps:

[0012] (1) Determine the action time through BET test;

[0013] (2) Vibrating and dispersing the lithium nitride raw material, placing it in the ALD reaction chamber, evacuating the chamber and heating it;

[0014] (3) In a vacuum environment, introducing a first inert carrier gas to carry the vapor of the compound containing the metal element and deposit it on the surface of the lithium nitride particles;

[0015] (4) introducing a second inert carrier gas to blow away the metal element-containing compound physically adsorbed on the surface of the lithium nitride particles, leaving behind a layer of chemically adsorbed metal element-containing compound;

[0016] (5) injecting ozone to carry out redox reaction;

[0017] (6) introducing a third inert carrier gas to blow away byproducts and excess ozone on the surface of the lithium nitride particles;

[0018] (7) Repeat steps (3) to (6).

[0019] Further, based on the above technical solution, in step (1), the action time is 60-65s;

[0020] and / or, in step (2), the temperature is raised to 60-350° C.;

[0021] and / or, in step (3), the flow rate of the first inert carrier gas is 20-240 ml / min, and the duration is 55-65 s;

[0022] and / or, the first inert carrier gas comprises one or more of helium, argon or xenon;

[0023] In step (3), the vapor of the compound containing the metal element includes one of trimethylzinc vapor, trimethylaluminum vapor, trimethyliron vapor, trimethyltitanium vapor, trimethyltungsten vapor, trimethylzirconium vapor, trimethylnickel and trimethylmanganese;

[0024] And / or, in step (3), the volume flow ratio of the vapor of the compound containing the metal element to the first inert carrier gas is (5-40): (95-60);

[0025] and / or, in step (4), the flow rate of the second inert carrier gas is 20-350 ml / min, and the blow-off time is 115-125 s;

[0026] and / or, the second inert carrier gas comprises one or more of helium, argon or xenon;

[0027] And / or, in step (5), the flow rate of ozone is 35-240 ml / min, and the duration is 55-65 s;

[0028] And / or, in step (6), the flow rate of the third inert carrier gas is 20-350 ml / min, and the time of introduction is 115-125 s;

[0029] And / or, the third inert carrier gas includes one or more of helium, argon or xenon.

[0030] Further, on the basis of the above technical solution, in step (2), the method for preparing the lithium nitride raw material comprises the following steps:

[0031] S1: weighing metallic lithium and pre-treating it;

[0032] S2: performing preliminary nitridation treatment on the pretreated metallic lithium;

[0033] S3: Grinding the material obtained in step S2 and transferring it to a tube furnace for calcination to obtain an initial lithium nitride material;

[0034] S4: ball-milling the initial lithium nitride material, sieving, and taking the sieve material to obtain a lithium nitride raw material, which is used as a raw material before ALD treatment.

[0035] Further, on the basis of the above technical solution, in step S1, the pretreatment is carried out in a nitrogen glove box to destroy the surface coating of the metal lithium;

[0036] Among them, metallic lithium includes one or more of lithium powder, lithium belt, lithium sheet, lithium ingot, lithium rope and lithium alloy.

[0037] Further, on the basis of the above technical solution, in step S2, the preliminary nitridation treatment refers to a nitridation reaction of metallic lithium in a glove box containing a protective atmosphere;

[0038] The protective atmosphere is a mixed atmosphere of nitrogen and argon; the volume flow ratio of nitrogen to argon is (5-40): (95-60);

[0039] The nitridation reaction time is 1-72h; the nitridation temperature is 20-30°C.

[0040] Further, on the basis of the above technical solution, in step S3, the grinding refers to grinding the material obtained in step S2 in a mortar for 20-40 minutes;

[0041] And / or, in step S3, the protective atmosphere in the tubular furnace is nitrogen, the calcination temperature is 80-800° C., and the calcination time is 1-25 h.

[0042] Further, based on the above technical solution, the decomposition potential of the lithium nitride raw material obtained in step S4 is 3.7-4.1V, and the purity is 97.1-99.4%;

[0043] The mass ratio of α-Li3N to β-Li3N in the lithium nitride raw material is in the range of (97-90):(3-10);

[0044] And / or, in step S4, the ball milling beads used in the ball milling process are zirconium oxide balls with a diameter of 0.1 to 20 mm; the ball to material ratio is (10-60):1;

[0045] The ball milling atmosphere is a mixed atmosphere of nitrogen and argon, wherein the volume flow ratio of nitrogen to argon is (5-40):(95-60);

[0046] The ball milling speed is 80-1200rpm;

[0047] The ball milling method is to work for 10 minutes, rest for 5 minutes, repeat the cycle 2-18 times, and the total ball milling time is 20-180 minutes;

[0048] And / or, in step S4, sieving refers to sieving through a 150-600 mesh sieve.

[0049] The present invention also provides an application of the ALD-coated lithium nitride composite material as described above, or prepared by the ALD-coated lithium nitride composite material preparation method as described above, as a lithium supplement additive for a positive electrode of a lithium-ion battery.

[0050] The present invention provides a lithium nitride composite material coated by ALD technology, a preparation method and an application thereof, and the beneficial effects are as follows:

[0051] 1. The present invention ball-mills the initial lithium nitride material in a mixed atmosphere of nitrogen and argon in a specific ratio, thereby controlling the mass ratio of α-Li3N and β-Li3N in the lithium nitride within the range of (97-90):(3-10), thereby increasing the content of active lithium nitride. The lithium nitride obtained by the preparation method of the invention has a smaller particle size, is evenly distributed, and has high activity. Compared with the conventional method for preparing lithium nitride (the prepared lithium nitride has a low purity, resulting in a higher decomposition potential of more than 4.3V), the decomposition rate of the lithium nitride as a lithium supplement additive is higher, and the decomposition potential is reduced. The optimal conditions can obtain a more suitable decomposition potential (3.7-4.1V). The red lithium nitride active powder is synthesized and a metal oxide coating layer is deposited on the surface of the lithium nitride using the ALD technology to obtain a composite material.

[0052] 2. The present invention deposits a metal oxide coating layer on the surface of lithium nitride through the ALD technology to obtain a composite material. When the lithium nitride composite material is added to the positive electrode material of a lithium-ion battery as a positive electrode lithium replenishing additive, the lithium nitride exhibits the characteristics of low decomposition potential and high decomposition rate during the first cycle of charging. Only a very small amount of lithium nitride needs to be added to make up for the active lithium consumed when the SEI film is formed. Lithium nitride has high compatibility and lithium replenishing performance in the positive electrode material of a lithium-ion battery.

[0053] 3. The present invention deposits a metal oxide coating layer on the surface of lithium nitride through ALD technology to obtain a composite material. The coating refers to forming a protective shell on the surface of the lithium supplement material, which can protect the internal lithium supplement material core and reduce the hydrolysis of the lithium supplement material in humid air. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0055] Figure 1 The XRD diagram of α-Li3N provided by the present invention;

[0056] Figure 2 This is a strength comparison diagram of α-Li3N and β-Li3N provided by the present invention. DETAILED DESCRIPTION

[0057] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.

[0058] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0059] According to a first aspect of the present invention, there is provided a lithium nitride composite material coated by ALD technology, the composite material comprising lithium nitride powder and a metal oxide layer coated on the outer surface of the lithium nitride powder;

[0060] The metal oxide layer is formed by using ALD technology.

