Battery cell preparation method and battery
Optimize the preparation method of the battery cell through laser processing and three-dimensional printing technology, and form a stable positive electrode active material layer and a high energy density negative electrode active material layer, which solves the problem of unstable battery cell preparation process in the prior art and significantly improves the battery energy density and cycling performance.
Patent Information
- Application Number
- CN202411288678.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-12
AI Technical Summary
The existing secondary battery technology is difficult to optimize the preparation process of the battery cell under the requirements of high energy density and long cycle performance, resulting in unstable bonding of the positive electrode active material layer and excessive use of the negative electrode active material, affecting the battery performance.
Laser processing technology is used to partially cure the positive electrode active material slurry and bond it to the positive electrode current collector to form a nanoprotective film. Through a three-dimensional printing process, a three-dimensional frame structure is formed on the negative electrode current collector, which is filled with the negative electrode active material, pressurized molding, and at the same time. The surface of the negative electrode sheet is modified with functional groups.
The durability and stability of the positive electrode active material layer and the positive electrode current collector are improved, the amount of negative electrode binder is reduced, the service life of the battery is extended, the internal resistance is reduced, and the energy density and circulation performance of the battery are improved.
Smart Images

Figure CN118943457A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of secondary batteries, and in particular to a method for preparing a battery cell and a battery. Background Art
[0002] With the development of secondary battery technology, secondary batteries are widely used in current household, personal electronic products and industrial electronic products. The battery cell of a secondary battery includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte.
[0003] In the preparation of positive and negative electrode sheets, the traditional technology is to coat the slurry on the current collector, and then obtain the electrode sheet through processes such as roller pressing and oven drying. However, with the demand for high energy density and long cycle performance of secondary batteries, the preparation process needs to be further optimized. Summary of the invention
[0004] Based on this, it is necessary to provide a method for preparing a battery cell and a battery with high energy density.
[0005] In a first aspect, the present application provides a method for preparing a battery cell, the method comprising the following steps:
[0006] S11, preparing a positive electrode sheet: coating a positive electrode active material slurry on a positive electrode current collector, laser processing, partially curing the positive electrode active material slurry to bond with the positive electrode current collector, and drying to form a positive electrode active material layer to obtain a positive electrode sheet;
[0007] S12, forming a film on the surface of the positive electrode sheet: forming a nano protective film on the surface of the positive electrode sheet prepared in step S11;
[0008] S13, preparing a negative electrode sheet: forming a three-dimensional framework structure formed by a negative electrode active material and a negative electrode binder on a negative electrode current collector through a three-dimensional printing process, then filling the negative electrode active material into the three-dimensional framework structure to form a negative electrode active material layer, and press-forming to obtain a negative electrode sheet;
[0009] S14, surface modification of the negative electrode plate: performing surface modification treatment on the negative electrode plate prepared in step S13 to form functional groups;
[0010] S15, preparing a battery cell: laminating the surface-filmed positive electrode sheet and the separator prepared in step S12 and the surface-modified negative electrode sheet prepared in step S14, and then performing hot pressing treatment to obtain a battery cell.
[0011] In some embodiments, the positive electrode active material slurry formed in step S11 has a solid content of 80% to 90%.
[0012] In some embodiments, the laser power density of the laser treatment in step S11 is 10 W / cm 2~15W / cm 2 , the scanning speed is 10mm / s~12mm / s.
[0013] In some embodiments, the material of the nano protective film formed in step S12 is one or more of metal oxides, metal fluorides, and metal phosphate compounds.
[0014] In some embodiments, the nano protective film is obtained by an atomic layer deposition process, in which the deposition temperature is 150° C. to 180° C. and the reaction cycle is 9 to 13 cycles.
[0015] In some embodiments, the thickness of the nano protective film is 10 nm to 12 nm.
[0016] In some embodiments, the functional group in step S14 includes one or a combination of a siloxane group and a trifluoromethyl group.
[0017] In some embodiments, in step S14, a plasma enhanced chemical vapor deposition process is used to perform surface modification treatment on the negative electrode plate by mixing the first gas and / or the second gas, wherein the plasma enhanced chemical vapor deposition process satisfies at least one of the following (i) to (v):
[0018] (i) The reaction temperature is 180°C to 200°C;
[0019] (ii) the first gas can modify siloxane groups on the surface of the negative electrode plate, including any one of silane, dichlorosilane, trichlorosilane, and silicon chloride;
[0020] (iii) the second gas can modify the trifluoromethyl group on the surface of the negative electrode plate, including any one of hydrogen fluoride, difluoromethane, trifluoromethane, and carbon tetrafluoride;
[0021] (iv) the flow rate of the first gas is 20-40 sccm;
[0022] (v) the flow rate of the second gas is 20-40 sccm;
[0023] (vi) The deposition time is 1h to 1.5h.
[0024] In some embodiments, in the three-dimensional framework structure formed in step S13, the mass proportion of the negative electrode active material is 95% to 98%, and the mass proportion of the negative electrode binder is 2% to 5%.
[0025] In a second aspect, the present application also provides a battery, which includes a battery cell prepared by the preparation method.
[0026] The preparation method of the battery cell includes the steps of preparing the positive electrode sheet and the negative electrode sheet. When preparing the positive electrode sheet, the positive active material slurry is partially solidified by laser treatment and then bonded to the positive current collector, and the positive active material layer is formed on the positive current collector to obtain the positive electrode sheet. On the one hand, the laser treatment can make the positive electrode binder in the positive electrode active material slurry melt quickly. During the curing process, the melted positive electrode binder is bonded to the positive current collector through molecular forces such as van der Waals force and hydrogen bond, and the melted positive electrode binder molecules diffuse with each other. This diffusion helps to form a stronger chemical bond, thereby improving the durability and stability of the bonding between the positive active material layer and the positive current collector; on the other hand, the laser induced hot melt technology makes the positive electrode binder melt and solidify and bond to the positive current collector. Compared with the traditional technology in which the positive electrode binder is dissolved in the first solvent and then dried in an oven and bonded to the positive current collector, it can reduce the use of the first solvent, save resources, and reduce costs.
