Sodium supplementing material and preparation method thereof, positive pole piece, diaphragm, electrode assembly, battery monomer, battery and electric device

By using sodium supplementary materials, doping and carbon coatings with chemical formula NaxM1-yNyOz in sodium secondary batteries, the problem of sodium loss in sodium secondary batteries is solved, the performance and stability of the battery are improved, and production is simplified process.

CN118943351AActive Publication Date: 2024-11-12CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
CN202310524096.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12
Estimated Expiration
2043-05-10

AI Technical Summary

Technical Problem

There is a problem of sodium loss during the circulation of sodium secondary batteries, resulting in poor battery performance.

Method used

The chemical formula of sodium supplementing material is NaxM1-yNyOz, where M and N include semiconductor elements, alkaline earth metal elements, and transition metal elements. The conductivity and catalytic activity are improved through doping and carbon coating, supplement sodium ions, and improve sodium secondary Battery performance.

Benefits of technology

Effectively supplement sodium ions, improve the circulation capacity retention rate and electrochemical performance of sodium secondary batteries, enhance the stability and safety of the battery, simplify the preparation process, and facilitate industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943351A_ABST
    Figure CN118943351A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to a sodium supplementing material and a preparation method thereof, a positive pole piece, a diaphragm, an electrode assembly, a battery monomer, a battery and an electric device. The chemical formula of the sodium supplementing material is NaxM1-yNyOz, and M comprises at least one of a semiconductor element, an alkaline earth metal element and a transition metal element; n comprises at least one of semiconductor elements, alkaline earth metal elements and transition metal elements, x is larger than or equal to 1 and smaller than or equal to 4, y is larger than or equal to 0 and smaller than or equal to 0.25, and z is larger than or equal to 2.5 and smaller than or equal to 4. Comprising the chemical formula can supplement sodium loss in the sodium secondary battery and improve the performance of the sodium secondary battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a sodium supplement material and a preparation method thereof, a positive electrode sheet, a diaphragm, an electrode assembly, a battery cell, a battery and an electrical device. Background Art

[0002] Sodium secondary batteries have great development prospects in the field of large-scale energy storage due to their abundant sodium reserves.

[0003] There is a problem of sodium loss during the cycle of sodium secondary batteries. Summary of the invention

[0004] The main purpose of the present invention is to provide a sodium supplement material, aiming to improve the performance of sodium secondary batteries.

[0005] To achieve the above object, the present invention provides a sodium supplement material, the chemical formula of which is Na x M 1- y N y O z , wherein M includes at least one of semiconductor elements, alkaline earth metal elements, and transition metal elements; N includes at least one of semiconductor elements, alkaline earth metal elements, and transition metal elements, wherein the range value of x is 1≤x≤4, the range value of y is 0≤y≤0.25, and the range value of z is 2.5≤z≤4.

[0006] The sodium supplement material including the above chemical formula can supplement the sodium loss in the sodium secondary battery and improve the performance of the sodium secondary battery. When y is greater than zero, the sodium supplement material is a metal sodium salt doped with multiple elements, and the sodium supplement performance is better. For example, doping with metal elements can increase the conductivity and catalytic activation of the electrochemical activity of the sodium supplement agent. The chemical formula of the sodium supplement material is Na x M 1-y N y O z , the range of x is 1≤x≤4, the range of y is 0≤y≤0.25, and the range of z is 2.5≤z≤4. The chemical formula of the sodium supplement material satisfies the above range, and the sodium supplement performance is better.

[0007] Optionally, the M includes Si, and the chemical formula of the sodium supplement material is Na4Si 1-y N y O4, wherein N includes at least one of an alkaline earth metal element and a transition metal element.

[0008] M includes Si, and the chemical formula of the sodium supplement material is Na4Si 1-y N yO4, the sodium supplement material is a metal-doped sodium silicate material, that is, the sodium supplement material includes a sodium silicate framework and a metal element embedded in the sodium silicate particles to replace part of the silicon element, wherein the doping method is chemical doping, and it can be understood that a coordination bond is formed between the metal doped in the chemical doping and the oxygen. The sodium silicate material doped with metal chemistry can improve the conductivity and stability of sodium silicate, and can also catalytically activate the electrochemical properties of sodium silicate, and promote its better release of charge and discharge capacity. It can also be understood that silicon is not only abundant in nature compared to other semiconductor elements, but also the sodium supplement process is more stable and not easy to produce secondary products. The sodium supplement material of the present application has stability and safety, that is, in the process of releasing sodium ions from the sodium supplement material, the structure of the sodium supplement material is stable and it is difficult to collapse, which improves the problem of the sodium supplement material decomposing and producing gas and harmful substances during the sodium supplement process.

[0009] Optionally, 0.01<y≤0.25.

[0010] In order to improve the sodium supplement material to have better conductivity and stability, 0.01<y≤0.25. It is understood that the value of y in the above range can improve the problem of insufficient conductivity of the sodium supplement material due to the metal element replacing less silicon element, and improve the problem of metal element dissolution and reduced battery performance during the charge and discharge cycle due to the metal element replacing more silicon element. It is understood that the dissolution of metal elements may cause the metal catalyzed electrolyte decomposition in some cases. It is also understood that excessive metal element doping to replace silicon may also reduce the stability of the sodium supplement.

[0011] Optionally, the semiconductor element includes at least one of Si, Ge, Se, and Te;

[0012] And / or, the alkaline earth metal element includes at least one of Be, Mg, Ca, Sr and Ba;

[0013] And / or, the transition metal element includes at least one of iron Fe, Ni, Ti, Co, Mo, and Nb.

[0014] It is understandable that semiconductor elements include but are not limited to at least one of Si, Ge, Se, and Te; alkaline earth metal elements include but are not limited to at least one of Be, Mg, Ca, Sr, and Ba; and transition metal elements include but are not limited to at least one of Fe, Ni, Ti, Co, Mo, and Nb.

[0015] Optionally, the volume average particle size Dv50 of the sodium supplementing material is in the range of 0.5 μm to 10 μm, preferably, 1 μm to 5 μm.

[0016] The volume average particle size Dv50 of the sodium supplement material is within the above range, which improves the filtration performance when preparing the sodium supplement slurry, improves the coating performance, and improves the problem that large particles of sodium supplement material are coated on the electrode, reducing the cycle performance during the charge and discharge process.

[0017] Optionally, a carbon coating layer is provided on the surface of the sodium supplement material.

[0018] The surface of the sodium-supplementing material is provided with a carbon coating layer, which can improve the electrical contact between particles, promote the escape of sodium ions, and improve the electrochemical performance of the sodium battery material.

[0019] Optionally, the carbon coating layer includes at least one of graphite, carbon nanotubes, carbon nanofibers, carbon black and graphene;

[0020] And / or, the thickness of the carbon coating layer is 10 nm to 5000 nm, preferably 10 nm to 500 nm;

[0021] And / or, the carbon coating layer completely covers the surface of the sodium supplementing material.

[0022] The carbon coating layer coated on the surface of the sodium supplementing material includes but is not limited to at least one of graphite, carbon nanotubes, carbon nanofibers, carbon black and graphene.

[0023] In order to improve the release of sodium ions, the thickness of the carbon coating layer is 10 nm to 5000 nm, preferably 10 nm to 500 nm.

[0024] Theoretically, there is no limitation on how the carbon coating layer is disposed on the surface of the sodium supplementing material. For example, the carbon coating layer may be disposed discontinuously on the surface of the sodium supplementing material. For example, the carbon coating layer includes multiple shells, and the multiple shells are discontinuously disposed on the surface of the sodium supplementing material. In order to improve the electrical contact of the sodium supplementing material and improve the problem of direct contact between the sodium supplementing material and the electrolyte to produce by-products, it is preferred that the carbon coating layer fully coats the surface of the sodium supplementing material.

[0025] The present application also provides a method for preparing a sodium supplement material, comprising:

[0026] Mixing a sodium source, an M element source, and an N element source to prepare a precursor;

[0027] The precursor is sintered in an inert atmosphere to obtain the sodium supplement material.