[0061] Specifically, the metal oxide is wrapped with lithium nitride using ALD technology. This composite material not only has a good lithium replenishment effect and improves the battery coulomb efficiency, but the presence of the coating layer can also inhibit active oxygen and capture free radicals generated during charging and discharging, significantly reducing the gas production of lithium-ion batteries during the charging and discharging process, and inhibiting the volume expansion of the battery, thereby effectively improving the charging and discharging stability and safety of lithium-ion batteries, and solving the safety hazards caused by adding lithium replenishers.

[0062] As an optional embodiment of the present invention, the metal oxide includes one or more of aluminum oxide, zinc oxide, tungsten oxide, zirconium oxide, iron oxide, titanium oxide, manganese oxide and nickel oxide;

[0063] Among them, aluminum oxide, zinc oxide, tungsten oxide, zirconium oxide, iron oxide, titanium oxide, manganese oxide and nickel oxide have different roles in the SEI film formation process, as follows:

[0064] Alumina can promote the formation of SEI film;

[0065] Zinc oxide has a high shielding coefficient and can form a dense, uniform, transparent and smooth film on the surface, protecting the material surface from external erosion and wear. This property helps to form a more stable SEI film;

[0066] Tungsten oxide has excellent physical and chemical stability, which may help enhance the durability of the SEI film;

[0067] As a ceramic material, zirconium oxide has high hardness, high melting point and high chemical stability, and these characteristics may play a role in enhancing the stability and density of the SEI film during its formation;

[0068] The iron ions in iron oxide may play a catalytic role in the battery reaction, promoting the formation and stabilization of the SEI film;

[0069] As a semiconductor material, titanium oxide has good photoelectric conversion effect and excellent chemical stability. It can participate in the formation of SEI film and provide a good ion transmission channel.

[0070] Manganese oxide and nickel oxide have similar effects. They can both act as catalysts to promote certain chemical reactions in the electrolyte. These reactions promote the formation of SEI film, improve cycle stability, reduce self-discharge, and improve the quality and stability of SEI film.

[0071] In contrast, although aluminum oxide is also a common oxide, its specific role in the formation of SEI film may be relatively single, and not as diverse and synergistic as several other oxides.

[0072] In order to achieve better effects, the thickness of the metal oxide layer in the composite material is 2-18 nm (for example, 3 nm, 5 nm, 7 nm, 9 nm, 11 nm, 13 nm, 15 nm, 17 nm, etc.).

[0073] Specifically, if the total thickness of the coated metal oxide layer is too thick, greater than the 18nm limit of this application, the diffusion path of lithium ions at the electrode or electrolyte interface will become longer, resulting in a decrease in the diffusion rate. This will increase the internal resistance of the battery, increase the battery polarization, and thus affect the battery capacity and efficiency, as well as the charge and discharge performance, etc.; too thick will also make it difficult for the lithium supplement to function;

[0074] If the coated metal oxide layer is too thin, less than the 2 nm limit of this application, the active material may be exposed due to insufficient coating, thereby increasing the risk of side reactions and resulting in unsatisfactory coating effects.

[0075] According to a second aspect of the present invention, there is provided a method for preparing a lithium nitride composite material coated by ALD technology, comprising the following steps:

[0076] (1) Determine the action time through BET test;

[0077] (2) Vibrating and dispersing the lithium nitride raw material, placing it in the ALD reaction chamber, evacuating the chamber and heating it;

[0078] (3) In a vacuum environment, introducing a first inert carrier gas to carry the vapor of the compound containing the metal element and deposit it on the surface of the lithium nitride particles;

[0079] (4) introducing a second inert carrier gas to blow away the metal element-containing compound physically adsorbed on the surface of the lithium nitride particles, leaving behind a layer of chemically adsorbed metal element-containing compound;

[0080] (5) injecting ozone to carry out redox reaction;

[0081] (6) introducing a third inert carrier gas to blow away byproducts and excess ozone on the surface of the lithium nitride particles;

[0082] (7) Repeat steps (3) to (6).

[0083] As an optional embodiment of the present invention, the preparation method of the lithium nitride composite material coated by ALD technology specifically includes the following steps:

[0084] (1) First, through the BET test, it is determined that the action time is 60-65s (for example, it can be 61s, 62s, 63s, 64s, etc.);

[0085] (2) The lithium nitride raw material is dispersed by vibration, and then placed in an ALD reaction chamber, evacuated and heated to 60-350°C (for example, 100°C, 150°C, 200°C, 250°C, 300°C, etc.), preferably 120°C; if the temperature is too low, the reaction will be slow or no reaction will occur, and if the temperature is too high, the reaction will be too violent.

[0086] (3) In a vacuum environment, a first inert carrier gas carries a vapor containing a metal element and deposits it on the surface of lithium nitride particles at a flow rate of 20-240 ml / min (for example, 50 ml / min, 100 ml / min, 150 ml / min, 200 ml / min, 220 ml / min, etc.), preferably 40 ml / min, for 55-65 s (for example, 58 s, 60 s, 62 s, 64 s, etc.);

[0087] The vapor of the compound containing the metal element includes one of trimethyl zinc vapor, trimethyl aluminum vapor, trimethyl iron vapor, trimethyl titanium vapor, trimethyl tungsten vapor, trimethyl zirconium vapor, trimethyl nickel and trimethyl manganese;

[0088] The first inert carrier gas includes one or more of helium, argon or xenon;

[0089] The volume flow ratio of the vapor of the metal element-containing compound and the first inert carrier gas is (5-40):(95-60), for example, 5:95, 10:90, 15:85, 20:80, 25:75, 30:70, 35:65, 40:60, etc.

[0090] Specifically, the volume flow ratio of the vapor of the metal element-containing compound and the first inert carrier gas is limited to (5-40): (95-60), which aims to ensure that within the entire delivery system, a sufficient amount of metal compound vapor can be effectively transported to the surface of the lithium nitride particles to participate in the reaction, and that an undesirable deposition effect will not occur due to excessively high or low vapor concentration.

[0091] When the volume flow rate of the metal element-containing compound vapor accounts for too much, the metal element-containing compound vapor will cause the surface of the lithium nitride particles to be quickly saturated, forming an overly thick physical adsorption layer. This adsorption layer not only increases the difficulty of subsequent processing, making it time-consuming and possibly incomplete to purge and remove excess metal elements, but also may cause excessive accumulation of local metal elements, making the thickness of the metal oxide layer extremely uneven when it is formed, thus affecting the performance and consistency of the overall material;

[0092] When the volume flow rate of the first inert carrier gas accounts for too high a proportion, although it can effectively protect the metal compound vapor from being oxidized or decomposed during the transportation process, it will also dilute the deposition density of the metal elements on the surface of the lithium nitride particles. In this case, due to insufficient metal element content, a continuous and uniform metal oxide layer may not be formed on the surface of the lithium nitride particles. Instead, problems such as incomplete coverage, holes or weak areas may occur, thereby weakening the protective effect or modification effect of the metal oxide layer on the lithium nitride particles.