[0027] Furthermore, a film is formed on the surface of the positive electrode plate to form a nano protective film. The formation of the nano protective film on the surface of the positive electrode plate can, on the one hand, reduce the direct contact area between the positive electrode active material and the electrolyte, reduce the dissolution of metal ions in the positive electrode active material by free HF in the electrolyte, alleviate the rate of destruction of the positive electrode active material, and avoid excessive loss of the positive electrode active material; on the other hand, after heat treatment or charge and discharge cycles, the nano protective film formed on the surface of the positive electrode plate can partially diffuse into the interior of the positive electrode active material layer to form a stable surface solid solution, thereby preventing the lattice structure of the positive electrode active material from changing during the charge and discharge cycle, and maintaining a stable structure of the positive electrode active material during the electrochemical process, thereby enabling the battery to obtain good electrochemical performance.
[0028] When preparing the negative electrode sheet, a three-dimensional framework structure formed by a negative electrode active material and a negative electrode binder is formed on the negative electrode collector through a three-dimensional printing process, and then the negative electrode active material is filled into the three-dimensional framework structure to form a negative electrode active material layer, and pressure molding is performed to obtain a negative electrode sheet. Three-dimensional printing is performed under high temperature conditions to bond the three-dimensional framework structure to the negative electrode collector, and then the negative electrode active material is filled into the three-dimensional framework structure to form a negative electrode active material layer, and pressure molding is performed to obtain a negative electrode sheet. This can reduce the amount of negative electrode binder used, increase the proportion of negative electrode active material in the negative electrode active material layer, and thus improve the energy density of the battery.
[0029] Furthermore, the surface of the negative electrode is modified to form functional groups, including siloxane groups (Si-O-Si) and trifluoromethyl groups (-CF 3 ) or a combination of two of them. The siloxane group (Si-O-Si) can reduce the negative electrode interface side reaction and extend the battery life; the trifluoromethyl group (-CF 3) can improve the conductivity of the negative electrode surface and help reduce the internal resistance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 A schematic diagram of a method for preparing a battery cell according to one embodiment. DETAILED DESCRIPTION
[0031] References to embodiments of the present application will now be provided in detail, one or more examples of which are described below. Each example is provided as an explanation rather than a limitation of the present application. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made to the present application without departing from the scope or spirit of the present application. For example, a feature described or described as part of one embodiment may be used in another embodiment to produce a further embodiment.
[0032] Therefore, it is intended that the present application covers such modifications and variations that fall within the scope of the appended claims and their equivalents. Other objects, features and aspects of the present application are disclosed in or are apparent from the following detailed description. It will be appreciated by those of ordinary skill in the art that this discussion is merely a description of exemplary embodiments and is not intended to limit the broader aspects of the present application.
[0033] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0034] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0035] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0036] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0037] If there is no special explanation, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps S12 and S14, which means that the method may include steps S12 and S14 performed sequentially, or may include steps S14 and S12 performed sequentially. For example, it is mentioned that the method may also include step S16, which means that step S16 may be added to the method in any order, for example, the method may include steps S12, S14 and S16, or may include steps S12, S16 and S14, or may include steps S16, S12 and S14, etc.
[0038] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0039] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0040] See also Figure 1 , a method for preparing a battery cell, comprising the following steps S11~S15.
[0041] S11, preparing a positive electrode sheet: coating a positive electrode active material slurry on a positive electrode current collector, laser processing to partially solidify the positive electrode active material slurry so that it adheres to the positive electrode current collector, and drying to form a positive electrode active material layer to obtain a positive electrode sheet.
[0042] Illustratively, the positive electrode active material slurry includes a positive electrode active material, a conductive agent, a positive electrode binder, and a first solvent.
[0043] Illustratively, the positive electrode active material slurry is coated on one side of the positive electrode current collector, or the positive electrode active material slurry is coated on both sides of the positive electrode current collector.
[0044] Illustratively, the laser treatment refers to emitting laser light on the side of the positive electrode current collector coated with the positive electrode active material slurry.
[0045] Furthermore, the laser treatment uses laser induced thermal melting technology, which melts the positive electrode binder in the positive electrode active material slurry and removes part of the first solvent, thereby shaping the partially solidified positive electrode active material slurry so as to bond with the positive electrode current collector, and further drying the positive electrode sheet.
[0046] In the traditional technology, the preparation of the positive electrode sheet requires mixing the positive electrode active material, the conductive agent, the positive electrode binder and the first solvent to form a positive electrode active material slurry, and then coating the positive electrode active material slurry on the positive electrode collector, and then baking in an oven to make the positive electrode active material slurry and the positive electrode collector bond to form a positive electrode sheet. In the traditional technology, on the one hand, a large amount of the first solvent is required to dissolve the positive electrode binder (for example, generally speaking, the mass ratio of the positive electrode binder to the first solvent is 1:80), the manufacturing cost is high, and it is not conducive to environmental protection; on the other hand, after drying in the oven, the positive electrode binder relies on the physical locking effect and the positive electrode collector to bond, does not involve chemical bonds and molecular diffusion, and has low adhesion. After a long period of charge and discharge cycles, the positive electrode active material layer is easy to peel off from the positive electrode collector, affecting the cycle and capacity of the battery.