[0028] A sodium source, an M element source, and an N element source are mixed to obtain a precursor, and the precursor is sintered in an inert atmosphere to obtain a sodium supplement material. Wherein, M includes at least one of a semiconductor element, an alkaline earth metal element, and a transition metal element; N includes at least one of a semiconductor element, an alkaline earth metal element, and a transition metal element, and M and N are different elements. By the above preparation method, a sodium supplement material can be obtained, and the chemical formula is Nax M 1-y N y O z .

[0029] The present application also provides a method for preparing a sodium supplement material, comprising:

[0030] Mixing a sodium source, an M element source, and an N element source to prepare a precursor;

[0031] The precursor is placed in an organic gaseous carbon source atmosphere and sintered to obtain the sodium supplement material.

[0032] A sodium source, an M element source, and an N element source are mixed to obtain a precursor, and the precursor is placed in an organic gaseous carbon source atmosphere for sintering to obtain a sodium supplementing material. A gaseous carbon source is introduced during the sintering process to coat a carbon layer on the surface of the sodium supplementing material formed by sintering by chemical vapor deposition. In addition to acting as a coating layer, the organic carbon source also acts as a loosening agent during the preparation of the sodium supplementing material, which can reduce the phenomenon of particle agglomeration during the sintering process. It is understandable that carbon is mixed between the inorganic particles, so that a heterogeneous interface is formed between the inorganic particles, which improves the problem of particle agglomeration during the sintering process. After the particles are coated with carbon, the particles are not easily bonded together again due to the nature of the carbon itself, thereby improving the agglomeration phenomenon.

[0033] The sodium supplement material of the present application has a stable structure, is safe to use during the sodium supplement process, has a simple preparation method, and is convenient for industrial production. Moreover, the sodium supplement material is easy to add to the sodium secondary battery, and there is no requirement for upgrading or improving the existing sodium secondary battery production process.

[0034] It can be understood that the M element source includes a silicon source, and the sodium source, the silicon source and the N element source are mixed to prepare a precursor, wherein N includes at least one of a semiconductor element, an alkaline earth metal element and a transition metal element. The chemical formula of the sodium supplement material prepared by the above method is Na4Si 1-y N y O4, sodium supplement materials include metal-doped sodium silicate materials. The metal-chemically doped sodium silicate materials can improve the conductivity and stability of sodium silicate, and can also catalytically activate the electrochemical properties of sodium silicate, promoting it to better release the charge and discharge capacity.

[0035] Optionally, the step of mixing the sodium source, the M element source, and the N element source to prepare the precursor includes:

[0036] A sodium source, an M element source, a solid carbon source and a N element source are mixed to prepare a precursor.

[0037] The present application adds a solid carbon source to the precursor to obtain a sodium-supplemented material by sintering in an inert atmosphere. In the preparation process of the sodium-supplemented material, the carbon source not only acts as a coating layer, but also acts as a loosening agent, which can reduce the phenomenon of particle agglomeration during the sintering process.

[0038] Optionally, in the step of mixing the sodium source, the M element source, and the N element source to prepare the precursor, the mixing step includes at least one of ball milling, grinding, or stirring;

[0039] In the step of sintering the precursor, the sintering temperature is 500° C. to 1000° C., and the sintering time is 3 hours to 10 hours.

[0040] The precursor raw materials are mixed uniformly by ball milling, grinding or stirring, and the sodium supplement material is obtained by sintering at a temperature of 500° C. to 1000° C. and a sintering time of 3 h to 10 h. It is understood that the sodium supplement material obtained by sintering can be in block form, and the block material is crushed into a material of a suitable size by crushing.

[0041] Optionally, the sodium source includes one or more of sodium hydroxide, sodium nitrate, sodium carbonate, sodium acetate, and sodium sulfate;

[0042] And / or, the M element source includes a silicon source, and the silicon source includes one or more of silicon, silicon monoxide, and silicon dioxide;

[0043] And / or, the N element source includes one or more of magnesium, iron, nickel, ferroferric oxide, titanium dioxide, cobalt oxide, cobalt acetate, cobalt sulfide, molybdenum oxide, niobium oxide, nickel acetate, nickel sulfate, nickel oxide, manganese dioxide and molybdenum dioxide;

[0044] And / or, the M element source includes a silicon source, and the volume average particle size Dv50 of the silicon source includes 50 nm to 20 μm, preferably, 500 nm to 10 μm;

[0045] And / or, the M element source includes a silicon source, and the molar ratio of Na in the sodium source to Si in the silicon source includes (2-4.5):1;

[0046] And / or, the M element source includes a silicon source, and the molar ratio of Si in the silicon source to N element in the N element source includes (3-99):1.

[0047] In the present application, the sodium source includes but is not limited to one or more of sodium hydroxide, sodium nitrate, sodium carbonate, sodium acetate, and sodium sulfate. The silicon source includes but is not limited to one or more of silicon, silicon dioxide, and silicon oxide. The N element source includes but is not limited to one or more of magnesium, iron, nickel, ferroferric oxide, titanium dioxide, cobalt oxide, cobalt acetate, cobalt sulfide, molybdenum oxide, niobium oxide, nickel acetate, nickel sulfate, and nickel oxide.

[0048] In the present application, in order to make the Dv50 of the prepared sodium supplement material in the range of 1 μm to 5 μm, the volume average particle size Dv50 of the silicon source includes 50 nm to 20 μm, preferably, 500 nm to 10 μm.

[0049] In order to make the chemical formula of the prepared sodium supplement material satisfy Na4Si 1-y N y O4, the molar ratio of Na in the sodium source to Si in the silicon source includes (2-4.5):1.

[0050] In order to chemically dope an appropriate amount of metal elements into sodium silicate, improve the problem of insufficient conductivity of the sodium supplement material due to the metal elements replacing a small amount of silicon elements, and improve the problem of metal elements dissolving during the charge and discharge cycle and reducing battery performance due to the metal elements replacing a large amount of silicon elements, the molar ratio of Si in the silicon source to the N element in the N element source includes (3-99):1.

[0051] Optionally, the solid carbon source includes a solid organic carbon source and / or a solid inorganic carbon source.

[0052] The solid carbon source in the present application includes a solid organic carbon source and / or a solid inorganic carbon source.

[0053] Optionally, the solid organic carbon source includes at least one of an organic polymer and a carbohydrate compound;

[0054] And / or, the solid inorganic carbon source includes at least one of graphite and carbon black.

[0055] The solid organic carbon source in the present application includes but is not limited to at least one of organic polymers and sugar compounds. The solid inorganic carbon source in the present application includes but is not limited to at least one of graphite and carbon black.

[0056] Optionally, the solid organic carbon source comprises an organic polymer, and the organic polymer comprises one or more of polyethylene, polypropylene, polystyrene, polyvinyl pyrrolidone, and phenolic resin;

[0057] And / or, the solid organic carbon source includes sugar compounds, and the sugar compounds include one or more of glucose, sucrose, citric acid, asphalt, polyvinyl pyrrolidone, cellulose, and starch.

[0058] The organic polymer includes, but is not limited to, one or more of polyethylene, polypropylene, polystyrene, polyvinyl pyrrolidone, and phenolic resin.

[0059] The carbohydrate compound includes, but is not limited to, one or more of glucose, sucrose, citric acid, asphalt, polyvinyl pyrrolidone, cellulose, and starch.

[0060] Optionally, the inert atmosphere includes at least one of nitrogen and argon;

[0061] And / or, the M element source includes a silicon source, and the mass ratio of the solid carbon source to the silicon source ranges from 10% to 40%, preferably, from 15% to 30%.

[0062] In the process of sintering the precursor under an inert atmosphere to obtain the sodium supplement material, the inert atmosphere includes at least one of nitrogen and argon.

[0063] In order to make the thickness of the carbon coating layer in the range of 10 nm to 5000 nm, the mass ratio of the solid carbon source to the silicon source is in the range of 10% to 40%, preferably, 15% to 30%.