[0093] (4) blowing off the metal element-containing compound physically adsorbed on the surface of the lithium nitride particles by a second inert carrier gas at a flow rate of 20-350 ml / min (e.g., 50 ml / min, 100 ml / min, 150 ml / min, 200 ml / min, 250 ml / min, 300 ml / min, etc.), preferably 80 ml / min, preferably 80 ml / min, leaving a layer of chemically adsorbed metal element-containing compound, and the blowing off time is 115-125 s (e.g., 118 s, 120 s, 122 s, 124 s, etc.);

[0094] The second inert carrier gas includes one or more of helium, argon or xenon;

[0095] If the metal element-containing compounds physically adsorbed on the surface of lithium nitride particles are not blown off, the thickness of the metal oxide layer coated on the surface of lithium nitride will be uneven, and the following problems will occur:

[0096] 1) Reduce lithium ion conduction efficiency:

[0097] The inhomogeneity of the oxide layer will lead to inconsistent diffusion paths of lithium ions on the electrode surface. Some areas may hinder the conduction of lithium ions due to excessively thick coating, while other areas may expose active materials due to insufficient coating, thereby increasing the risk of side reactions. This inhomogeneity will reduce the overall lithium ion conduction efficiency of the battery and affect the battery's charge and discharge performance;

[0098] 2) Increase electrode polarization:

[0099] Uneven oxide layers will lead to uneven charge distribution on the electrode surface, resulting in local polarization. Increased polarization will cause the battery's charge and discharge voltage platform to shift, reducing the battery's capacity and efficiency. In addition, polarization may also cause the temperature inside the battery to rise, further exacerbating the deterioration of battery performance.

[0100] 3) Reduce capacity retention rate:

[0101] The unevenness of the oxide layer may lead to inconsistent contact areas between the active material and the electrolyte. Some areas may have reduced contact with the electrolyte due to excessive coating, thereby reducing the utilization rate of the active material. This will lead to increased capacity decay during the battery cycle and reduce the battery's cycle stability and capacity retention rate.

[0102] 4) Increased risk of side effects:

[0103] The uneven oxide layer may introduce new interface problems, such as interface stress and interface defects, which may become the cause of side reactions. Especially at the contact interface between the electrolyte and the active material, the uneven coating may cause the local electrolyte concentration to be too high or too low, thus triggering side reactions such as electrolyte decomposition and gas generation.

[0104] 5) Impact on battery safety:

[0105] The unevenness of the oxide layer may also have an adverse effect on the safety of the battery. For example, during the battery charging and discharging process, the uneven coating may lead to uneven heat distribution, and the temperature of some areas rises too quickly due to heat accumulation, increasing the risk of thermal runaway of the battery. In addition, the uneven coating may also affect the performance of the battery under extreme conditions, such as high temperature, low temperature or rapid charging and discharging.

[0106] (5) injecting ozone, with an ozone flow rate of 35-240 ml / min (for example, 50 ml / min, 100 ml / min, 150 ml / min, 200 ml / min, 220 ml / min, etc.), preferably 80 ml / min, to react with the metal elements adsorbed on the surface of the lithium nitride particles to produce an oxidation-reduction reaction, for a duration of 55-65 s (for example, 58 s, 60 s, 62 s, 64 s, etc.);

[0107] (6) blowing the byproducts on the surface of the lithium nitride particles and excess ozone off the surface of the lithium nitride particles by a third inert carrier gas at a flow rate of 20-350 ml / min (e.g., 50 ml / min, 100 ml / min, 150 ml / min, 200 ml / min, 250 ml / min, 300 ml / min, etc.), preferably 80 ml / min, for 115-125 s (e.g., 118 s, 120 s, 122 s, 124 s, etc.);

[0108] The third inert carrier gas includes one or more of helium, argon or xenon;

[0109] (7) Repeat steps (3) to (6) 3-6 times to obtain an ALD-coated lithium nitride composite material.

[0110] The gas flow rates in steps (1)-(6) need to be controlled within a limited range because excessive gas flow will cause the raw materials to be blown away, while excessive gas flow will result in insufficient reaction.

[0111] Specifically, atomic layer deposition (ALD) technology is an advanced nanostructure manufacturing and surface modification technology. This technology achieves controllable thin film growth with atomic-level precision by periodically controlling the saturated chemical reaction between the gaseous reactant precursor and the surface of the substrate material. The unique film thickness control mechanism of ALD technology makes this technology applicable to the surface modification of high specific surface area particles and powdered materials. Another feature of ALD technology is that the film growth temperature is low, which is particularly important for energetic materials that are extremely sensitive to temperature. ALD metal oxide film on the surface of lithium nitride can reduce the water molecule permeability to 6×10 -6 g / (m 2 d) Effectively extend the service life. Therefore, depositing ALD metal oxide on the surface of lithium nitride can hinder the diffusion of water molecules, thereby reducing the reaction between lithium nitride and water. ALD technology generates a metal oxide coating film to cover the surface of lithium nitride, and accurately adjusts the thickness of the coating film by changing the number of deposition cycles to achieve the optimal coating effect. The control of the number of repetitions is to control the thickness of the final metal oxide coating layer, and the final thickness is controlled at 2-18nm. Too thin will result in unsatisfactory coating effect, and too thick will make it difficult for the lithium supplement to work.

[0112] As an optional embodiment of the present invention, in step (2), the method for preparing the lithium nitride raw material comprises the following steps:

[0113] S1: weighing metallic lithium and pre-treating it;

[0114] S2: performing preliminary nitridation treatment on the pretreated metallic lithium;

[0115] S3: Grinding the material obtained in step S2 and transferring it to a tube furnace for calcination to obtain an initial lithium nitride material;

[0116] S4: ball-milling the initial lithium nitride material, sieving, and taking the sieve material to obtain a lithium nitride raw material, which is used as a raw material before ALD treatment.

[0117] Specifically, a physical model of Li3N composite structure SEI with interfacial synergistic effect is constructed, and a new mechanically stable interface is constructed while retaining high ionic conductivity. The uneven composition and thickness of the improved SEI film can cause irreversible growth of lithium negative electrode dendrites and attenuation of battery performance. After the solid electrolyte interface (SEI) is spontaneously formed, the metal lithium negative electrode undergoes infinite volume expansion during the cycle. The SEI with low mechanical strength cannot adapt to the interface changes caused by this volume expansion, causing SEI self-fracture and reducing the coulombic efficiency of the battery. The artificial solid electrolyte interface (SEI) generated by the lithium nitride composite structure has a good driving effect on the lithium deposition behavior on the surface of the lithium metal negative electrode, including (1) preventing electrolyte decomposition: SEI film can prevent electrolyte decomposition, thereby extending the life of the battery; (2) maintaining battery capacity: SEI film can prevent unnecessary reactions between lithium ions and internal materials of the battery, which helps to maintain the battery capacity; (3) improving battery performance: SEI film can reduce the internal resistance of the battery, improve the performance and efficiency of the battery, etc.; SEI film can also alleviate the interface fluctuation caused by volume change. The better driving behavior of the layered composite SEI for deposited lithium atoms can inhibit the growth of dendrites on the surface of the lithium negative electrode.

[0118] As an optional embodiment of the present invention, in step S1, the pretreatment is to destroy the surface coating of the metal lithium in a nitrogen glove box, such as by grinding, scraping, etc.;

[0119] Among them, metallic lithium includes one or more of lithium powder, lithium belt, lithium sheet, lithium ingot, lithium rope, and lithium alloy. When the metallic lithium is a large surface area material such as lithium powder, it can be placed in a large surface container and slightly polished by machinery.