[0047] In the present application, the positive electrode active material slurry is partially solidified by laser induced hot melting technology and then bonded to the positive electrode current collector, and dried to form a positive electrode active material layer to obtain a positive electrode sheet. On the one hand, the laser induced hot melting technology can cause the positive electrode binder in the positive electrode active material slurry to melt rapidly. During the curing process, the melted positive electrode binder is bonded to the positive electrode current collector through molecular forces such as van der Waals force and hydrogen bond, and the melted positive electrode binder molecules diffuse with each other. This diffusion helps to form a stronger chemical bond, thereby improving the durability and stability of the bonding between the positive electrode active material layer and the positive electrode current collector; on the other hand, the laser induced hot melting technology causes the positive electrode binder to melt and solidify and bond to the positive electrode current collector. Compared with the traditional technology in which the positive electrode binder is dissolved in the first solvent and then dried in an oven and bonded to the positive electrode current collector, it can reduce the use of the first solvent, save resources, and reduce costs.
[0048] S12, film formation on the surface of the positive electrode plate: a nano protective film is formed on the surface of the positive electrode plate prepared in step S11.
[0049] For example, the electrolyte in the electrolyte will undergo a hydrolysis reaction to generate HF, which has a strong corrosive effect on the positive electrode active material, causing the dissolution of metal ions in the positive electrode active material, thereby causing irreversible capacity decay of the battery. Forming a nano protective film on the surface of the positive electrode plate can, on the one hand, reduce the direct contact area between the positive electrode active material and the electrolyte, reduce the dissolution of metal ions in the positive electrode active material by HF, alleviate the rate of destruction of the positive electrode active material, and avoid excessive loss of the positive electrode active material; on the other hand, after heat treatment or charge and discharge cycles, the nano protective film formed on the surface of the positive electrode plate can partially diffuse into the interior of the positive electrode active material layer to form a stable surface solid solution, preventing the positive electrode active material from changing its lattice structure during the charge and discharge cycle, so that the positive electrode active material maintains a stable structure during the electrochemical process, thereby enabling the battery to obtain good electrochemical performance.
[0050] S13, preparing a negative electrode sheet: forming a three-dimensional framework structure formed by a negative electrode active material and a negative electrode binder on the negative electrode current collector through a three-dimensional printing process, and then filling the negative electrode active material into the three-dimensional framework structure to form a negative electrode active material layer, and press-forming to obtain a negative electrode sheet.
[0051] Exemplarily, the three-dimensional framework structure is formed by three-dimensional printing of negative electrode active materials and negative electrode binders. The three-dimensional printing is performed under high temperature conditions so that the three-dimensional framework structure is bonded to the negative electrode current collector. The negative electrode active material is then filled into the three-dimensional framework structure to form a negative electrode active material layer, which is pressurized to obtain a negative electrode sheet. This can reduce the amount of negative electrode binder used and increase the proportion of negative electrode active material in the negative electrode active material layer, thereby improving the energy density of the battery.
[0052] S14, surface modification of the negative electrode plate: performing surface modification treatment on the negative electrode plate prepared in step S13 to form functional groups.
[0053] Exemplarily, the functional groups include siloxane groups (Si-O-Si) and trifluoromethyl groups (-CF 3 ) or a combination of two of them. The siloxane group (Si-O-Si) can reduce the negative electrode interface side reaction and extend the battery life; the trifluoromethyl group (-CF 3 ) can improve the conductivity of the negative electrode surface and help reduce the internal resistance of the battery.
[0054] S15, preparing a battery cell: laminating the surface film-forming positive electrode sheet and the separator prepared in step S12 and the surface modified negative electrode sheet prepared in step S14, and then performing hot pressing treatment to obtain a battery cell.
[0055] The preparation method of the battery cell includes the steps of preparing the positive electrode sheet and the negative electrode sheet. When preparing the positive electrode sheet, the positive active material slurry is partially solidified by laser treatment and then bonded to the positive current collector, and the positive active material layer is formed on the positive current collector to obtain the positive electrode sheet. On the one hand, the laser treatment can make the positive electrode binder in the positive electrode active material slurry melt quickly. During the curing process, the melted positive electrode binder is bonded to the positive current collector through molecular forces such as van der Waals force and hydrogen bond, and the melted positive electrode binder molecules diffuse with each other. This diffusion helps to form a stronger chemical bond, thereby improving the durability and stability of the bonding between the positive active material layer and the positive current collector; on the other hand, the laser induced hot melt technology makes the positive electrode binder melt and solidify and bond to the positive current collector. Compared with the traditional technology in which the positive electrode binder is dissolved in the first solvent and then dried in an oven and bonded to the positive current collector, it can reduce the use of the first solvent, save resources, and reduce costs.
[0056] Furthermore, a film is formed on the surface of the positive electrode plate to form a nano protective film. The formation of the nano protective film on the surface of the positive electrode plate can, on the one hand, reduce the direct contact area between the positive electrode active material and the electrolyte, reduce the dissolution of metal ions in the positive electrode active material by free HF in the electrolyte, alleviate the rate of destruction of the positive electrode active material, and avoid excessive loss of the positive electrode active material; on the other hand, after heat treatment or charge and discharge cycles, the nano protective film formed on the surface of the positive electrode plate can partially diffuse into the interior of the positive electrode active material layer to form a stable surface solid solution, thereby preventing the lattice structure of the positive electrode active material from changing during the charge and discharge cycle, and maintaining a stable structure of the positive electrode active material during the electrochemical process, thereby enabling the battery to obtain good electrochemical performance.
[0057] When preparing the negative electrode sheet, a three-dimensional framework structure formed by a negative electrode active material and a negative electrode binder is formed on the negative electrode collector through a three-dimensional printing process, and then the negative electrode active material is filled into the three-dimensional framework structure to form a negative electrode active material layer, and pressure molding is performed to obtain a negative electrode sheet. Three-dimensional printing is performed under high temperature conditions to bond the three-dimensional framework structure to the negative electrode collector, and then the negative electrode active material is filled into the three-dimensional framework structure to form a negative electrode active material layer, and pressure molding is performed to obtain a negative electrode sheet. This can reduce the amount of negative electrode binder used, increase the proportion of negative electrode active material in the negative electrode active material layer, and thus improve the energy density of the battery.
