Solid electrolyte diaphragm and battery formation method

By using a solid electrolyte coating with high content of LATP and a modified polyolefin-based film on the lithium-ion battery separator, a dense thermal stability protective layer is formed, which solves the problem of thermal runaway for lithium-ion batteries at high temperatures and improves battery safety Performance and cycling performance.

CN118943472APending Publication Date: 2024-11-12东莞维科电池有限公司

Patent Information

Application Number
CN202410906833.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Lithium-ion batteries are prone to thermal runaway at high temperatures. Traditional polyolefin separators will shrink or melt, causing short circuits of positive and negative electrodes. Although existing ceramic coatings can inhibit heat shrinkage, they hinder lithium ion transmission and reduce battery capacity retention.

Method used

A solid electrolyte separator is used, the coating consists of 80% to 95% LATP or mixtures, the thickness and surface density meet a specific ratio, forming a dense thermal stability protective layer, combined with a modified polyolefin base film, improving lithium ion conductivity and thermal stability.

Benefits of technology

Effectively suppresses thermal shrinkage and deformation of the diaphragm, improves the safety boundary of thermal runaway of the battery, reduces internal resistance, enhances circulation performance and stability, and extends battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943472A_ABST
    Figure CN118943472A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of batteries, and particularly relates to a solid electrolyte diaphragm which comprises a base membrane and a solid electrolyte coating coated on at least one surface of the base membrane, the solid electrolyte coating comprises a solid electrolyte, and the solid electrolyte accounts for 80%-95% of the mass of the solid electrolyte coating; the solid electrolyte is LATP or a mixture formed by LATP and at least one of LLZO, LLTO and LAGP. Through the arrangement of the solid electrolyte coating, when the battery is formed, the solid electrolyte coating can form a compact thermal stability protection layer, so that the thermal shrinkage deformation of the diaphragm can be inhibited, the thermal runaway safety boundary of the battery is improved, and the ion conduction performance of the solid electrolyte coating is good. In addition, the invention also discloses a battery formation method for improving the thermal stability of the solid electrolyte diaphragm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries, and in particular relates to a solid electrolyte diaphragm and a battery formation method. Background Art

[0002] Lithium-ion batteries have been increasingly widely used in mobile phones, computers, tablets, Bluetooth headsets, power tools, automobiles, energy storage and other fields. Users have put forward higher requirements for the energy density of lithium-ion batteries. As the energy density of lithium-ion batteries continues to increase, the problem of thermal runaway has become increasingly prominent, and the thermal runaway problem has become a bottleneck restricting the further development of batteries. At high temperatures such as 110°C, traditional polyolefin separators will shrink or even melt, causing direct contact between the positive and negative electrodes of the battery, resulting in a short circuit, which in turn causes thermal runaway and ultimately a safety accident, endangering the lives and property of users.

[0003] At present, the base film of lithium-ion battery separators generally uses polyolefin or modified polyolefin materials, such as PP, PE, PP / PE / PP, etc., and needs to be coated with a layer of ceramics such as boehmite, aluminum oxide, magnesium oxide, silicon oxide, calcium oxide, etc. on its surface to inhibit the thermal shrinkage deformation of the separator. However, these ceramics will hinder the transmission of lithium ions in the battery, resulting in an increase in battery impedance and a decrease in capacity retention.

[0004] Based on this, there is an urgent need to invent a solid electrolyte membrane to solve the aforementioned technical problems. Summary of the invention

[0005] One of the purposes of the present invention is to provide a solid electrolyte membrane with excellent lithium ion conductivity, suppress thermal shrinkage deformation of the membrane, and improve the thermal runaway safety margin of the battery in order to address the deficiencies of the prior art.

[0006] In order to solve the above technical problems, this application adopts the following technical solutions:

[0007] A solid electrolyte membrane comprises a base membrane and a solid electrolyte coating coated on at least one surface of the base membrane;

[0008] The solid electrolyte coating comprises a solid electrolyte, and the solid electrolyte accounts for 80% to 95% by mass of the solid electrolyte coating;

[0009] The solid electrolyte is LATP, or a mixture of LATP and at least one of LLZO, LLTO and LAGP.

[0010] Specifically, the thickness H1 of the solid electrolyte coating and the thickness H2 of the base film satisfy the relationship: H1 / H2≥10%; the surface density w1 of the solid electrolyte coating and the surface density w2 of the base film satisfy the relationship: w1 / w2≥50%.

[0011] Specifically, the thickness of the solid electrolyte coating is 0.5-5 μm, and the surface density is 2-4 g / m 2 The thickness of the base film is 4 to 10 um, and the surface density is 1.8 to 3.8 g / m 2 .

[0012] Specifically, the structural formula of the LATP is Li 1+x Al x Ti 2-x (PO4)3, where x ranges from 0 to 0.5.