[0120] As an optional embodiment of the present invention, in step S2, the preliminary nitridation treatment refers to a nitridation reaction of metallic lithium in a glove box containing a protective atmosphere;

[0121] Wherein, the protective atmosphere is a mixed atmosphere of nitrogen and argon;

[0122] The volume flow ratio of nitrogen to argon is (5-40):(95-60), for example, it can be 5:95, 10:90, 15:85, 20:80, 25:75, 30:70, 35:65, 40:60, etc.

[0123] Specifically, by optimizing the flow ratio of nitrogen to argon, it is beneficial to further control the mass ratio of α-Li3N and β-Li3N in lithium nitride within a preferred range.

[0124] As an optional embodiment of the present invention, the nitridation reaction time is 1-72h (the nitridation time can be, for example, 1h, 5h, 10h, 15h, 20h, 25h, 30h, 35h, 40h, 45h, 50h, 55h, 60h, 65h, 70h or 72h), preferably 20h; the nitridation temperature is 20-30°C (for example, 22°C, 24°C, 26°C, 28°C, etc.), preferably 25°C.

[0125] Specifically, the nitriding time is related to the nitriding temperature. The higher the nitriding temperature, the shorter the corresponding nitriding time. After the nitriding reaction is completed, the color of the metallic lithium changes from white to black-red, and the initial reaction generates lithium nitride material with a harder texture.

[0126] As an optional embodiment of the present invention, in step S3, the grinding refers to grinding the material obtained in step S2 in a mortar for 20-40 minutes (for example, 25 minutes, 30 minutes, 35 minutes, etc.), preferably 30 minutes.

[0127] As an optional embodiment of the present invention, in step S3, the protective atmosphere in the tubular furnace is nitrogen, the calcination temperature is 80-800°C (for example, it can be 100°C, 200°C, 300°C, 400°C, 500°C, 600°C, 700°C, etc.), preferably 100°C, and the calcination time is 1-25h (for example, it can be 1h, 5h, 10h, 15h, 20h, 21h, 22h, 23h, 24h or 25h).

[0128] Specifically, the calcination time is related to the calcination temperature. The higher the calcination temperature, the shorter the corresponding calcination time. However, the calcination needs to be controlled within a reasonable temperature range. A low temperature will result in too long an action time or uneven phase distribution. A high temperature may result in uneven phase distribution or decomposition of lithium nitride. The reaction process at 80-800°C is mild and the phase distribution can achieve the expected effect.

[0129] As an optional embodiment of the present invention, the decomposition potential of the lithium nitride raw material obtained in step S4 is 3.7-4.1V (for example, 3.75V, 3.8V, 3.85V, 3.9V, 3.95V, 4.0V, etc.), and the purity is 97.1-99.4% (for example, 97.5%, 97.7%, 97.9%, 98%, 98.3%, 98.5%, 98.7%, 99%, etc.).

[0130] As an optional embodiment of the present invention, the mass ratio of α-Li3N and β-Li3N in the lithium nitride raw material is in the range of (97-90):(3-10), for example, it can be 91:9, 92:8, 93:7, 94:6, 95:5, 96:4, 97:3, etc.

[0131] As an optional embodiment of the present invention, in step S4, the ball milling is to further control the mass ratio of α-Li3N and β-Li3N in lithium nitride within a preferred range;

[0132] The ball milling beads used in the ball milling process are zirconia balls with a diameter of 0.1-20 mm (for example, a combination of one or more of 0.3 mm, 0.5 mm, 1 mm, 3 mm, 5 mm, 8 mm, 10 mm, 15 mm, and 20 mm), preferably 3 mm; the ball-to-material ratio is (10-60): 1 (for example, 20:1, 40:1, etc.), preferably 20:1; the ball-to-material ratio refers to the ratio of the weight of the ball milling beads to the weight of the initial lithium nitride material. The ball-to-material ratio in this range can achieve a good ball milling effect during the ball milling process, save ball milling time, and control the particle size distribution.

[0133] Specifically, by controlling the diameter of the ball milling beads within the above range, it is beneficial to improve the ball milling efficiency, reduce the ball milling time, and improve the uniform distribution of the particle size of the lithium nitride product.

[0134] Further, the ball milling atmosphere is a mixed atmosphere of nitrogen and argon, wherein the volume flow ratio of nitrogen to argon is (5-40):(95-60), for example, 5:95, 10:90, 15:85, 20:80, 25:75, 30:70, 35:65, 40:60, etc.;

[0135] Specifically, nitrogen is the reaction gas in the synthesis process of lithium nitride, which is beneficial to further control the mass ratio of α-Li3N and β-Li3N in lithium nitride within the preferred range and achieve the effect of inhibiting side reactions. Adjusting the ratio of the mixed gas can control the progress of phase conversion. The same ratio of the gas flow before and after step S2 and step S4 can simplify the operation and also control good reaction consistency.

[0136] Further, the rotation speed of the ball mill is 80-1200 rpm (for example, 200 rpm, 400 rpm, 600 rpm, 800 rpm, 1000 rpm, etc.), preferably 700 rpm;

[0137] Specifically, the speed during ball milling directly affects the mechanical force collision. If the speed is too high, α-Li3N is very likely to undergo phase change and generate β-Li3N. By controlling the ball milling speed within the above range, it is beneficial to control the mass ratio of α-Li3N and β-Li3N in lithium nitride within a suitable range, while reducing the high reactivity of lithium nitride, while maintaining the characteristics of low decomposition potential and high capacity.

[0138] Furthermore, the ball milling method is to work for 10 minutes, rest for 5 minutes, and repeat the cycle 2-18 times (for example, 3 times, 6 times, 9 times, 12 times, 15 times, etc.), preferably 6 times, and the total ball milling time (excluding the ball milling rest time) is 20-180 minutes (for example, 50 minutes, 70 minutes, 100 minutes, 130 minutes, 150 minutes, etc.), preferably 60 minutes.

[0139] Specifically, ball milling can uniformly control the particle size. The reaction time can also be controlled during high-energy ball milling to control the particle size distribution. Too short a total ball milling time will result in uneven particle size distribution, while too long a ball milling time will result in phase transformation of lithium nitride.

[0140] As an optional embodiment of the present invention, in step S4, sieving refers to sieving through a 150-600 mesh sieve, preferably a 400 mesh sieve.

[0141] According to a third aspect of the present invention, there is provided an application of the ALD-coated lithium nitride composite material as described above or prepared by the preparation method of the ALD-coated lithium nitride composite material as described above, which can be used as a positive electrode lithium supplement material for lithium ion batteries. Preferably, the lithium nitride composite material of the present invention is added together with the positive electrode active material during the preparation of the positive electrode slurry, and its addition amount accounts for 0.5%-4.5% of the mass of the positive electrode active material.

[0142] The present invention will be further described in detail below with reference to specific embodiments and comparative examples.

[0143] Embodiment 1:

[0144] S1: In a nitrogen glove box, weigh 50g of lithium sheet and polish the surface coating of the lithium sheet.

[0145] S2: Perform preliminary nitridation treatment in a glove box containing a mixed atmosphere of nitrogen and argon at 25°C for 20 hours to generate a black-red lithium nitride material;

[0146] Among them, the volume flow ratio of nitrogen and argon is 15:85;

[0147] S3: Grind the preliminarily nitrided lithium nitride material in a mortar for 30 minutes, transfer it to a nitrogen tube furnace, and calcine it at 100° C. for 25 hours to obtain an initial lithium nitride material;

[0148] S4: ball milling in a mixed atmosphere of nitrogen and argon;

[0149] The volume flow ratio of nitrogen to argon was 15:85, the diameter of the zirconia ball was 3 mm, the ball-to-material ratio was 20:1, the ball milling speed was 700 rpm, the ball milling method was 10 min of work, 5 min of rest, repeated 6 times, and the total ball milling time was 1 h.