[0058] Furthermore, the surface of the negative electrode is modified to form functional groups, including siloxane groups (Si-O-Si) and trifluoromethyl groups (-CF 3 ) or a combination of two of them. The siloxane group (Si-O-Si) can reduce the negative electrode interface side reaction and extend the battery life; the trifluoromethyl group (-CF 3 ) can improve the conductivity of the negative electrode surface and help reduce the internal resistance of the battery.
[0059] Exemplarily, before step S15, the following steps may also be included: laser cutting, using laser cutting technology to cut the film-formed positive electrode sheet and the surface-modified negative electrode sheet, and accurately cut them into required sizes. Exemplarily, the laser power in laser cutting is 50W to 70W, the scanning speed is 1000 mm / s to 1200 mm / s, and the cutting accuracy is controlled at ±0.1mm.
[0060] In some embodiments, in step S11, the positive electrode active material slurry includes a positive electrode active material, and the positive electrode active material includes LiCo 1-y M y O 2 、LiNi 1-y M y O 2 、LiMn2-y M y O 4 、LiNi x Co y Mn z M 1-x-y-z O 2 One or more of, wherein M is selected from one or more of Fe, Co, Ni, Mn, Mg, Cu, Zn, Al, Sn, B, Ga, Cr, Sr, V and Ti, and 0≤y≤1, 0≤x≤1, 0≤z≤1, x+y+z≤1. Further, the positive electrode active material can be nano-lithium cobalt manganese oxide LiCoMnO 4 , and its particle size is 10nm~100nm.
[0061] Exemplarily, the positive electrode active material can be prepared by mechanical ball milling. Exemplarily, the ball milling time of the mechanical ball milling method can be 12h to 15h, the ball milling medium is a zirconia ball, and the rotation speed is 200rpm to 250rpm. After the positive electrode active material is prepared, the positive electrode active material, the conductive agent, the positive electrode binder and the first solvent are stirred evenly to form a positive electrode active material slurry. Exemplarily, the positive electrode active material slurry can be mixed under constant temperature stirring conditions, the stirring speed is 400rpm to 500rpm, the temperature is 50℃ to 60℃, and the mixing time is 0.5~1h.
[0062] In some embodiments, in step S11, the positive electrode binder includes but is not limited to one or more of polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyvinylidene fluoride hexafluoropropylene (PVDF-HFP), polypropylene (PP), polyethylene (PE), styrene-butadiene rubber (SBR), nitrile rubber (NBR), sodium carboxymethyl cellulose (CMC), polyacrylic acid, polyacrylonitrile, and sodium alginate.
[0063] In some embodiments, in step S11, the conductive agent includes but is not limited to one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, carbon nanofibers, and graphene.
[0064] In some embodiments, in step S11, the first solvent includes, but is not limited to, one or more of N-methylpyrrolidone (NMP), dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), dimethyl sulfoxide (DMSO), and deionized water.
[0065] Exemplarily, the solid content of the positive electrode active material slurry formed in step S11 is 80% to 90%. Exemplarily, the solid content of the positive electrode active material slurry may be, but is not limited to, 80%, 82%, 84%, 86%, 88% or 90%.
[0066] In one embodiment, in step S11, the laser power density of the laser treatment is 10 W / cm 2 ~15W / cm 2 , the scanning speed is 10mm / s~12mm / s.
[0067] For example, the laser power density may be, but is not limited to, 10 W / cm 2 , 11W / cm 2 、12W / cm 2 、13W / cm 2 、14W / cm 2 or 15W / cm 2 For example, the scanning speed of the laser processing may be, but is not limited to, 10 mm / s, 10.2 mm / s, 10.5 mm / s, 10.8 mm / s, 11 mm / s, 11.2 mm / s, 11.5 mm / s, 11.8 mm / s or 12 mm / s.
[0068] If the laser power is too low or the scanning speed is too fast, the binder in the positive electrode active material slurry cannot be completely melted, thereby affecting the bonding effect between the positive electrode active material layer and the positive electrode current collector, resulting in a decrease in the battery's cycle performance; if the laser power is too high or the scanning speed is too slow, the heat generated by the laser will be too concentrated, thereby destroying the structure of the positive electrode active material, resulting in a decrease in the battery's capacity and cycle performance.
[0069] In one embodiment, in step S11, the drying treatment adopts spray drying, wherein the spray drying temperature is 75°C to 80°C, the air flow velocity is 5m / s to 8m / s, and the time is 30min to 40min. The spray drying technology is used to perform secondary drying on the partially solidified positive active material slurry. Compared with the traditional oven drying method, the spray drying has higher thermal efficiency, can quickly remove the residual first solvent in a shorter time and ensure that the nanostructure of the positive active material in the positive active material slurry is not damaged. In addition, the spray drying method is more energy-saving and more in line with the needs of energy conservation, emission reduction and resource conservation.
[0070] Exemplarily, the temperature of spray drying may be, but is not limited to, 75°C, 76°C, 77°C, 78°C, 79°C, or 80°C. Exemplarily, the air flow rate of spray drying may be, but is not limited to, 5m / s, 6m / s, 7m / s, or 8m / s. Exemplarily, the time of spray drying may be, but is not limited to, 30min, 32min, 34min, 36min, 38min, or 40min. Within the above range, spray drying can quickly dry the positive active material slurry to solidify it.
[0071] In one embodiment, in step S13, the printing speed in the three-dimensional printing process is 10 mm / s to 12 mm / s, and the printing temperature is 320° C. to 350° C. Exemplarily, the printing speed in the three-dimensional printing process is 10 mm / s, 10.5 mm / s, 11 mm / s, 11.5 mm / s or 12 mm / s. Exemplarily, the printing temperature may be, but is not limited to, 320° C., 330° C., 340° C. or 350° C.