[0013] Specifically, the LATP is Li 1.5 Al 0.5 Ti 1.5 (PO4)3、Li 1.4 Al 0.4 Ti 1.6 (PO4)3 or Li 1.3 Al 0.3 Ti 1.7 (PO4)3, the LLZO is Li7La3Zr2O 12 , the LLTO is Li 0.5 La 0.5 TiO3 or Li 0.33 La 0.557 TiO3, the LAGP is Li 1.5 Al 0.5 Ge 1.5 (PO4)3.

[0014] Specifically, the base film is polyolefin or modified polyolefin material.

[0015] Specifically, the base film has a porosity of 20% to 40%, an air permeability of 180 to 300 sec / 100 cc, a needle puncture strength greater than or equal to 200 gf, and a longitudinal tensile strength greater than or equal to 2000 kgf / cm 2 , transverse tensile strength greater than or equal to 1800kgf / cm 2 , the longitudinal elongation is greater than or equal to 30%, the transverse elongation is greater than or equal to 30%, and the melting point is greater than or equal to 135°C.

[0016] Specifically, the solid electrolyte coating further includes a water-based binder or an oil-based binder with a mass fraction of 5% to 20%, the water-based binder is one or more of PMMA, PAA, SBR, and CMC, and the oil-based binder is PVDF.

[0017] Specifically, the solid electrolyte membrane includes a first state and a second state, the first state is the state of the solid electrolyte membrane before formation, and the second state is the state of the solid electrolyte membrane after formation. In the second state, a dense thermal stability protective layer is formed on the surface of the solid electrolyte membrane.

[0018] The beneficial effects of the present invention are as follows: through the provision of a solid electrolyte coating, when the battery is formed, the solid electrolyte coating will form a dense thermal stability protective layer, which can inhibit the thermal shrinkage deformation of the diaphragm, increase the temperature of the thermal runaway safety boundary of the battery, and improve the thermal stability of the diaphragm. In addition, the solid electrolyte coating has good ion conductivity, which can effectively reduce the internal resistance and improve the cycle performance.

[0019] The second object of the present invention is to provide a battery formation method for improving the thermal stability of the above-mentioned solid electrolyte membrane, comprising the following steps:

[0020] Step 1: Under a preset heating temperature and pressure, a voltage in the range of 4.0 to 5.0 V is applied to the electrodes of the battery to be formed, and the battery is charged at a first charging rate for a first preset time;

[0021] Step 2: Under a preset heating temperature and pressure, a voltage in the range of 4.0 to 5.0 V is applied to the electrodes of the battery to be formed, and the battery is charged at a second charging rate for a second preset time;

[0022] Step 3: Under a preset heating temperature and pressure, a voltage in the range of 4.0 to 5.0 V is applied to the electrodes of the battery to be formed, and the battery is charged at a third charging rate for a third preset time;

[0023] Wherein, the battery is preset to be left for a predetermined time between adjacent steps, the second charging rate is greater than the first charging rate, and the third charging rate is greater than the second charging rate.

[0024] Specifically, the heating temperature is 70-90°C, the pressurization pressure is 0.3-2MPa, the first charging rate range is 0.1-0.5C, the second charging rate range is 0.5-1.5C, the third charging rate range is 1-3C, the first preset time range is 1-3min, the second preset time range is 2-4min, the third preset time range is 20-30min, and the shelf time is 5-60s. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0026] Figure 1 It is a schematic structural diagram of the solid electrolyte membrane in the present invention;

[0027] Figure 2 It is a schematic diagram of the structure of the solid electrolyte membrane after battery formation in the present invention;

[0028] Figure 3 This is a schematic diagram of the thermal runaway mechanism of the diaphragm in Comparative Example 1 of the present invention;

[0029] Figure 4 Schematic diagram of thermal runaway mechanism of the solid electrolyte membrane of the present invention;

[0030] Among them: 1-base film; 2-solid electrolyte coating; 3-thermal stability protective layer. DETAILED DESCRIPTION

[0031] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by technicians in the technical field of the present application. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application.

[0032] The present invention will be further described in detail below in conjunction with the accompanying drawings, but this is not intended to limit the present invention.