[0150] Pass the mixture through a 400-mesh sieve and take the material under the sieve as the lithium nitride raw material before ALD treatment;

[0151] like Figure 1 As shown, it is the XRD pattern of the lithium nitride raw material prepared in this embodiment. Compared with the reference standard PDF#02-0301, the peak positions are almost the same, indicating that the purity of the prepared lithium nitride raw material is relatively high.

[0152] The mass ratio of α-Li3N and β-Li3N in the lithium nitride prepared in this embodiment is 95:5. Figure 2 As shown, it is a comparison chart of the intensity of α-Li3N and β-Li3N in lithium nitride.

[0153] S5: ALD technology is used to deposit zinc oxide nZnO (n is the number of layers, 3≤n≤6) on the surface of the lithium nitride raw material:

[0154] (1) After BET test, the action time is determined to be 65s.

[0155] (2) First, the lithium nitride powder is dispersed by vibration, and then placed in the ALD reaction chamber, evacuated and heated to 120°C;

[0156] (3) In a vacuum environment, argon gas with a flow rate of 40 ml / min carries trimethyl zinc vapor and deposits it on the surface of lithium nitride particles for 60 seconds;

[0157] The volume flow ratio of argon gas to trimethyl zinc vapor is 95:5;

[0158] (4) The argon gas with a flow rate of 80 ml / min was used to blow away the trimethyl zinc physically adsorbed on the surface of the lithium nitride particles, leaving a layer of trimethyl zinc chemically adsorbed. The blowing time was 120 s.

[0159] (5) Ozone undergoes a redox reaction with trimethylzinc adsorbed on the surface of lithium nitride particles, and the ozone injection time is 60 s;

[0160] (6) Argon gas with a flow rate of 80 ml / min was used to blow away the byproducts and excess ozone on the surface of the lithium nitride particles. The time of introduction was 120 s.

[0161] Steps (3) to (6) constitute one cycle, and one layer of ZnO particles is deposited on the surface of lithium nitride. This cycle is repeated 3-6 times to prepare lithium nitride with three layers of ZnO deposition (labeled as 3Zn@LN), lithium nitride with four layers of ZnO deposition (labeled as 4Zn@LN), and LN with six layers of ZnO deposition (labeled as 6Zn@LN).

[0162] Embodiment 2:

[0163] Aluminum oxide nAl2O3 (n is the number of layers, 3≤n≤6) is deposited on the surface of the lithium nitride raw material prepared in step S4 of Example 1 using ALD technology:

[0164] (1) After BET test, the action time is determined to be 65s.

[0165] (2) First, disperse the lithium nitride powder by vibration, then place it into the ALD reaction chamber, evacuate it and heat it to 150°C;

[0166] (3) In a vacuum environment, helium gas with a flow rate of 50 ml / min carries trimethylaluminum vapor and deposits it on the surface of lithium nitride particles for 55 seconds;

[0167] The volume flow ratio of helium and trimethylaluminum vapor is 90:10;

[0168] (4) Helium gas with a flow rate of 100 ml / min blows off the trimethylaluminum physically adsorbed on the surface of the lithium nitride particles, leaving a layer of trimethylaluminum chemically adsorbed. The blowing time is 125 s.

[0169] (5) Ozone undergoes a redox reaction with trimethylaluminum adsorbed on the surface of lithium nitride particles, and the ozone injection time is 55 s;

[0170] (6) Helium gas with a flow rate of 100 ml / min was used to blow away the byproducts and excess ozone on the surface of the lithium nitride particles. The time of introduction was 125 s.

[0171] Steps (3) to (6) constitute a cycle, and one layer of Al2O3 particles is deposited on the surface of lithium nitride. This cycle is repeated 3-6 times to prepare lithium nitride with three layers of Al2O3 deposited (labeled as 3Al@LN), lithium nitride with four layers of Al2O3 deposited (labeled as 4Al@LN), and LN with six layers of Al2O3 deposited (labeled as 6Al@LN).

[0172] Embodiment 3:

[0173] Aluminum oxide nFe2O3 (n is the number of layers, 3≤n≤6) is deposited on the surface of the lithium nitride raw material prepared in step S4 of Example 1 using ALD technology:

[0174] (1) After BET test, the action time is determined to be 60s.

[0175] (2) First, disperse the lithium nitride powder by vibration, then place it into the ALD reaction chamber, evacuate it and heat it to 150°C;

[0176] (3) In a vacuum environment, argon gas with a flow rate of 60 ml / min carries trimethyl iron vapor and deposits it on the surface of lithium nitride particles for 60 seconds;

[0177] The volume flow ratio of argon gas to trimethyl iron vapor is 75:25;

[0178] (4) The argon gas with a flow rate of 90 ml / min was used to blow off the trimethyl iron physically adsorbed on the surface of the lithium nitride particles, leaving a layer of chemically adsorbed trimethyl iron. The blowing time was 120 s.

[0179] (5) Ozone undergoes a redox reaction with trimethyl iron adsorbed on the surface of lithium nitride particles, and the ozone injection time is 60 seconds;

[0180] (6) Argon gas with a flow rate of 90 ml / min was used to blow away the byproducts and excess ozone on the surface of the lithium nitride particles. The time of introduction was 120 s.

[0181] Steps (3) to (6) constitute a cycle, and one layer of Fe2O3 particles is deposited on the surface of lithium nitride. This cycle is repeated 3-6 times to prepare lithium nitride with three layers of Fe2O3 deposited (labeled as 3Fe@LN), lithium nitride with four layers of Fe2O3 deposited (labeled as 4Fe@LN), and LN with six layers of Fe2O3 deposited (labeled as 6Fe@LN).

[0182] Embodiment 4:

[0183] Titanium oxide nTiO2 (n is the number of layers, 3≤n≤6) is deposited on the surface of the lithium nitride raw material prepared in step S4 of Example 1 using ALD technology:

[0184] (1) After BET test, the action time is determined to be 60s.

[0185] (2) First, the lithium nitride powder is dispersed by vibration, and then placed in the ALD reaction chamber, evacuated and heated to 160°C;

[0186] (3) In a vacuum environment, argon gas with a flow rate of 100 ml / min carries trimethyl titanium vapor and deposits it on the surface of lithium nitride particles for 65 seconds;

[0187] The volume flow ratio of argon gas to trimethyl titanium vapor is 65:35;

[0188] (4) The argon gas with a flow rate of 150 ml / min was used to blow away the trimethyl titanium physically adsorbed on the surface of the lithium nitride particles, leaving a layer of chemically adsorbed trimethyl titanium. The blowing time was 115 s.

[0189] (5) Ozone undergoes a redox reaction with trimethyltitanium adsorbed on the surface of lithium nitride particles, and the ozone injection time is 65 s;

[0190] (6) Argon gas with a flow rate of 150 ml / min was used to blow away byproducts and excess ozone from the surface of the lithium nitride particles. The time of introduction was 115 s.