[0072] For example, the negative electrode active material may be three-dimensional graphene, which may be prepared by a liquid phase exfoliation method. Further, the liquid phase exfoliation method may be a vapor phase deposition method, with a reaction temperature of 900°C to 1000°C and a holding time of 25min to 35min. For example, the surface area of the three-dimensional graphene is 1000m 2 / g~2000m 2 / g range.
[0073] Illustratively, the negative electrode binder may be one or more of polytetrafluoroethylene, ABS resin, polyacrylic acid, and polyacrylonitrile.
[0074] Exemplarily, in the formed three-dimensional framework structure, the mass proportion of the negative electrode active material is 95% to 98%, and the mass proportion of the negative electrode binder is 2% to 5%. Exemplarily, the mass proportion of the negative electrode active material can be but not limited to 95%, 96%, 97% or 98%, and the mass proportion of the negative electrode binder can be but not limited to 2%, 3%, 4% or 5%.
[0075] In one embodiment, the thickness of the positive electrode sheet is 140 μm to 170 μm, and the thickness of the negative electrode sheet is 100 μm to 120 μm. For example, the thickness of the positive electrode sheet can be but not limited to 140 μm, 145 μm, 150 μm, 155 μm, 160 μm, 165 μm or 170 μm. For example, the thickness of the negative electrode sheet can be but not limited to 100 μm, 105 μm, 110 μm, 115 μm or 120 μm.
[0076] In one embodiment, in step S12, the material of the nano protective film is one or more of metal oxides, metal fluorides, and metal phosphate compounds, and the thickness is 10nm to 12nm. Exemplarily, the material of the nano protective film can be a metal oxide, for example, it can be one or more of zinc oxide, aluminum oxide, manganese oxide, tin oxide, bismuth oxide, titanium oxide, and zirconium oxide. Exemplarily, the material of the nano protective film can be a metal fluoride, for example, it can be one or more of aluminum fluoride, calcium fluoride, and magnesium fluoride. Exemplarily, the material of the nano protective film can be a metal phosphate compound, for example, it can be one or more of aluminum phosphate and magnesium phosphate.
[0077] For example, the thickness of the nano protective film can be, but is not limited to, 10 nm, 10.5 nm, 11 nm, 11.5 nm or 12 nm. If the thickness of the nano protective film is too thick, it will affect the deintercalation of lithium ions in the positive electrode active material, thereby affecting the rate performance of the battery; if the thickness of the nano protective film is too thin, it is not enough to avoid direct contact between the positive electrode active material and the electrolyte, thereby causing excessive loss of the positive electrode active material, thereby affecting the battery capacity and cycle performance.
[0078] In one embodiment, in step S12, the nano protective film is obtained by an atomic layer deposition process; the deposition temperature in the atomic layer deposition process is 150°C to 180°C, and the reaction cycle is 9 to 13 cycles. Exemplarily, the deposition temperature in the atomic layer deposition process may be, but is not limited to, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C or 180°C. If the deposition temperature in the atomic layer deposition process is too low, the reaction rate will be slow, the surface reaction process will be incomplete, and a nano protective film with good thickness consistency cannot be formed on the surface of the positive electrode; if the deposition temperature in the atomic layer deposition process is too high, the bonding force between the nano protective film and the positive electrode will be reduced, and the nano protective film will easily fall off from the positive electrode after the battery cycle, and it will not play a protective role. If the reaction cycle in the atomic layer deposition process is too few, the thickness of the nano protective film on the surface of the positive electrode will be too low. If the reaction cycle in the atomic layer deposition process is too many, the thickness of the nano protective film on the surface of the positive electrode will be too high.
[0079] In one of the embodiments, in step S14, the surface of the negative electrode plate is modified to form a functional group, which is obtained by a plasma enhanced chemical vapor deposition process, wherein the reaction temperature of the plasma enhanced chemical vapor deposition is 180°C to 200°C, and the gas used includes a first gas and / or a second gas, the first gas can modify the siloxane group on the surface of the negative electrode plate, the first gas includes any one of silane, dichlorosilane, trichlorosilane, and silicon chloride, the second gas can modify the trifluoromethyl group on the surface of the negative electrode plate, the second gas includes any one of trifluoromethane, difluoromethane, hydrogen fluoride, and carbon tetrafluoride, the flow rate of the first gas is 20~40sccm, the flow rate of the second gas is 20~40sccm, and the modification time is 1h~1.5h.
[0080] If the reaction temperature in the plasma enhanced chemical vapor deposition process is too low, the reaction rate is too slow, the first gas or the second gas does not react fully, and it is impossible to modify the surface of the negative electrode plate into a uniform functional group, resulting in a decrease in the discharge capacity and cycle performance of the battery; if the reaction temperature in the plasma enhanced chemical vapor deposition process is too high, it will cause the negative electrode binder in the three-dimensional framework structure to soften and the structure to collapse, ultimately affecting the cycle performance of the battery. If the flow rate of the first gas and / or the second gas in the plasma enhanced chemical vapor deposition process is too low, the functional group layer modified on the surface of the negative electrode plate is too thin and cannot effectively protect the negative electrode active material. The interface side reaction between the electrolyte and the negative electrode active material will cause the battery capacity to decay and shorten the service life; if the flow rate of the first gas and / or the second gas in the plasma enhanced chemical vapor deposition process is too high, the functional group layer modified on the surface of the negative electrode plate is too thick, which will make it difficult for lithium ions to embed into the negative electrode active material and reduce the battery capacity.
[0081] In one embodiment, in step S15, the pressing temperature of the hot pressing treatment is 110°C to 120°C, the pressing pressure is 5MPa to 10MPa, and the pressing time is 10min to 15min. Exemplarily, the pressing temperature of the hot pressing treatment may be, but is not limited to, 110°C, 112°C, 114°C, 115°C, 118°C, 112°C, 115°C, 118°C or 120°C. Exemplarily, the pressing time may be, but is not limited to, 10min, 11min, 12min, 13min, 14min or 15min. Within the above range, the positive electrode sheet, the separator and the negative electrode sheet can be pressed and fitted, and the three-dimensional support structure on the negative electrode sheet will not be destroyed.