[0064] Optionally, the organic gaseous carbon source includes at least one of alkanes and alkenes;

[0065] Preferably, the organic gaseous carbon source includes one or more of methane, ethylene, and acetylene;

[0066] The organic gaseous carbon source in the present application includes but is not limited to at least one of alkanes and alkenes.

[0067] The organic gaseous carbon source includes, but is not limited to, one or more of methane, ethylene, and acetylene.

[0068] Optionally, the purity of the organic gaseous carbon source is 90% to 100%, preferably, 95% to 100%;

[0069] And / or, the flow rate of the organic gaseous carbon source is 30 ml / min to 100 ml / min, preferably 60 ml / min to 100 ml / min.

[0070] An organic gaseous carbon source is introduced as a sintering atmosphere, and the purity of the organic gaseous carbon source is 90% to 100%, preferably, 95% to 100%.

[0071] The thickness of the carbon layer is controlled within the range of 10 nm to 5000 nm, and the flow rate of the introduced gas is controlled to meet the flow rate of the organic gaseous carbon source within the range of 30 ml / min to 100 ml / min, preferably 60 ml / min to 100 ml / min.

[0072] The present application also provides a positive electrode plate, the positive electrode plate comprising the sodium supplement material as described above;

[0073] Alternatively, the sodium-supplementing material comprises the sodium-supplementing material obtained by the preparation method of the sodium-supplementing material.

[0074] Optionally, the positive electrode plate includes a current collector and a coating arranged on at least one side of the current collector, the coating includes the sodium-supplementing material, and the mass of the sodium-supplementing material accounts for a range of greater than 0% and less than or equal to 5% of the mass of the coating, preferably 1% to 3%.

[0075] In order to improve the sodium supplementation effect and to solve the problem that too much sodium supplementation material will affect the energy density, the mass of the sodium supplementation material accounts for a range of greater than 0% and less than or equal to 5% of the coating mass, preferably, 1% to 3%.

[0076] The present application also provides a diaphragm, the diaphragm comprising the sodium supplement material as described;

[0077] Alternatively, the sodium-supplementing material comprises the sodium-supplementing material obtained by the preparation method of the sodium-supplementing material.

[0078] Optionally, the diaphragm includes a base film and a sodium-compensating layer disposed on at least one side of the base film, the sodium-compensating layer includes the sodium-compensating material, and the thickness of the sodium-compensating layer is greater than 0 μm and less than or equal to 10 μm, preferably 3 μm to 6 μm.

[0079] In order to improve the problem that the sodium supplement layer is too thin and the amount of sodium supplement is small, and the sodium supplement layer is too thick and affects the performance of the diaphragm, the thickness of the sodium supplement layer is greater than 0μm and less than or equal to 10μm, preferably, 3μm to 6μm.

[0080] The present application also provides an electrode assembly, which includes the positive electrode plate as described above, or includes the separator as described above.

[0081] The present application also provides a battery cell, which includes the electrode assembly as described above.

[0082] The present application also provides a battery, which includes the battery cell as described above.

[0083] The present application also provides an electrical device, which includes the battery cell or the battery as described above.

[0084] The sodium supplement material of the present application has the chemical formula Na x M 1-y N y O z, wherein M includes at least one of semiconductor elements, alkaline earth metal elements, and transition metal elements; N includes at least one of semiconductor elements, alkaline earth metal elements, and transition metal elements, wherein the range of x is 1≤x≤4, the range of y is 0≤y≤0.25, and the range of z is 2.5≤z≤4. The inorganic sodium supplement material including the above chemical formula can supplement the sodium loss in the sodium secondary battery and improve the performance of the sodium secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0085] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0086] Figure 1 This is a scanning electron microscope image of the sodium supplement material of Example 1 of the present application;

[0087] Figure 2 A schematic diagram of the structure of a positive electrode sheet according to an embodiment of the present application;

[0088] Figure 3 This is a schematic diagram of the structure of a diaphragm according to an embodiment of the present application;

[0089] Figure 4 A schematic diagram of a method for preparing a sodium supplement material according to an embodiment of the present application;

[0090] Figure 5 is a schematic diagram of a secondary battery according to an embodiment of the present application;

[0091] Figure 6 yes Figure 5 An exploded view of a secondary battery according to an embodiment of the present application is shown;

[0092] Figure 7 is a schematic diagram of a battery module according to an embodiment of the present application;

[0093] Figure 8 is a schematic diagram of a battery pack according to an embodiment of the present application;

[0094] Fig. 9 yes Figure 8 An exploded view of a battery pack according to an embodiment of the present application is shown;

[0095] Fig.10 FIG. 1 is a schematic diagram of an electric device using a secondary battery according to an embodiment of the present application as a power source.

[0096] Description of Figure Numbers:

[0097] Label name Label name 100 Positive electrode 2 Upper box 110 current collector 3 Lower box 120 First coating 4 Battery Module 130 Second coating 5 Secondary battery 200 Diaphragm 51 case 210 Basement membrane 52 Electrode assembly 220 Sodium supplementation layer 53 Top cover assembly 1 Battery Pack

[0098] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0099] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0100] Hereinafter, the embodiments of the positive electrode sheet, separator, electrode assembly, battery cell, battery and electrical device of the present application will be specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0101] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0102] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0103] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0104] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0105] Compared with lithium secondary batteries with scarce elements such as lithium, cobalt and nickel, sodium secondary batteries have the advantages of abundant sodium resources and low raw material costs, which makes sodium secondary batteries have great development prospects in the field of energy storage.

[0106] There is a problem of sodium loss during the cycle of sodium secondary batteries.

[0107] For example, due to some irreversible reactions such as the formation of the solid electrolyte film (SEI film) on the negative electrode surface during the initial charge and discharge process, the positive electrode material will experience sodium ion loss, resulting in low initial coulombic efficiency and energy density of the sodium ion battery.

[0108] In order to solve the above technical problems, the present application provides a sodium supplement material, aiming to improve the performance of sodium secondary batteries.

[0109] The chemical formula of the sodium supplement material is Na x M 1-y N y O z , wherein M includes at least one of semiconductor elements, alkaline earth metal elements, and transition metal elements; N includes at least one of semiconductor elements, alkaline earth metal elements, and transition metal elements, wherein 1≤x≤4, the range value of y is 0≤y≤0.25, and the range value of z is 2.5≤z≤4.

[0110] Sodium replenishing materials, including compounds containing sodium elements, can replenish the sodium lost in the positive electrode in sodium secondary batteries.

[0111] The sodium supplement material including the above chemical formula can supplement the sodium loss in the sodium secondary battery and improve the performance of the sodium secondary battery. When y is greater than zero, the sodium supplement material is a metal sodium salt doped with multiple elements, and the sodium supplement performance is better. For example, doping with metal elements can increase the conductivity and catalytic activation of the electrochemical activity of the sodium supplement agent. The chemical formula of the sodium supplement material is Nax M 1-y N y O z , the range of x is 1≤x≤4, the range of y is 0≤y≤0.25, and the range of z is 2.5≤z≤4. The chemical formula of the sodium supplement material satisfies the above range, and the sodium supplement performance is better.

[0112] In the above 1≤x≤4, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1, 2, 3, 4, etc., and the range values ​​between any two of the above point values.

[0113] In the above 0≤y≤0.25, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 0, 0.005, 0.01, 0.015, 0.02, 0.05, 0.08, 0.1, 0.12, 0.15, 0.16, 0.18, 0.2, 0.22, 0.24, 0.25, etc., and the range values ​​between any two of the above point values.

[0114] In the above 2.5≤z≤4, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 2.5, 2.7, 2.9, 3, 3.2, 3.4, 3.6, 3.8, 4, etc., and the range values ​​between any two of the above point values.

[0115] In one embodiment, M includes Si, and the chemical formula of the sodium supplement material is Na4Si 1-y N y O4, wherein N includes at least one of an alkaline earth metal element and a transition metal element.