[0191] Steps (3) to (6) constitute a cycle, and a layer of TiO2 particles is deposited on the surface of lithium nitride. This cycle is repeated 3-6 times to prepare lithium nitride with 3 layers of TiO2 deposited (labeled as 3Ti@LN), lithium nitride with 4 layers of TiO2 deposited (labeled as 4Ti@LN), and LN with 6 layers of TiO2 deposited (labeled as 6Ti@LN).

[0192] Embodiment 5:

[0193] Titanium oxide nNiO (n is the number of layers, 3≤n≤6) is deposited on the surface of the lithium nitride raw material prepared in step S4 of Example 1 using ALD technology:

[0194] (1) After BET test, the action time is determined to be 60s.

[0195] (2) First, the lithium nitride powder is dispersed by vibration, and then placed in the ALD reaction chamber, evacuated and heated to 160°C;

[0196] (3) In a vacuum environment, argon gas with a flow rate of 100 ml / min carries trimethylnickel vapor and deposits it on the surface of lithium nitride particles for 60 seconds;

[0197] The volume flow ratio of argon gas to trimethylnickel vapor is 85:15;

[0198] (4) using argon gas at a flow rate of 150 ml / min to blow away the trimethylnickel physically adsorbed on the surface of the lithium nitride particles, leaving behind a layer of trimethylnickel chemically adsorbed. The blowing time is 120 s.

[0199] (5) Ozone undergoes a redox reaction with trimethylnickel adsorbed on the surface of lithium nitride particles, and the ozone injection time is 60 s;

[0200] (6) Argon gas with a flow rate of 150 ml / min was used to blow away the byproducts and excess ozone on the surface of the lithium nitride particles. The time of introduction was 120 s.

[0201] Steps (3) to (6) constitute a cycle, and one layer of NiO particles is deposited on the surface of lithium nitride. This cycle is repeated 3-6 times to prepare lithium nitride with three layers of NiO deposition (labeled as 3Ni@LN), lithium nitride with four layers of NiO deposition (labeled as 4Ni@LN), and LN with six layers of NiO deposition (labeled as 6Ni@LN).

[0202] Embodiment 6:

[0203] Titanium oxide nMnO (n is the number of layers, 3≤n≤6) is deposited on the surface of the lithium nitride raw material prepared in step S4 of Example 1 using ALD technology:

[0204] (1) After BET test, the action time is determined to be 60s.

[0205] (2) First, the lithium nitride powder is dispersed by vibration, and then placed in the ALD reaction chamber, evacuated and heated to 160°C;

[0206] (3) In a vacuum environment, argon gas with a flow rate of 100 ml / min carries trimethyl manganese vapor and deposits it on the surface of lithium nitride particles for 65 seconds;

[0207] The volume flow ratio of argon gas to trimethylmanganese vapor is 85:15;

[0208] (4) The argon gas with a flow rate of 150 ml / min was used to blow off the trimethyl manganese physically adsorbed on the surface of the lithium nitride particles, leaving a layer of trimethyl manganese chemically adsorbed. The blowing time was 115 s.

[0209] (5) Ozone undergoes a redox reaction with trimethylmanganese adsorbed on the surface of lithium nitride particles, and the ozone injection time is 65 seconds;

[0210] (6) Argon gas with a flow rate of 150 ml / min was used to blow away byproducts and excess ozone from the surface of the lithium nitride particles. The time of introduction was 115 s.

[0211] Steps (3) to (6) constitute one cycle, and one layer of MnO particles is deposited on the surface of lithium nitride. This cycle is repeated 3-6 times to prepare lithium nitride with three layers of MnO deposited (labeled as 3Mn@LN), lithium nitride with four layers of MnO deposited (labeled as 4Mn@LN), and LN with six layers of MnO deposited (labeled as 6Mn@LN).

[0212] Comparative Example 1:

[0213] ALD technology is used to deposit iron oxide nFe2O3 (n is the number of layers, n=1) on the surface of the lithium nitride raw material prepared in step S4 of Example 1:

[0214] (1) After BET test, the action time is determined to be 60s. The specific steps are as follows:

[0215] (2) First, disperse the lithium nitride powder by vibration, then place it into the ALD reaction chamber, evacuate it and heat it to 150°C;

[0216] (3) In a vacuum environment, argon gas with a flow rate of 60 ml / min carries trimethyl iron vapor and deposits it on the surface of lithium nitride particles for 60 seconds;

[0217] The volume flow ratio of argon gas to trimethyl iron vapor is 75:25;

[0218] (4) The argon gas with a flow rate of 90 ml / min was used to blow off the trimethyl iron physically adsorbed on the surface of the lithium nitride particles, leaving a layer of chemically adsorbed trimethyl iron. The blowing time was 120 s.

[0219] (5) Ozone undergoes a redox reaction with trimethyl iron adsorbed on the surface of lithium nitride particles, and the ozone injection time is 60 seconds;

[0220] (6) Argon gas with a flow rate of 90 ml / min was used to blow away the byproducts and excess ozone on the surface of the lithium nitride particles. The time of introduction was 120 s.

[0221] Steps (3) to (6) constitute one cycle, and a layer of Fe2O3 particles is deposited on the surface of lithium nitride. Repeat this cycle once to obtain a layer of Fe2O3-deposited lithium nitride (labeled as Fe@LN).

[0222] Comparative Example 2:

[0223] Titanium oxide nTiO2 (n is the number of layers, n=1) is deposited on the surface of the lithium nitride raw material prepared in step S4 of Example 1 using ALD technology:

[0224] (1) After BET test, the action time is determined to be 60s.

[0225] (2) First, the lithium nitride powder is dispersed by vibration, and then placed in the ALD reaction chamber, evacuated and heated to 160°C;

[0226] (3) In a vacuum environment, argon gas with a flow rate of 100 ml / min carries trimethyl titanium vapor and deposits it on the surface of lithium nitride particles for 65 seconds;

[0227] The volume flow ratio of argon gas to trimethyl titanium vapor is 65:35;

[0228] (4) The argon gas with a flow rate of 150 ml / min was used to blow away the trimethyl titanium physically adsorbed on the surface of the lithium nitride particles, leaving a layer of chemically adsorbed trimethyl titanium. The blowing time was 115 s.

[0229] (5) Ozone undergoes a redox reaction with trimethyltitanium adsorbed on the surface of lithium nitride particles, and the ozone injection time is 65 s;

[0230] (6) Argon gas with a flow rate of 150 ml / min was used to blow away byproducts and excess ozone from the surface of the lithium nitride particles. The time of introduction was 115 s.

[0231] Steps (3) to (6) constitute a cycle, and a layer of TiO2 particles is deposited on the surface of lithium nitride. Repeat this cycle once to obtain a layer of lithium nitride with TiO2 deposited (labeled as Ti@LN).

[0232] Comparative Example 3:

[0233] Titanium oxide nTiO2 (n is the number of layers, n=2) is deposited on the surface of the lithium nitride raw material prepared in step S4 of Example 1 using ALD technology:

[0234] (1) After BET test, the action time is determined to be 60s.

[0235] (2) First, the lithium nitride powder is dispersed by vibration, and then placed in the ALD reaction chamber, evacuated and heated to 160°C;

[0236] (3) In a vacuum environment, argon gas with a flow rate of 100 ml / min carries trimethyl titanium vapor and deposits it on the surface of lithium nitride particles for 65 seconds;

[0237] The volume flow ratio of argon gas to trimethyl titanium vapor is 65:35;

[0238] (4) The argon gas with a flow rate of 150 ml / min was used to blow away the trimethyl titanium physically adsorbed on the surface of the lithium nitride particles, leaving a layer of chemically adsorbed trimethyl titanium. The blowing time was 115 s.