[0082] The present application also provides a battery, which includes a battery cell prepared by the preparation method provided by any of the above embodiments.
[0083] In some embodiments, the battery further includes an electrolyte. Exemplarily, the electrolyte is a polymer electrolyte, and the concentration of the polymer electrolyte solution is 1wt% to 2wt%. The polymer electrolyte is mixed without solvent under an inert gas, and specifically includes by mass: 30% to 50% dimethyl carbonate, 20% to 40% butyl acrylate, 20% to 30% dimethylacetamide, 20% to 30% lithium hexafluorophosphate, 0.1% to 2% divinyldimethylsilane, 0.1% to 1% acrylamide, and 0.1% to 0.5% phosphorus trioxide.
[0084] The following are specific embodiments.
[0085] Example 1
[0086] Preparation of battery cells
[0087] (1) Prepare positive electrode active material slurry and negative electrode 3D printing precursor material
[0088] Cathode active material slurry: The positive electrode active material nano-lithium cobalt manganese oxide (LiCoMnO) was prepared by mechanical ball milling with zirconium oxide balls as the ball milling medium at 200 rpm for 12 h. 4 ), the particle size of the obtained nano-lithium cobalt manganese oxide is 40nm. Then, the nano-lithium cobalt manganese oxide, the positive electrode binder PVDF and the conductive agent carbon black are mixed in a mass ratio of 95.3:1.7:3, and added to the N-methylpyrrolidone (NMP) solvent to make the solid content of the slurry 85%, and stirred at 55°C and 500rpm for 0.5h to obtain the positive electrode active material slurry.
[0089] Negative 3D printing precursor material: 3D graphene was prepared by vapor deposition method, the reaction temperature was 1000℃, the holding time was 30min, and the surface area of the obtained 3D graphene was 1100m 2 / g. The three-dimensional graphene and the negative electrode binder PTFE were mixed in a mass ratio of 96:4 as a three-dimensional printing precursor material.
[0090] (2) Preparation of positive electrode sheet
[0091] The positive electrode active material slurry prepared in step (1) is coated on the positive electrode current collector aluminum foil and laser treated by laser induced thermal melting technology, wherein the laser power density is 12 W / cm 2 , the scanning speed is 12mm / s.
[0092] The spray drying technology is used for rapid drying, wherein the drying temperature is 75° C., the air flow velocity of the drying gas is 8 m / s, and the drying time is 40 min to obtain the positive electrode sheet.
[0093] (3) Film formation on the surface of the positive electrode
[0094] Through the atomic layer deposition process, the deposition temperature is 165°C, the reaction cycle is 12 times, and a zinc oxide protective film with a thickness of 11nm is formed on one side of the positive electrode.
[0095] (4) Preparation of negative electrode sheet
[0096] The three-dimensional printing precursor solution prepared in step (1) is used to form a three-dimensional framework structure on the negative electrode current collector copper foil through a three-dimensional printing process, and then the three-dimensional graphene of the negative electrode active material is filled into the three-dimensional framework structure to form a negative electrode active material layer, and then pressed to form a negative electrode sheet. The printing speed in the three-dimensional printing process is 12 mm / s and the temperature is 330°C.
[0097] (5) Surface modification of negative electrode
[0098] Siloxane and fluorinated carbon functional groups are formed on the surface of the negative electrode by plasma enhanced chemical vapor deposition technology. The reaction temperature in the plasma enhanced chemical vapor deposition process is 190°C, the first gas silane and the second gas trifluoromethane are used, the gas flow rates of silane and trifluoromethane are 30sccm and 30sccm respectively, and the modification time is 1.2h.
[0099] (6) Laser cutting
[0100] The film-formed positive electrode sheet and the surface-modified negative electrode sheet are cut into 50mm*65mm sizes using laser cutting technology. The scanning speed of laser cutting is 1200mm / s, and the cutting accuracy is controlled to ±0.1mm.
[0101] (7) Preparation of battery cells
[0102] The positive electrode sheet and separator (Celgard ® 2400) and the surface-modified negative electrode sheets are stacked in order and then hot-pressed to obtain a battery cell. The hot-pressing temperature is 110°C, the pressure is 8MPa, and the pressing time is 10min.
[0103] Lithium battery assembly
[0104] The prepared battery cell is placed in an aluminum shell and sealed with electrolyte to obtain a lithium battery. The electrolyte is a polymer electrolyte, the polymer electrolyte solution concentration is 1wt%, and solvent-free mixing is performed under inert gas, and the specific mass ratio is: 33% dimethyl carbonate, 23% butyl acrylate, 20% dimethylacetamide, 22% lithium hexafluorophosphate, 1% divinyldimethylsilane, 0.5% acrylamide and 0.5% phosphorus trioxide.
[0105] Example 2
[0106] The preparation method of Example 2 is substantially the same as that of Example 1, except that:
[0107] The solid content of the positive electrode active material slurry in step (1) is 80%.
[0108] The laser power density of the laser induced melting technique in step (2) is 10W / cm 2 The scanning speed is 10 mm / s. The drying temperature of the spray drying technology is 80°C and the drying time is 30 min.
[0109] In step (3), the deposition temperature of the atomic layer deposition process is 150° C., the reaction cycle is 11 times, and a 10 nm aluminum fluoride protective film is formed on one side of the positive electrode.
[0110] In step (4), the printing speed in the 3D printing process is 10 mm / s and the temperature is 350°C.
[0111] In step (5), the reaction temperature of the plasma enhanced chemical vapor deposition technology is 180° C., and the gas flow rates of silane and trifluoromethane are 20 sccm and 20 sccm, respectively.
[0112] In step (7), the pressing temperature of the hot pressing treatment is 115° C. and the pressure is 5 MPa.