[0116] M includes Si, and the chemical formula of the sodium supplement material is Na4Si 1-y N yO4, the sodium supplement material is a metal-doped sodium silicate material, that is, the sodium supplement material includes a sodium silicate framework and a metal element embedded in the sodium silicate particles to replace part of the silicon element, wherein the doping method is chemical doping, and it can be understood that a coordination bond is formed between the metal doped in the chemical doping and the oxygen. The sodium silicate material doped with metal chemistry can improve the conductivity and stability of sodium silicate, and can also catalytically activate the electrochemical properties of sodium silicate, and promote its better release of charge and discharge capacity. It can also be understood that silicon is not only abundant in nature compared to other semiconductor elements, but also the sodium supplement process is more stable and not easy to produce secondary products. The sodium supplement material of the present application has stability and safety, that is, in the process of releasing sodium ions from the sodium supplement material, the structure of the sodium supplement material is stable and it is difficult to collapse, which improves the problem of the sodium supplement material decomposing and producing gas and harmful substances during the sodium supplement process.

[0117] In one embodiment, 0.01<y≤0.25.

[0118] In order to improve the sodium supplement material to have better conductivity and stability, 0.01<y≤0.25. It is understood that the value of y in the above range can improve the problem of insufficient conductivity of the sodium supplement material due to the metal element replacing less silicon element, and improve the problem of metal element dissolution and reduced battery performance during the charge and discharge cycle due to the metal element replacing more silicon element. It is understood that the dissolution of metal elements may cause the metal catalyzed electrolyte decomposition in some cases. It is also understood that excessive metal element doping to replace silicon may also reduce the stability of the sodium supplement.

[0119] In the above 0.01<y≤0.25, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 0.011, 0.02, 0.05, 0.08, 0.1, 0.12, 0.15, 0.18, 0.2, 0.21, 0.22, 0.24, 0.25, etc., and the range values ​​between any two of the above point values.

[0120] In one embodiment, the semiconductor element includes at least one of Si, Ge, Se, and Te; and / or the alkaline earth metal element includes at least one of Be, Mg, Ca, Sr, and Ba; and / or the transition metal element includes at least one of iron Fe, Ni, Ti, Co, Mo, and Nb.

[0121] It is understandable that semiconductor elements include but are not limited to at least one of Si, Ge, Se, and Te; alkaline earth metal elements include but are not limited to at least one of Be, Mg, Ca, Sr, and Ba; and transition metal elements include but are not limited to at least one of Fe, Ni, Ti, Co, Mo, and Nb.

[0122] In one embodiment, the volume average particle size Dv50 of the sodium supplement material is in the range of 0.5 μm to 10 μm, preferably, 1 μm to 5 μm.

[0123] Dv50: Among the sample particles, 50% of the total volume of the particles have a particle size larger than this value, and another 50% of the total volume of the particles have a particle size smaller than this value; Dv50 can represent the median particle size of the sample.

[0124] The volume average particle size Dv50 can be tested by a method known in the art. For example, GB / T 19077-2016 can be referred to, and a Malvern laser particle size analyzer can be used for characterization testing, such as a Malvern Mastersizer-3000 or other instrument.

[0125] The volume average particle size Dv50 of the sodium supplement material is within the above range, which improves the filtration performance when preparing the sodium supplement slurry, improves the coating performance, and improves the problem that large particles of sodium supplement material are coated on the electrode, reducing the cycle performance during the charge and discharge process.

[0126] In the above-mentioned 0.5μm to 10μm, the values ​​include the minimum and maximum values ​​of the range, and every value between such minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 0.5μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 5.5μm, 6μm, 6.5μm, 7μm, 7.5μm, 8μm, 8.5μm, 9μm, 9.5μm, 10μm, etc., and the range value between any two of the above-mentioned point values.

[0127] In the above-mentioned 1μm to 5μm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, etc., as well as the range values ​​between any two of the above-mentioned point values.

[0128] In one embodiment, a carbon coating layer is provided on the surface of the sodium supplementing material.

[0129] The surface of the sodium-supplementing material is provided with a carbon coating layer, which means that the carbon material is arranged on the surface of the sodium-supplementing material. The carbon coating layer can improve the electrical contact between particles, promote the release of sodium ions, and improve the electrochemical performance of the sodium battery material.

[0130] In one embodiment, the carbon coating layer includes at least one of graphite, carbon nanotubes, carbon nanofibers, carbon black and graphene; and / or the thickness of the carbon coating layer is 10nm to 5000nm, preferably 10nm to 500nm; and / or the carbon coating layer is fully coated on the surface of the sodium supplement material.

[0131] The carbon coating layer coated on the surface of the sodium supplementing material includes but is not limited to at least one of graphite, carbon nanotubes, carbon nanofibers, carbon black and graphene.

[0132] In order to improve the release of sodium ions, the thickness of the carbon coating layer is 10 nm to 5000 nm, preferably 10 nm to 500 nm.

[0133] Theoretically, there is no limitation on how the carbon coating layer is disposed on the surface of the sodium supplementing material. For example, the carbon coating layer may be disposed discontinuously on the surface of the sodium supplementing material. For example, the carbon coating layer includes multiple shells, and the multiple shells are discontinuously disposed on the surface of the sodium supplementing material. In order to improve the electrical contact of the sodium supplementing material and improve the problem of direct contact between the sodium supplementing material and the electrolyte to produce by-products, it is preferred that the carbon coating layer fully coats the surface of the sodium supplementing material.

[0134] In the above-mentioned 10nm to 5000nm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 10nm, 50nm, 100nm, 150nm, 200nm, 350nm, 400nm, 650nm, 800nm, 1000nm, 2000nm, 3000nm, 4000nm, 5000nm, etc., and the range values ​​between any two of the above-mentioned point values.

[0135] In the above 10nm to 500nm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 10nm, 50nm, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm, 500nm, etc., and the range values ​​between any two of the above point values.

[0136] In one embodiment, the present application also provides a method for preparing a sodium-supplementing material, comprising: mixing a sodium source, an M element source, and an N element source to obtain a precursor; and sintering the precursor under an inert atmosphere to obtain the sodium-supplementing material.

[0137] The M element source refers to a compound including the M element. For example, if the M element includes silicon, iron, etc., then the M element source includes silicon dioxide, ferrosoferric oxide, etc.

[0138] The N element source refers to a compound including the N element. For example, if the N element includes cobalt, iron, etc., the N element source includes cobalt oxide, ferrosoferric oxide, etc.

[0139] like Figure 4 As shown in the figure, it is a schematic flow chart of the preparation method of the sodium supplement material. A sodium source, an M element source, and an N element source are mixed to obtain a precursor, and the precursor is sintered under an inert atmosphere to obtain the sodium supplement material. Among them, M includes at least one of a semiconductor element, an alkaline earth metal element, and a transition metal element; N includes at least one of a semiconductor element, an alkaline earth metal element, and a transition metal element, and M and N are different elements. By the above preparation method, a sodium supplement material can be obtained, and the chemical formula is Na x M 1-y N y O z .

[0140] In one embodiment, the present application also provides a method for preparing a sodium-supplementing material, comprising: mixing a sodium source, an M element source, and an N element source to obtain a precursor; and sintering the precursor in an organic gaseous carbon source atmosphere to obtain a sodium-supplementing material.

[0141] Organic gaseous carbon source, a carbon-containing organic compound in gaseous state.

[0142] A sodium source, an M element source, and an N element source are mixed to obtain a precursor, and the precursor is placed in an organic gaseous carbon source atmosphere for sintering to obtain a sodium supplementing material. A gaseous carbon source is introduced during the sintering process to coat a carbon layer on the surface of the sodium supplementing material formed by sintering by chemical vapor deposition. In addition to acting as a coating layer, the organic carbon source also acts as a loosening agent during the preparation of the sodium supplementing material, which can reduce the phenomenon of particle agglomeration during the sintering process. It is understandable that carbon is mixed between the inorganic particles, so that a heterogeneous interface is formed between the inorganic particles, which improves the problem of particle agglomeration during the sintering process. After the particles are coated with carbon, the particles are not easily bonded together again due to the nature of the carbon itself, thereby improving the agglomeration phenomenon.