[0239] (5) Ozone undergoes a redox reaction with trimethyltitanium adsorbed on the surface of lithium nitride particles, and the ozone injection time is 65 s;

[0240] (6) Argon gas with a flow rate of 150 ml / min was used to blow away byproducts and excess ozone from the surface of the lithium nitride particles. The time of introduction was 115 s.

[0241] Steps (3) to (6) constitute a cycle, and two layers of TiO2 particles are deposited on the surface of lithium nitride. This cycle is repeated twice to prepare lithium nitride with two layers of TiO2 deposited (labeled as 2Ti@LN).

[0242] Comparative Example 4

[0243] The lithium nitride raw material used in this comparative example is the lithium nitride raw material prepared in step S4 of Example 1;

[0244] The main difference between this comparative example and Example 1 is that when the ALD technology is used to coat zinc oxide, step (4) is omitted and step (5) is directly performed. The prepared lithium nitride composite materials are marked as 3'Zn@LN, 4'Zn@LN and 6'Zn@LN, respectively. The remaining technical parameters and operating steps are the same as those in Example 1.

[0245] Comparative Example 5

[0246] The lithium nitride raw material used in this comparative example is the lithium nitride raw material prepared in step S4 of Example 1;

[0247] The main difference between this comparative example and Example 1 is that when zinc oxide nZnO is deposited on the surface of the lithium nitride raw material using the ALD technology, steps (3) to (6) are repeated 8 times, and the prepared lithium nitride with 8 layers of zinc oxide ZnO deposited is marked as 8'Zn@LN. The remaining technical parameters and operating steps are the same as those in Example 1.

[0248] Application Examples

[0249] Preparation of half-cell containing lithium nitride:

[0250] The positive electrode active material used is lithium iron phosphate;

[0251] The diaphragm is a 9+3 ceramic single-sided adhesive PE diaphragm;

[0252] The electrolyte is a commercially available lithium hexafluorophosphate electrolyte;

[0253] The lithium nitride composite materials prepared in the embodiment and the comparative example are respectively used as positive electrode lithium supplement materials for lithium ion batteries, and are added together with the positive electrode active material during the homogenization process of the positive electrode material;

[0254] Preparation of positive electrode sheet: Disperse 1.96g lithium iron phosphate in an appropriate amount of N,N-dimethylformamide DMF, stir and mix well, then add 0.04g lithium nitride composite material, 0.0526g binder polyvinylidene fluoride PVDF (add binder in the form of PVDF and DMF to form a glue), 0.0526g conductive agent SP, continue to homogenize, mix evenly until the slurry has good fluidity, and obtain positive electrode slurry. The positive electrode current collector uses 13μm aluminum foil, and the positive electrode slurry is coated on the side of the positive electrode current collector and compacted. The density after roller pressing is 374g / m 2 After drying, the positive electrode sheet is obtained, wherein the coating surface density of the positive electrode sheet is 376.4g / m 2 .

[0255] Preparation of negative electrode sheet: Graphite, SP, CMC and SBR are prepared into slurry in a mass ratio of 95.5:1.5:1.2:1.8, the slurry viscosity is adjusted to 4000±200mPa·s, and the prepared slurry is prepared into a slurry with a double-sided surface density of 136g / m 2 They are evenly coated on 8μm copper foil and the compaction density is 1.50g / cm 3 The negative electrode is rolled into a negative electrode sheet.

[0256] The positive electrode sheet and the negative electrode sheet are assembled into a half-cell, with a theoretical charge capacity of 160 mAh / g and a theoretical discharge capacity of 144 mAh / g.

[0257] Half-cell performance test:

[0258] 1. Lithium nitride decomposition potential test:

[0259] The half-cell charge and discharge test was carried out on the Blue Electric Battery Test System. The charge and discharge voltage was 2.0-4.5V and the charge and discharge rate was 0.05C. The first-cycle charging platform and the capacity change after adding lithium nitride to the lithium iron half-cell were observed to obtain the decomposition potential of lithium nitride.

[0260] 2. Lithium nitride purity:

[0261] It is obtained after processing according to the XRD characterization results.

[0262] 3. Battery capacity retention rate

[0263] The capacity retention rate refers to the ratio of the discharge capacity of the battery to the initial discharge capacity after a certain period of time or a certain number of cycles, and is usually expressed as a percentage. The half-battery is tested for the battery capacity retention rate. The specific test method includes the following steps:

[0264] 1) Initial discharge capacity test: First, the battery is fully charged and then discharged at a standard discharge rate to obtain the initial discharge capacity C0 of the battery;

[0265] 2) Cycle: The battery is charged and discharged for 500 times;

[0266] 3) Re-discharge test: After storage or cycling, the battery is fully charged again and discharged at the standard discharge rate to obtain the discharge capacity C1 at this time;

[0267] Calculate the capacity retention rate: According to the definition of capacity retention rate, that is, the ratio of C1 to C0, the capacity retention rate of the battery is calculated;

[0268] The higher the capacity retention rate, the more stable the battery performance and the longer its service life.

[0269] 4. Coulombic efficiency of the battery

[0270] The coulombic efficiency of a battery refers to the ratio of the output charge to the input charge during the charge and discharge process of the battery, usually expressed as a percentage. The coulombic efficiency test of a half-battery is performed. The specific test method includes the following steps:

[0271] 1) Preparation stage: Place the battery in a thermostat and connect the battery and the test equipment using a four-wire method. Set the thermostat temperature to 35°C to simulate the temperature conditions of the actual working environment.

[0272] 2) Connect the test equipment: Make sure the battery is properly connected to the test equipment for subsequent charge and discharge tests;

[0273] 3) Charge and discharge test: Perform charge and discharge test on the battery according to the requirements of the test equipment. During the charging process, record the input charge of the battery; during the discharging process, record the output charge of the battery;

[0274] The value of the coulombic efficiency was calculated based on the ratio of the recorded output charge to the input charge.

[0275] The higher the coulombic efficiency, the smaller the charge loss of the battery during the charging and discharging process, and the better the performance.

[0276] 5. Thickness of metal oxide layer:

[0277] The thickness of the oxide layer is calculated by measuring the diffraction intensity of X-rays on the surface of lithium nitride.

[0278] Performance data

[0279] Table 1

[0280]

[0281]

[0282] According to Table 1, the present application uses ALD technology to deposit 3-6 layers of metal oxide layers on the surface of lithium nitride. The lithium-ion positive electrode battery prepared therefrom can make the battery capacity retention rate and coulomb efficiency range from 98.3-102.7% and 88.1-91.0%, respectively, so that the battery maintains good stability and improves the charging and discharging performance of the battery.

[0283] According to Table 1, since only one layer of Fe2O3 particles is deposited on the surface of lithium nitride in Comparative Example 1, the thickness of the iron oxide layer is relatively thin, resulting in an unsatisfactory coating effect. Therefore, the capacity retention rate and coulombic efficiency of the battery in Comparative Example 1 are much lower than those in Example 3.

[0284] According to Table 1, in Comparative Example 2, since only one layer of TiO2 particles is deposited on the surface of lithium nitride, the thickness of the titanium oxide layer is relatively thin, resulting in an unsatisfactory coating effect. Therefore, the capacity retention rate and coulombic efficiency of the battery in Comparative Example 2 are much lower than those in Example 4.