[0113] Example 3
[0114] The preparation method of Example 3 is substantially the same as that of Example 1, except that:
[0115] The solid content of the positive electrode active material slurry in step (1) is 90%.
[0116] The laser power density of the laser induced thermal melting technology in step (2) is 15W / cm 2 The scanning speed is 11 mm / s. The drying temperature of the spray drying technology is 78°C and the drying time is 35 min.
[0117] In step (3), the deposition temperature of the atomic layer deposition process is 180° C., the reaction cycle is 13 times, and a 12 nm aluminum phosphate protective film is formed on one side of the positive electrode.
[0118] In step (4), the printing speed in the 3D printing process is 11 mm / s and the temperature is 320°C.
[0119] In step (5), the reaction temperature of the plasma enhanced chemical vapor deposition technology is 220° C., and the gas flow rates of silane and trifluoromethane are 40 sccm and 40 sccm, respectively.
[0120] In step (7), the pressing temperature of the hot pressing treatment is 120° C. and the pressure is 10 MPa.
[0121] Example 4
[0122] The preparation method of Example 4 is substantially the same as that of Example 1, except that:
[0123] The laser power density of the laser induced melting technique in step (2) is 9 W / cm 2 , the scanning speed is 13mm / s.
[0124] Example 5
[0125] The preparation method of Example 5 is substantially the same as that of Example 1, except that:
[0126] The laser power density of the laser induced melting technique in step (2) is 16 W / cm 2 , the scanning speed is 9mm / s.
[0127] Example 6
[0128] The preparation method of Example 6 is substantially the same as that of Example 1, except that:
[0129] Step (1) Preparation of lithium cobalt oxide LiCoO 2 , as the positive electrode active material.
[0130] Example 7
[0131] The preparation method of Example 7 is substantially the same as that of Example 1, except that:
[0132] In step (3), the deposition temperature of the atomic layer deposition process is 140° C., the reaction cycle is 8 times, and a 9 nm zinc oxide protective film is formed on one side of the positive electrode.
[0133] Example 8
[0134] The preparation method of Example 8 is substantially the same as that of Example 1, except that:
[0135] In step (3), the deposition temperature of the atomic layer deposition process is 190° C., the reaction cycle is 14 times, and a 13 nm aluminum fluoride protective film is formed on one side of the positive electrode.
[0136] Example 9
[0137] The preparation method of Example 9 is substantially the same as that of Example 1, except that:
[0138] In step (5), the reaction temperature of the plasma enhanced chemical vapor deposition technology is 170°C.
[0139] Example 10
[0140] The preparation method of Example 10 is substantially the same as that of Example 1, except that:
[0141] In step (5), the reaction temperature of the plasma enhanced chemical vapor deposition technology is 230°C.
[0142] Embodiment 11
[0143] The preparation method of Example 11 is substantially the same as that of Example 1, except that:
[0144] In step (5), the gas flow rates of silane and trifluoromethane are 15 sccm and 15 sccm, respectively.
[0145] Example 12
[0146] The preparation method of Example 12 is substantially the same as that of Example 1, except that:
[0147] In step (5), the gas flow rates of silane and trifluoromethane are 45 sccm and 45 sccm, respectively.
[0148] Embodiment 13
[0149] The preparation method of Example 13 is substantially the same as that of Example 1, except that:
[0150] In step (5), only the first gas silane is introduced in the plasma enhanced chemical vapor deposition technology, that is, only the siloxane groups are modified on the surface of the negative electrode.
[0151] Embodiment 14
[0152] The preparation method of Example 14 is substantially the same as that of Example 1, except that:
[0153] In step (5), only difluoromethane is introduced as the second gas in the plasma enhanced chemical vapor deposition technology, that is, only the fluorinated carbon groups are modified on the surface of the negative electrode.
[0154] Comparative Example 1
[0155] The preparation method of Comparative Example 1 is substantially the same as that of Example 1, except that:
[0156] No laser treatment was performed in step (2).
[0157] Comparative Example 2
[0158] The preparation method of Comparative Example 2 is substantially the same as that of Example 1, except that:
[0159] The process does not include step (3), i.e., no protective film is formed on the positive electrode plate.
[0160] Comparative Example 3
[0161] The preparation method of Comparative Example 3 is substantially the same as that of Example 1, except that:
[0162] In step (4), no three-dimensional printing process is performed. Instead, the negative electrode sheet is prepared using existing technology. Specifically, the three-dimensional graphene as the negative electrode active material and the negative electrode binder PTFE are mixed in a mass ratio of 97:3, and N-methylpyrrolidone (NMP) is added as a solvent to prepare a slurry with a solid content of 50%. The slurry is coated on the negative electrode current collector copper foil, and then further oven dried.
[0163] Comparative Example 4
[0164] The preparation method of Comparative Example 4 is substantially the same as that of Example 1, except that:
[0165] Step (5) is not included, that is, no functional groups are modified on the surface of the negative electrode.
[0166] The raw materials and process parameters in the preparation methods of Examples 1 to 14 and Comparative Examples 1 to 4 are listed in Table 1 below:
[0167] Table 1
[0168]
[0169] The battery cells or batteries prepared in Examples 1 to 14 and Comparative Examples 1 to 4 were subjected to performance tests, and the test results are shown in Table 2 below.
[0170] Among them, the test conditions or test standards for each performance test item are:
[0171] The test method for the 0.1C charging capacity at room temperature is as follows: In a 25°C constant temperature box, charge the battery at a constant current of 0.1C to an upper voltage limit of 4.2V, and record the charging capacity.
[0172] The test method for the 0.1C discharge capacity at room temperature is as follows: in a constant temperature box at 25°C, a fully charged battery is discharged at 0.1C to a cut-off voltage of 3.0V, and the discharge capacity is recorded.
[0173] The test method for 1C charging capacity at room temperature is: in a 25℃ constant temperature box, charge the battery at a 1C constant current to an upper limit voltage of 4.2V, and record the charging capacity.