[0143] The sodium supplement material of the present application has a stable structure, is safe to use during the sodium supplement process, has a simple preparation method, and is convenient for industrial production. Moreover, the sodium supplement material is easy to add to the sodium secondary battery, and there is no requirement for upgrading or improving the existing sodium secondary battery production process.

[0144] In one embodiment, the step of mixing a sodium source, an M element source, and an N element source to obtain a precursor includes: mixing a sodium source, a silicon source, and an N element source to obtain a precursor.

[0145] That is, the M element source includes a silicon source, and the sodium source, the silicon source and the N element source are mixed to prepare a precursor, wherein N includes at least one of a semiconductor element, an alkaline earth metal element and a transition metal element. The chemical formula of the sodium supplement material prepared by the above method is Na4Si1-y N y O4, sodium supplement materials include metal-doped sodium silicate materials. The metal-chemically doped sodium silicate materials can improve the conductivity and stability of sodium silicate, and can also catalytically activate the electrochemical properties of sodium silicate, promoting it to better release the charge and discharge capacity.

[0146] In one embodiment, the step of mixing a sodium source, an M element source, and an N element source to obtain a precursor includes: mixing a sodium source, an M element source, a solid carbon source, and an N element source to obtain a precursor.

[0147] Solid carbon source is a carbon-containing compound material in a solid state, including, for example, graphite, polyethylene, polypropylene, etc.

[0148] The present application adds a solid carbon source to the precursor to obtain a sodium-supplemented material by sintering in an inert atmosphere. In the preparation process of the sodium-supplemented material, the carbon source not only acts as a coating layer, but also acts as a loosening agent, which can reduce the phenomenon of particle agglomeration during the sintering process.

[0149] In one embodiment, in the step of mixing a sodium source, an M element source, and an N element source to obtain a precursor, the mixing step includes at least one of ball milling mixing, grinding mixing, or stirring mixing; in the step of sintering the precursor, the sintering temperature is 500°C to 1000°C, and the sintering time is 3h to 10h.

[0150] The precursor raw materials are mixed uniformly by ball milling, grinding or stirring, and the sodium supplement material is obtained by sintering at a temperature of 500° C. to 1000° C. and a sintering time of 3 h to 10 h. It is understood that the sodium supplement material obtained by sintering can be in block form, and the block material is crushed into a material of a suitable size by crushing.

[0151] In the above 500°C to 1000°C, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, etc., as well as the range values ​​between any two of the above point values.

[0152] In the above 3h to 10h, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, etc., and the range values ​​between any two of the above point values.

[0153] In one embodiment, the sodium source includes one or more of sodium hydroxide, sodium nitrate, sodium carbonate, sodium acetate, and sodium sulfate; and / or, the M element source includes a silicon source, and the silicon source includes one or more of silicon, silicon monoxide, and silicon dioxide; and / or, the N element source includes one or more of magnesium element, iron element, nickel element, ferroferric oxide, titanium dioxide, cobalt oxide, cobalt acetate, cobalt sulfide, molybdenum oxide, niobium oxide, nickel acetate, nickel sulfate, and nickel oxide.

[0154] In the present application, the sodium source includes but is not limited to one or more of sodium hydroxide, sodium nitrate, sodium carbonate, sodium acetate, and sodium sulfate. The silicon source includes but is not limited to one or more of silicon, silicon dioxide, and silicon oxide. The N element source includes but is not limited to one or more of magnesium, iron, nickel, ferroferric oxide, titanium dioxide, cobalt oxide, cobalt acetate, cobalt sulfide, molybdenum oxide, niobium oxide, nickel acetate, nickel sulfate, nickel oxide, manganese dioxide, and molybdenum dioxide.

[0155] In one embodiment, the volume average particle size Dv50 of the silicon source is 50 nm to 20 μm, preferably, 500 nm to 10 μm.

[0156] In the present application, in order to make the Dv50 of the prepared sodium supplement material in the range of 0.5 μm to 10 μm, the volume average particle size Dv50 of the silicon source includes 50 nm to 20 μm, preferably, 500 nm to 10 μm.

[0157] In the above-mentioned 50nm to 20μm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 50nm, 70nm, 90nm, 100nm, 500nm, 1μm, 5μm, 10μm, 15μm, 20μm, etc., as well as the range values ​​between any two of the above-mentioned point values.

[0158] In the above 500nm to 10μm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 500nm, 700nm, 1μm, 3nm, 5μm, 8nm, 10μm, etc., as well as the range values ​​between any two of the above point values.

[0159] In one embodiment, the M element source includes a silicon source, and the molar ratio of Na in the sodium source to Si in the silicon source includes (2-4.5):1; and / or, the M element source includes a silicon source, and the molar ratio of Si in the silicon source to N in the N element source includes (3-99):1.

[0160] The testing method of molar ratio is as follows: during the preparation of sodium supplemented materials, various raw materials used to prepare precursors input during the reaction are recorded, wherein the molar number of various raw materials is equal to the mass of various raw materials divided by the molecular weight of various raw materials. The molar number of Na in the sodium source is defined as a, the molar number of Si in the silicon source is defined as b, and the molar number of N element in the N element source is defined as c. Then, the molar ratio of Na to Si is a:b, and the molar ratio of Si to N element is b:c.

[0161] In order to make the chemical formula of the prepared sodium supplement material satisfy Na4Si 1-y N y O4, the molar ratio of Na in the sodium source to Si in the silicon source includes (2-4.5):1.

[0162] In order to chemically dope an appropriate amount of metal elements into sodium silicate, improve the problem of insufficient conductivity of the sodium supplement material due to the metal elements replacing a small amount of silicon elements, and improve the problem of metal elements dissolving during the charge and discharge cycle and reducing battery performance due to the metal elements replacing a large amount of silicon elements, the molar ratio of Si in the silicon source to N in the N element source includes (3-99):1.

[0163] In one embodiment, the solid carbon source includes a solid organic carbon source and / or a solid inorganic carbon source.

[0164] The solid carbon source in the present application includes a solid organic carbon source and / or a solid inorganic carbon source.

[0165] In one embodiment, the solid organic carbon source includes at least one of an organic polymer and a carbohydrate compound; and / or the solid inorganic carbon source includes at least one of graphite and carbon black.

[0166] The solid organic carbon source in the present application includes but is not limited to at least one of organic polymers and sugar compounds. The solid inorganic carbon source in the present application includes but is not limited to at least one of graphite and carbon black.

[0167] In one embodiment, the solid organic carbon source includes an organic polymer, which includes one or more of polyethylene, polypropylene, polystyrene, polyvinyl pyrrolidone, and phenolic resin; and / or the solid organic carbon source includes a carbohydrate compound, which includes one or more of glucose, sucrose, citric acid, asphalt, polyvinyl pyrrolidone, cellulose, and starch.

[0168] Carbohydrate compounds are a general term for polyhydroxy ketones or polyhydroxy aldehydes and their derivatives. Sugar molecules contain three elements: carbon, hydrogen and oxygen.

[0169] The solid organic carbon source in the present application includes but is not limited to at least one of an organic polymer and a carbohydrate compound. The organic polymer includes but is not limited to one or more of polyethylene, polypropylene, polystyrene, polyvinyl pyrrolidone, and phenolic resin. The carbohydrate compound includes but is not limited to one or more of glucose, sucrose, citric acid, asphalt, polyvinyl pyrrolidone, cellulose, and starch.

[0170] In one embodiment, the inert atmosphere includes at least one of nitrogen and argon; and / or the M element source includes a silicon source, and the mass ratio of the solid carbon source to the silicon source ranges from 10% to 40%, preferably, from 15% to 30%.

[0171] In the process of sintering the precursor under an inert atmosphere to obtain the sodium supplement material, the inert atmosphere includes at least one of nitrogen and argon.