[0285] According to Table 1, since Comparative Example 3 only deposits two layers of TiO2 particles on the surface of lithium nitride, compared with Comparative Example 2, the capacity retention rate and coulombic efficiency are better than those of Comparative Example 2, but the thickness of the titanium oxide layer is still relatively thin, resulting in unsatisfactory coating effect.

[0286] According to Table 1, in Comparative Example 4, since step (4) is omitted and step (5) is directly performed during the ALD process, resulting in uneven thickness of the metal oxide layer coated on the surface of lithium nitride, the capacity retention rate and coulombic efficiency of the battery in Comparative Example 4 are much lower than those in Example 1.

[0287] According to Table 1, in Comparative Example 5, since steps (3) to (6) were repeated 8 times, the total thickness of the zinc oxide layer reached 20.4 nm due to excessive repetitions. The total thickness of the zinc oxide layer was too thick, which affected the capacity retention rate and coulombic efficiency of the battery.

[0288] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A lithium nitride composite material coated by ALD technology, characterized in that: The composite material comprises lithium nitride powder and a metal oxide layer coated on the outer surface of the lithium nitride powder; The metal oxide layer is formed by using ALD technology.

2. The lithium nitride composite material coated by ALD technology according to claim 1, characterized in that: The metal oxide includes one or more of aluminum oxide, zinc oxide, tungsten oxide, zirconium oxide, iron oxide, titanium oxide, nickel oxide, and manganese oxide; And / or, the thickness of the metal oxide layer in the composite material is 2-18 nm.

3. A method for preparing a lithium nitride composite material coated by ALD technology as claimed in any one of claims 1 to 2, characterized in that: The steps include: (1) Determine the action time through BET test; (2) Vibrating and dispersing the lithium nitride raw material, placing it in the ALD reaction chamber, evacuating the chamber and heating it; (3) In a vacuum environment, introducing a first inert carrier gas to carry the vapor of the compound containing the metal element and deposit it on the surface of the lithium nitride particles; (4) introducing a second inert carrier gas to blow away the metal element-containing compound physically adsorbed on the surface of the lithium nitride particles, leaving behind a layer of chemically adsorbed metal element-containing compound; (5) injecting ozone to carry out redox reaction; (6) introducing a third inert carrier gas to blow away byproducts and excess ozone on the surface of the lithium nitride particles; (7) Repeat steps (3) to (6).

4. The method for preparing a lithium nitride composite material coated by ALD technology according to claim 3, characterized in that: In step (1), the action time is 60-65 s; and / or, in step (2), the temperature is raised to 60-350° C.; and / or, in step (3), the flow rate of the first inert carrier gas is 20-240 ml / min, and the duration is 55-65 s; and / or, the first inert carrier gas comprises one or more of helium, argon or xenon; and / or, in step (3), the vapor of the compound containing the metal element comprises one of trimethylzinc vapor, trimethylaluminum vapor, trimethyliron vapor, trimethyltitanium vapor, trimethyltungsten vapor, trimethylzirconium vapor, trimethylnickel and trimethylmanganese; And / or, in step (3), the volume flow ratio of the vapor of the compound containing the metal element to the first inert carrier gas is (5-40): (95-60); and / or, in step (4), the flow rate of the second inert carrier gas is 20-350 ml / min, and the blow-off time is 115-125 s; and / or, the second inert carrier gas comprises one or more of helium, argon or xenon; And / or, in step (5), the flow rate of ozone is 35-240 ml / min, and the duration is 55-65 s; And / or, in step (6), the flow rate of the third inert carrier gas is 20-350 ml / min, and the time of introduction is 115-125 s; And / or, the third inert carrier gas includes one or more of helium, argon or xenon.

5. The method for preparing the lithium nitride composite material coated by ALD technology according to claim 3, characterized in that: In step (2), the method for preparing the lithium nitride raw material comprises the following steps: S1: weighing metallic lithium and pre-treating it; S2: performing preliminary nitridation treatment on the pretreated metallic lithium; S3: Grinding the material obtained in step S2 and transferring it to a tube furnace for calcination to obtain an initial lithium nitride material; S4: ball-milling the initial lithium nitride material, sieving, and taking the sieve material to obtain a lithium nitride raw material, which is used as a raw material before ALD treatment.

6. The method for preparing a lithium nitride composite material coated by ALD technology according to claim 5, characterized in that: In step S1, the pretreatment is carried out in a nitrogen glove box to destroy the surface coating of the metallic lithium; Among them, metallic lithium includes one or more of lithium powder, lithium belt, lithium sheet, lithium ingot, lithium rope and lithium alloy.

7. The method for preparing a lithium nitride composite material coated by ALD technology according to claim 5, characterized in that: In step S2, the preliminary nitridation treatment refers to a nitridation reaction of metallic lithium in a glove box containing a protective atmosphere; The protective atmosphere is a mixed atmosphere of nitrogen and argon; the volume flow ratio of nitrogen to argon is (5-40): (95-60); The nitridation reaction time is 1-72h; the nitridation temperature is 20-30°C.

8. The method for preparing a lithium nitride composite material coated by ALD technology according to claim 5, characterized in that: In step S3, the grinding refers to grinding the material obtained in step S2 in a mortar for 20-40 minutes; And / or, in step S3, the protective atmosphere in the tubular furnace is nitrogen, the calcination temperature is 80-800° C., and the calcination time is 1-25 h.

9. The method for preparing a lithium nitride composite material coated by ALD technology according to claim 5, characterized in that: The decomposition potential of the lithium nitride raw material obtained in step S4 is 3.7-4.1V, and the purity is 97.1-99.4%; the mass ratio of α-Li3N and β-Li3N in the lithium nitride raw material is in the range of (97-90):(3-10); And / or, in step S4, the ball milling beads used in the ball milling process are zirconium oxide balls with a diameter of 0.1-20 mm; the ball-to-material ratio is (10-60):1; the ball milling atmosphere is a mixed atmosphere of nitrogen and argon, wherein the volume flow ratio of nitrogen to argon is (5-40):(95-60); the ball milling speed is 80-1200 rpm; the ball milling method is to work for 10 minutes, rest for 5 minutes, repeat the cycle 2-18 times, and the total ball milling time is 20-180 minutes; And / or, in step S4, sieving refers to sieving through a 150-600 mesh sieve.

10. An application of an ALD-coated lithium nitride composite material prepared by the ALD-coated lithium nitride composite material according to any one of claims 1 to 2 or the method for preparing an ALD-coated lithium nitride composite material according to any one of claims 3 to 9, characterized in that: As a lithium supplement additive for lithium-ion battery positive electrode.

Citation Information

Patent Citations

  • Preparation method of positive electrode active material for secondary battery

    CN114762148A

  • Lithium supplement additive for core-shell positive electrode as well as preparation method and application of lithium supplement additive

    CN115692698A

  • Preparation method and application of atomic layer deposition technology modified metal oxide positive electrode

    CN116377423A

  • Positive electrode lithium supplementing material and preparation method and application thereof

    CN116525823A

  • Preparation method of lithium nitride

    CN117486175A

Cited By

  • Composite lithium supplementing material, lithium supplementing positive electrode and lithium ion battery

    CN119361710A

  • Modified ternary lithium electrode material and preparation method and application thereof

    CN120589806A