[0174] The test method for 1C discharge capacity at room temperature is: in a constant temperature box at 25℃, discharge the fully charged battery at 1C to a cut-off voltage of 3.0V, and record the discharge capacity.
[0175] The test method for the discharge capacity retention rate after 100 cycles at 25°C is as follows: in a constant temperature box at 25°C, the battery is charged using a constant current and constant voltage charging method, with a constant current of 1C, and the constant voltage charging is stopped when the charging cut-off voltage reaches 1 / 30C; let it stand for 20 minutes; discharge at 1C to 3.0V; let it stand for 20 minutes. Repeat the above steps and record the discharge capacity after 100 cycles.
[0176] The test method for the discharge capacity retention rate after 100 cycles at 55°C is as follows: in a constant temperature box at 55°C, the battery is charged using a constant current and constant voltage charging method, with a constant current of 1C, and the constant voltage charging is stopped when the charging cut-off voltage reaches 1 / 30C; let it stand for 20 minutes; discharge at 1C to 3.0V; let it stand for 20 minutes. Repeat the above steps and record the discharge capacity after 100 cycles.
[0177] The test method for the discharge capacity retention rate after 1000 cycles at 25°C is as follows: in a constant temperature box at 25°C, the battery is charged using a constant current and constant voltage charging method, with a constant current of 1C, and the constant voltage charging is stopped when the charging cut-off voltage reaches 1 / 30C; let it stand for 20 minutes; discharge at 1C to 3.0V; let it stand for 20 minutes. Repeat the above steps and record the discharge capacity after 1000 cycles.
[0178] Table 2
[0179]
[0180] As can be seen from Table 2 above, the capacity and cycle retention rate of Examples 1 to 14 are higher than those of Comparative Examples 1 to 4, indicating that in the battery cell preparation method provided in the present application, laser treatment can improve the durability and stability of the bonding between the positive electrode active material layer and the positive electrode current collector, and at the same time, a nano protective film is formed on the surface of the positive electrode plate. The nano protective film avoids excessive loss of positive electrode active materials and improves cycle stability. A three-dimensional framework structure formed by negative electrode active materials and negative electrode binders is formed by a three-dimensional printing process, and then the negative electrode active materials are filled into the three-dimensional framework structure, which can increase the proportion of negative electrode active materials in the negative electrode active material layer, thereby increasing the energy density of the battery. At the same time, the surface of the negative electrode plate is modified to form functional groups, which can reduce negative electrode interface side reactions, extend the service life of the battery, improve cycle performance, and improve the conductivity of the surface of the negative electrode plate, thereby increasing the battery capacity.
[0181] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0182] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.
Claims
1. A method for preparing a battery cell, characterized in that: The method comprises the following steps: S11, preparing a positive electrode sheet: coating a positive electrode active material slurry on a positive electrode current collector, laser processing, partially curing the positive electrode active material slurry to bond with the positive electrode current collector, and drying to form a positive electrode active material layer to obtain a positive electrode sheet; S12, forming a film on the surface of the positive electrode sheet: forming a nano protective film on the surface of the positive electrode sheet prepared in step S11; S13, preparing a negative electrode sheet: forming a three-dimensional framework structure formed by a negative electrode active material and a negative electrode binder on a negative electrode current collector through a three-dimensional printing process, then filling the negative electrode active material into the three-dimensional framework structure to form a negative electrode active material layer, and press-forming to obtain a negative electrode sheet; S14, surface modification of the negative electrode plate: performing surface modification treatment on the negative electrode plate prepared in step S13 to form functional groups; S15, preparing a battery cell: laminating the surface-filmed positive electrode sheet and the separator prepared in step S12 and the surface-modified negative electrode sheet prepared in step S14, and then performing hot pressing treatment to obtain a battery cell.
2. The preparation method according to claim 1, characterized in that: The positive electrode active material slurry formed in step S11 has a solid content of 80% to 90%.
3. The preparation method according to claim 1, characterized in that: The laser power density of the laser treatment in step S11 is 10 W / cm 2 ~15W / cm 2 , the scanning speed is 10mm / s~12mm / s.
4. The preparation method according to claim 1, characterized in that: The material of the nano protective film formed in step S12 is one or more of metal oxides, metal fluorides, and metal phosphate compounds.
5. The preparation method according to claim 4, characterized in that: The nano protective film is obtained by an atomic layer deposition process, in which the deposition temperature is 150° C. to 180° C. and the reaction cycle is 9 to 13 cycles.
6. The preparation method according to claim 1, 4 or 5, characterized in that: The thickness of the nano protective film is 10nm-12nm.
7. The preparation method according to claim 1, characterized in that: In step S14, the functional group includes one or a combination of a siloxane group and a trifluoromethyl group.
8. The preparation method according to claim 7, characterized in that: In step S14, a plasma enhanced chemical vapor deposition process is used to perform surface modification treatment on the negative electrode plate by mixing the first gas and / or the second gas, wherein the plasma enhanced chemical vapor deposition process satisfies at least one of the following (i) to (vi): (i) The reaction temperature is 180°C to 200°C; (ii) the first gas can modify siloxane groups on the surface of the negative electrode plate, including any one of silane, dichlorosilane, trichlorosilane, and silicon chloride; (iii) the second gas can modify the trifluoromethyl group on the surface of the negative electrode plate, including any one of hydrogen fluoride, difluoromethane, trifluoromethane, and carbon tetrafluoride; (iv) the flow rate of the first gas is 20-40 sccm; (v) the flow rate of the second gas is 20-40 sccm; (vi) The deposition time is 1h to 1.5h.
9. The preparation method according to claim 1, characterized in that: In the three-dimensional framework structure formed in step S13, the mass proportion of the negative electrode active material is 95% to 98%, and the mass proportion of the negative electrode binder is 2% to 5%.
10. A battery, characterized in that: The battery comprises a battery cell prepared by the preparation method according to any one of claims 1 to 9.