[0172] In order to make the thickness of the carbon coating layer in the range of 10 nm to 5000 nm, the mass ratio of the solid carbon source to the silicon source is in the range of 10% to 40%, preferably, 15% to 30%.

[0173] In the above 10% to 40%, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 10%, 15%, 20%, 25%, 30%, 35%, 40%, etc., and the range values ​​between any two of the above point values.

[0174] In the above 15% to 30%, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 15%, 20%, 25%, 30%, etc., and the range values ​​between any two of the above point values.

[0175] In one embodiment, the organic gaseous carbon source includes at least one of alkanes and olefins; preferably, the organic gaseous carbon source includes one or more of methane, ethylene, and acetylene.

[0176] In the present application, the organic gaseous carbon source includes but is not limited to at least one of alkanes and alkenes, and includes but is not limited to one or more of methane, ethylene, and acetylene.

[0177] In one embodiment, the purity of the organic gaseous carbon source is 90% to 100%, preferably 95% to 100%; and / or the flow rate of the organic gaseous carbon source is 30 ml / min to 100 ml / min, preferably 60 ml / min to 100 ml / min.

[0178] The precursor is sintered in an organic gaseous carbon source atmosphere. During the sintering process, the organic gaseous carbon source needs to be continuously introduced as the sintering atmosphere. The purity of the organic gaseous carbon source ranges from 90% to 100%, preferably, from 95% to 100%.

[0179] The thickness of the carbon layer is controlled within the range of 10 nm to 5000 nm, and the flow rate of the introduced gas is controlled to meet the flow rate of the organic gaseous carbon source within the range of 30 ml / min to 100 ml / min, preferably 60 ml / min to 100 ml / min.

[0180] In the above 30ml / min to 100ml / min, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 30ml / min, 40ml / min, 50ml / min, 60ml / min, 70ml / min, 80ml / min, 90ml / min, 100ml / min, etc., and the range values ​​between any two of the above point values.

[0181] In the above-mentioned 60ml / min to 100ml / min, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 60ml / min, 65ml / min, 70ml / min, 75ml / min, 80ml / min, 85ml / min, 90ml / min, 95ml / min, 100ml / min, etc., and the range values ​​between any two of the above-mentioned point values.

[0182] In one embodiment, the present application also provides a positive electrode plate, which includes a sodium-supplementing material as shown; or, includes a sodium-supplementing material obtained by a preparation method of a sodium-supplementing material as shown.

[0183] The positive electrode sheet includes a current collector and an active material arranged on the current collector.

[0184] In one embodiment, the positive electrode plate includes a current collector and a coating arranged on at least one side of the current collector, the coating includes a sodium supplement material, and the mass of the sodium supplement material accounts for a range of greater than 0% and less than or equal to 5% of the mass of the coating, preferably, 1% to 3%.

[0185] like Figure 2 As shown, it is a schematic diagram of the structure of the positive electrode plate in one embodiment. In order to improve the sodium supplement effect and improve the problem that too much sodium supplement material will affect the energy density, the mass of the sodium supplement material accounts for a range of greater than 0% and less than or equal to 5% of the coating mass, preferably, 1% to 3%.

[0186] In the above-mentioned greater than 0% and less than or equal to 5%, the values ​​include the minimum and maximum values ​​of the range, and every value between such minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, etc., as well as the range values ​​between any two of the above-mentioned point values.

[0187] In the above-mentioned greater than 1% to 3%, the values ​​include the minimum and maximum values ​​of the range, and every value between such minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 1%, 1.5%, 2%, 2.5%, 3%, etc., and the range values ​​between any two of the above-mentioned point values.

[0188] In one embodiment, the present application also provides a diaphragm, which includes a sodium-supplementing material as shown; or, includes a sodium-supplementing material obtained by the preparation method of a sodium-supplementing material as shown.

[0189] Diaphragm, in the structure of secondary battery, diaphragm is one of the key internal components. The performance of diaphragm determines the interface structure and internal resistance of the battery, directly affecting the battery's capacity, cycle and safety performance. Excellent performance diaphragm plays an important role in improving the comprehensive performance of the battery. The main function of the diaphragm is to separate the positive and negative electrodes of the battery to prevent the two electrodes from contacting and short-circuiting. In addition, it also has the function of allowing electrolyte ions to pass through.

[0190] In one embodiment, the diaphragm includes a base film and a sodium supplement layer disposed on at least one side of the base film, the sodium supplement layer includes a sodium supplement material, and the thickness of the sodium supplement layer is greater than 0 μm and less than or equal to 10 μm, preferably 3 μm to 6 μm.

[0191] The base membrane is an organic microporous membrane, which refers to a membrane structure with micropores composed of organic materials.

[0192] like Figure 3 In order to improve the problem that the sodium supplement layer is too thin and the sodium supplement amount is small, and the sodium supplement layer is too thick and affects the performance of the diaphragm, the thickness of the sodium supplement layer is greater than 0 and less than or equal to 10 μm, preferably 3 μm to 6 μm.

[0193] Among the above-mentioned values ​​greater than 0 and less than or equal to 10μm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 0.5μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, etc., and the range value between any two of the above-mentioned point values.

[0194] In the above-mentioned 3μm to 6μm, the values ​​include the minimum and maximum values ​​of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values ​​in the embodiments and 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 6μm, etc., as well as the range values ​​between any two of the above-mentioned point values.

[0195] In one embodiment, the present application also provides an electrode assembly, the electrode assembly includes a positive electrode plate as shown, or includes a separator as shown.

[0196] In one embodiment, the present application further provides a battery cell, which includes the electrode assembly as described above.

[0197] In one embodiment, the present application further provides a battery, which includes the battery cell as described above.

[0198] In one embodiment, the present application further provides an electrical device, which includes the battery cell or battery described above.

[0199] Since the battery cell or battery adopts all the technical solutions of all the above embodiments, it at least has all the beneficial effects brought by the technical solutions of the above embodiments, which will not be described one by one here.

[0200] In addition, the battery (secondary battery, battery module, battery pack) and the electric device of the present application will be described below with reference to the drawings as appropriate.

[0201] In one embodiment of the present application, a secondary battery is provided.

[0202] Typically, a secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator. During the battery charge and discharge process, active ions are embedded and removed back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through. The separator is the separator improved above in this application.

[0203] The positive electrode plate includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector.

[0204] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.

[0205] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0206] In some embodiments, the positive electrode film layer may also optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.

[0207] In some embodiments, the positive electrode film layer may further include a conductive agent, for example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0208] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0209] The negative electrode plate includes a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector, and the negative electrode film layer includes a negative electrode active material.

[0210] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0211] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0212] In some embodiments, the negative electrode active material may adopt the negative electrode active material for the battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0213] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).

[0214] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0215] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0216] In some embodiments, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0217] The electrolyte plays a role in conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs.

[0218] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.

[0219] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.

[0220] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous structure separator with good chemical stability and mechanical stability can be selected.

[0221] In some embodiments, the material of the diaphragm can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The diaphragm can be a single-layer film or a multi-layer composite film, without particular limitation. When the diaphragm is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0222] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.

[0223] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.

[0224] In some embodiments, the outer packaging of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0225] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 5 The secondary battery 5 is a square structure as an example.

[0226] In some embodiments, reference Figure 6 , the outer package may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the diaphragm can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0227] In some embodiments, secondary batteries may be assembled into a battery module. The number of secondary batteries contained in the battery module may be one or more, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery module.

[0228] Figure 7 4 is an example of a battery module. Figure 7In the battery module 4, the plurality of secondary batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of secondary batteries 5 may be fixed by fasteners.

[0229] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.

[0230] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery pack.

[0231] Figure 8 and Fig. 9 1 is a battery pack 1 as an example. Figure 8 and Fig. 9 The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.

[0232] In addition, the present application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0233] As an electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.

[0234] Fig.10 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for the secondary battery, a battery pack or a battery module can be used.

[0235] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a secondary battery may be used as a power source.

[0236] Example

[0237] Example 1

[0238] Take 600 ml of deionized water as a solvent, add 114 g of nano-silicon dioxide and 300 g of sodium carbonate thereto, mix well and put into a ball mill, add 8 g of titanium dioxide and then 26.7 g of polyvinyl pyrrolidone, then stir and ball mill, put the slurry into a blast drying oven and bake at 80°C for 10 hours after ball milling, crush and sieve to obtain a precursor of sodium orthosilicate, put the precursor into a tubular furnace for sintering under argon protection at 700°C for 4 hours, take out the sample after the tubular furnace is naturally cooled, crush and sieve to obtain a titanium-doped carbon-coated sodium orthosilicate material. The Na3V2(PO4)3 positive electrode active material, the above-mentioned titanium-doped carbon-coated sodium orthosilicate material, polyvinylidene fluoride (PVDF) and the conductive agent acetylene black are dispersed and dissolved in N-methylpyrrolidone (NMP) solvent in a mass ratio of 88:2:5:5, and evenly coated on the Al foil current collector as the positive electrode sheet. The artificial graphite material is used as the negative electrode. The electrolyte is selected as the NaPF6+EMC+EC system, and the above materials are assembled into a full battery.

[0239] Example 2 to Example 10

[0240] On the basis of Example 1, the material and mass of the sodium source, the material and mass of the M element source, the material and mass of the N element source, and the material and mass of the carbon source are adjusted to obtain Examples 2 to 10.

[0241] Comparative Example 1

[0242] On the basis of Example 1, the sodium supplement material in Example 1 is replaced by Na2CO3.

[0243] Embodiment 11

[0244] Take 114g of nano-silicon dioxide, 300g of sodium carbonate and 8g of titanium dioxide, mix and then ball-mill, then put the ground mixed powder into a tube furnace for sintering, sintering in a methane atmosphere, the purity of methane is 90%, the sintering condition is 800℃ for 6 hours, after the tube furnace is naturally cooled, take out the sample, crush and sieve, and obtain titanium-doped carbon-coated sodium silicate material. A polypropylene film with a ceramic layer on the surface is selected as an isolation membrane, and a sodium supplement layer is set on the ceramic layer with the prepared titanium-doped carbon-coated sodium silicate material, and the thickness of the ceramic layer and the sodium supplement layer are 4um and 5um respectively. Na3V2(PO4)3 active material, PVDF and acetylene black are dissolved in NMP in a mass ratio of 90:5:5 to make a positive electrode slurry, and other materials are the same as in Example 1, and assembled into a full battery.

[0245] Example 12 to Example 14

[0246] On the basis of Example 11, the quality of the M element source and the carbon source atmosphere were adjusted to obtain Examples 12 to 14.

[0247] Preparation of positive electrode

[0248] The Na3V2(PO4)3 positive electrode active material, the above-mentioned sodium supplement material, the binder PVDF and the conductive agent acetylene black are dispersed and dissolved in NMP solvent in a mass ratio of 88:2:5:5 to form a uniformly dispersed slurry, and then the slurry is evenly coated on the aluminum foil current collector, and then dried, cold pressed and cut to obtain the positive electrode sheet.

[0249] Preparation of negative electrode

[0250] The active material artificial graphite, the conductive agent carbon black, the binder styrene-butadiene rubber (SBR), and the thickener sodium hydroxymethyl cellulose (CMC) are dissolved in the solvent deionized water in a weight ratio of 96.2:0.8:0.8:1.2, and the mixture is evenly mixed to prepare a negative electrode slurry; the negative electrode slurry is evenly coated on the negative electrode current collector copper foil once or multiple times, and the negative electrode sheet is obtained after drying, cold pressing, and slitting.

[0251] Preparation of electrolyte

[0252] In an argon atmosphere glove box (H2O<0.1ppm, O2<0.1ppm), organic solvents ethylene carbonate (EC) / ethyl methyl carbonate (EMC) were mixed evenly in a volume ratio of 3 / 7, 12.5% ​​NaPF6 sodium salt was added and dissolved in the organic solvent, and stirred evenly.

[0253] Isolation film

[0254] Polypropylene film is used as the isolation film.

[0255] Preparation of sodium ion batteries

[0256] The positive electrode sheet, the separator, and the negative electrode sheet of Example 1 are stacked in order, so that the separator is between the positive and negative electrode sheets to play an isolating role, and then wound to obtain a bare cell, and the bare cell is welded with a pole ear, and the bare cell is placed in an aluminum shell, and baked at 100°C to remove water, and then the electrolyte is injected and sealed to obtain an uncharged battery. The uncharged battery is then subjected to the processes of static, hot and cold pressing, formation, shaping, and capacity testing in sequence to obtain the sodium ion battery product of Example 1.

[0257] The sodium ion battery products of Comparative Example 1 and Examples 2-14 were also prepared according to the above steps.

[0258] Sodium Supplement Material Related Parameters Test The relevant parameter test process of the sodium orthosilicate composite material of the embodiment and the comparative example of the present application is as follows:

[0259] 1. Volume average particle size Dv50 test

[0260] Equipment model: Malvern 2000 (MasterSizer 2000) laser particle size analyzer, reference standard process: GB / T19077-2016 / ISO 13320:2009, specific test process: take an appropriate amount of the sample to be tested (the sample concentration is guaranteed to be 8-12% shading), add 20ml of deionized water, and simultaneously ultraviolet for 5min (53KHz / 120W) to ensure that the sample is completely dispersed, and then measure the sample according to GB / T19077-2016 / ISO 13320:2009 standard.

[0261] 2. Morphology test

[0262] The positive electrode active materials of all the embodiments and comparative examples were tested using a ZEISS sigma 300 scanning electron microscope, and then tested according to the standard JY / T010-1996 to observe the morphology of the samples.

[0263] The shape of the sodium supplement material prepared in the present application is not necessarily spherical, but may also be irregular.

[0264] Battery performance test

[0265] 1. Battery capacity retention rate test

[0266] Taking Example 1 as an example, the battery capacity retention rate test process is as follows: at 25°C, the battery corresponding to Example 1 is charged to 4.3V at a constant current of 1 / 3C, then charged to a current of 0.05C at a constant voltage of 4.3V, left for 5 minutes, and then discharged to 2.8V at 1 / 3C. The obtained capacity is recorded as the initial capacity C0. Repeat the above steps for the same battery, and record the discharge capacity Cn of the battery after the nth cycle at the same time. Then, the battery capacity retention rate Pn after each cycle is Cn / C0*100%. In this test process, the first cycle corresponds to n=1, the second cycle corresponds to n=2, and ... the 200th cycle corresponds to n=200. The battery capacity retention rate data corresponding to the embodiments and comparative examples in Tables 1 and 2 are the data measured after 200 cycles under the above test conditions, that is, the value of P200.

[0267] Table 1: Summary of sodium supplement materials prepared by doping with carbon source powder and corresponding battery performance

[0268]

[0269]

[0270] Various metal-doped sodium-supplementing materials are used in secondary batteries to improve the battery's cycle capacity retention rate.

[0271] By comparing Example 1 with Example 7, it is found that the particle size of the titanium-doped sodium silicate material that is not carbon-coated is significantly increased, and the battery made of the positive electrode containing the titanium-doped sodium silicate material that is not carbon-coated has a 200-cycle capacity retention rate that is significantly lower than that of Example 1.

[0272] Table 2: Summary of sodium supplement materials prepared by sintering in carbon source atmosphere and corresponding battery performance

[0273]

[0274] By comparing Example 11 with Example 14, it is found that when the sodium supplement material without metal doping is used as the sodium supplement layer of the isolation membrane, the 200-cycle capacity retention rate of the prepared battery is significantly lower than that of Example 11. The above are only preferred embodiments of the present invention, and the patent scope of the present invention is not limited thereto. All equivalent structural changes made by using the contents of the present specification and drawings under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A sodium supplement material, characterized in that: The chemical formula of the sodium supplement material is Na x M 1-y N y O z , wherein M includes at least one of semiconductor elements, alkaline earth metal elements, and transition metal elements; N includes at least one of semiconductor elements, alkaline earth metal elements, and transition metal elements, wherein the range value of x is 1≤x≤4, the range value of y is 0≤y≤0.25, and the range value of z is 2.5≤z≤4.

2. The sodium supplement material according to claim 1, characterized in that The M includes Si, and the chemical formula of the sodium supplement material is Na4Si 1-y N y O4, wherein N includes at least one of an alkaline earth metal element and a transition metal element.

3. The sodium supplement material according to claim 2, characterized in that 0.01<y≤0.25。 4. The sodium supplement material according to any one of claims 1 to 3, characterized in that The semiconductor element includes at least one of Si, Ge, Se, and Te; And / or, the alkaline earth metal element includes at least one of Be, Mg, Ca, Sr and Ba; And / or, the transition metal element includes at least one of Fe, Ni, Ti, Co, Mo, and Nb.

5. The sodium supplement material according to any one of claims 1 to 4, characterized in that The volume average particle size Dv50 of the sodium supplement material ranges from 0.5 μm to 10 μm, preferably, from 1 μm to 5 μm.

6. The sodium supplement material according to any one of claims 1 to 5, characterized in that A carbon coating layer is provided on the surface of the sodium supplement material.

7. The sodium supplement material according to claim 6, characterized in that The carbon coating layer comprises at least one of graphite, carbon nanotubes, carbon nanofibers, carbon black and graphene; And / or, the thickness of the carbon coating layer is 10 nm to 5000 nm, preferably 10 nm to 500 nm; And / or, the carbon coating layer completely covers the surface of the sodium supplementing material.

8. A method for preparing a sodium supplement material according to any one of claims 1 to 7, characterized in that: include: Mixing a sodium source, an M element source, and an N element source to prepare a precursor; The precursor is sintered in an inert atmosphere to obtain the sodium supplement material.

9. A method for preparing a sodium supplement material according to any one of claims 1 to 7, characterized in that: Mixing a sodium source, an M element source, and an N element source to prepare a precursor; The precursor is placed in an organic gaseous carbon source atmosphere and sintered to obtain the sodium supplement material.

10. The method for preparing the sodium supplement material according to claim 8, characterized in that: The step of mixing the sodium source, the M element source, and the N element source to prepare the precursor includes: A sodium source, an M element source, a solid carbon source and a N element source are mixed to prepare a precursor.

11. The method for preparing the sodium supplement material according to any one of claims 8 to 10, characterized in that: In the step of mixing the sodium source, the M element source, and the N element source to prepare the precursor, the mixing step includes at least one of ball milling, grinding, or stirring; In the step of sintering the precursor, the sintering temperature is 500° C. to 1000° C., and the sintering time is 3 hours to 10 hours.

12. The method for preparing the sodium supplement material according to any one of claims 8 to 11, characterized in that: The sodium source includes one or more of sodium hydroxide, sodium nitrate, sodium carbonate, sodium acetate, and sodium sulfate; And / or, the M element source includes a silicon source, and the silicon source includes one or more of silicon, silicon monoxide, and silicon dioxide; And / or, the N element source includes one or more of magnesium, iron, nickel, ferroferric oxide, titanium dioxide, cobalt oxide, cobalt acetate, cobalt sulfide, molybdenum oxide, niobium oxide, nickel acetate, nickel sulfate, nickel oxide, manganese dioxide and molybdenum dioxide; And / or, the M element source includes a silicon source, and the volume average particle size Dv50 of the silicon source includes 50 nm to 20 μm, preferably, 500 nm to 10 μm; And / or, the M element source includes a silicon source, and the molar ratio of Na in the sodium source to Si in the silicon source includes (2-4.5):1; And / or, the M element source includes a silicon source, and the molar ratio of Si in the silicon source to N element in the N element source includes (3-99):

1.

13. The method for preparing the sodium supplement material according to claim 10, characterized in that: The solid carbon source includes a solid organic carbon source and / or a solid inorganic carbon source.

14. The method for preparing the sodium supplement material according to claim 13, characterized in that: The solid organic carbon source includes at least one of an organic polymer and a sugar compound; And / or, the solid inorganic carbon source includes at least one of graphite and carbon black.

15. The method for preparing the sodium supplement material according to claim 14, characterized in that: The solid organic carbon source includes an organic polymer, and the organic polymer includes one or more of polyethylene, polypropylene, polystyrene, polyvinyl pyrrolidone, and phenolic resin; And / or, the solid organic carbon source includes sugar compounds, and the sugar compounds include one or more of glucose, sucrose, citric acid, asphalt, polyvinyl pyrrolidone, cellulose, and starch.

16. The method for preparing the sodium supplement material according to any one of claims 10, 13 to 15, characterized in that: The inert atmosphere includes at least one of nitrogen and argon; And / or, the M element source includes a silicon source, and the mass ratio of the solid carbon source to the silicon source ranges from 10% to 40%, preferably, from 15% to 30%.

17. The method for preparing the sodium supplement material according to claim 9, characterized in that: The organic gaseous carbon source includes at least one of alkanes and alkenes; Preferably, the organic gaseous carbon source includes one or more of methane, ethylene and acetylene.

18. The method for preparing the sodium supplement material according to claim 9 or 17, characterized in that: The purity of the organic gaseous carbon source is 90% to 100%, preferably 95% to 100%; And / or, the flow rate of the organic gaseous carbon source is 30 ml / min to 100 ml / min, preferably 60 ml / min to 100 ml / min.

19. A positive electrode plate, characterized in that: The positive electrode plate comprises a sodium supplement material as claimed in any one of claims 1 to 7; Alternatively, the sodium-supplementing material comprises the sodium-supplementing material obtained by the preparation method of the sodium-supplementing material according to any one of claims 8 to 18.

20. The positive electrode sheet according to claim 19, characterized in that: The positive electrode plate includes a current collector and a coating arranged on at least one side of the current collector, the coating includes the sodium supplement material, and the mass of the sodium supplement material accounts for more than 0% and less than or equal to 5% of the mass of the coating, preferably, 1% to 3%.

21. A diaphragm, characterized in that: The diaphragm comprises a sodium supplement material as claimed in any one of claims 1 to 7; Alternatively, the sodium-supplementing material comprises the sodium-supplementing material obtained by the preparation method of the sodium-supplementing material according to any one of claims 8 to 18.

22. The diaphragm according to claim 21, characterized in that The diaphragm includes a base film and a sodium-compensating layer disposed on at least one side of the base film, the sodium-compensating layer includes the sodium-compensating material, and the thickness of the sodium-compensating layer is greater than 0 μm and less than or equal to 10 μm, preferably, 3 μm to 6 μm.

23. An electrode assembly, characterized in that: The electrode assembly comprises the positive electrode sheet as claimed in claim 19 or 20; Alternatively, it comprises the diaphragm as claimed in claim 21 or 22.

24. A battery cell, characterized in that: The battery cell includes the electrode assembly as claimed in claim 23 .

25. A battery, characterized in that: The battery comprises the battery cell as claimed in claim 24.

26. An electrical device, characterized in that: The electrical device comprises the battery cell according to claim 24 or the battery according to claim 25 .

Citation Information

Patent Citations

  • Doped silicate sodium ion battery positive electrode material and preparation method thereof

    CN105819461A

  • Sodium Transition Metal Silicate And Method Of Forming Same

    CN107709237A

  • Sodium-rich transition metal oxide composite sodium-supplementing positive electrode active material, positive electrode material, positive electrode, preparation of positive electrode and application of positive electrode in sodium-ion battery

    CN111293290A

  • Sodium-ion battery negative electrode sodium supplement additive and negative electrode material

    CN113644271A

  • Compound for pre-sodium modification and preparation method thereof, positive electrode pre-sodium modification material and preparation method thereof, and sodium ion battery

    CN113896240A

Cited By

  • Sodium supplementing agent, sodium ion battery, electronic equipment and preparation method of sodium supplementing agent

    CN121172308A