[0033] Battery thermal runaway refers to the phenomenon that the battery temperature rises uncontrollably due to the chain reaction of heat release from battery cells, which is usually induced by mechanical, electrical, thermal and other factors alone or in combination. When the battery accumulates heat under the action of inducing factors, it is called the heat accumulation stage, also known as the self-heating stage; when the temperature exceeds the temperature range of the battery design, side reactions inside the battery will continue to occur and release a large amount of heat, thereby causing thermal runaway. The development process of thermal runaway at this stage can be roughly summarized as SEI film decomposition, diaphragm melting, Li / LixC6 and electrolyte reaction, among which diaphragm melting is considered to be the beginning of thermal runaway, and the temperature at which the diaphragm melts is lower than that at which the SEI film decomposition and Li / LixC6 and electrolyte reaction occur. Therefore, to increase the temperature boundary of battery thermal runaway, the first thing to do is to increase the temperature of the diaphragm melting. The existing diaphragms are generally made of PP, PE, PP / PE / PP, etc. These materials have low melting points and are easily deformed after being heated. After the diaphragm melts and deforms, a short circuit will occur between the positive and negative electrodes of the battery, and the heating rate will increase rapidly. The violent reaction will generate a large amount of gas and release a large amount of heat. After heating, the rapidly expanding gas will break through the battery core shell, causing material spray or even combustion. The existing technology suppresses the thermal shrinkage deformation of the diaphragm by coating a layer of ceramics such as boehmite, aluminum oxide, magnesium oxide, silicon oxide, calcium oxide, etc. on the surface of the diaphragm. However, these ceramics will hinder the transmission of lithium ions in the battery, resulting in an increase in battery impedance and a decrease in capacity retention.

[0034] like Figure 1 As shown, the present application sets a solid electrolyte coating 2 on the surface of the diaphragm, and when the battery is formed, the solid electrolyte coating 2 will form a dense thermal stability protective layer 3. The dense thermal stability protective layer 3 will play a self-supporting role for the diaphragm, inhibit the thermal shrinkage deformation of the diaphragm, greatly reduce the thermal shrinkage rate of the diaphragm, and greatly reduce the probability of internal short circuit caused by thermal deformation of the diaphragm, thereby improving the thermal runaway safety margin of the battery, and the solid electrolyte coating 2 has good ionic conductivity.

[0035] According to the first aspect of the present application, the present invention provides a solid electrolyte membrane, comprising a base membrane 1 and a solid electrolyte coating 2 coated on at least one surface of the base membrane 1; the solid electrolyte coating 2 comprises a solid electrolyte, and the solid electrolyte accounts for 80% to 95% by mass of the solid electrolyte coating 2; the exemplary solid electrolyte accounts for 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95% by mass of the solid electrolyte coating 2. Within the above range, the solid electrolyte coating 2 can improve the ion conductivity, help reduce resistance, improve the rate performance of the battery, and enhance the cycle stability. The solid electrolyte coating 2 can provide a protective layer, reduce the loss of electrolyte and overflow during the cycle, reduce the internal chemical reaction of the battery and the loss of electrolyte, extend the cycle life of the battery, and improve the reliability and stability of the battery. The solid electrolyte is LATP, or a mixture of LATP and at least one of LLZO, LLTO, and LAGP. When the solid electrolyte is only LATP, LATP accounts for 80% to 95% of the mass percentage of the solid electrolyte coating 2. In some embodiments, when the solid electrolyte is LATP and at least one of LLZO, LLTO, and LAGP, a mixture of 60% to 85% of LATP and 10% to 20% of one or more of LLZO, LLTO, and LAGP is selected.

[0036] During the battery formation process, the solid electrolyte coating 2 with the solid electrolyte added thereto reacts with the electrolyte, titanium is reduced, and Ti 4+ Become Ti 3+ , and the generated LiF, Li2CO3, organic lithium salts, etc. can further fill the gaps between the coating particles and form a dense thermal stability protective layer 3. The solid electrolyte ratio under the above mass percentage is appropriate, and the generated thermal stability protective layer 3 has good thermal stability, which can provide support for the base film 1, prevent the base film 1 from being greatly deformed at high temperature and causing short circuit, increase the thermal stability boundary temperature of the diaphragm, and improve the safety performance of the battery.

[0037] X-ray photoelectron spectroscopy (XPS) can analyze the chemical composition changes of the solid electrolyte coating 2 before and after the formation. After the reaction, LiF, Li2CO3, organic lithium salts, etc. appear in the solid electrolyte coating 2. 4+ Become Ti 3+ , and PO4 3- No changes.

[0038] Among them, LATP:Li 1+x Al x Ti 2-x(PO4)3 is a ceramic material composed of five elements: lithium (Li), aluminum (Al), titanium (Ti), phosphorus (P) and oxygen (O). In this chemical formula, the proportion of each element varies depending on the value of x, but in general, the proportions of lithium and phosphorus are higher because they occupy most of the positions in the chemical formula respectively. The proportions of titanium and aluminum are relatively low, but they are very important for forming the crystal structure of LATP. The lithium ions in the crystal structure usually act as mobile ions in the battery and are transported through the solid phase interface to realize the charging and discharging process of the battery. LLZO: There are two crystal structures, cubic phase (c-LLZO) and tetragonal phase (t-LLZO), of which the ionic conductivity of the cubic phase is higher than that of the tetragonal phase. In the cubic phase of LLZO, lithium ions partially occupy the interstitial sites, while in the tetragonal phase, lithium ions occupy all the interstitial sites. The cubic phase of LLZO has a higher ionic conductivity, which is mainly due to the rapid migration of lithium ions in its crystal skeleton network. LLTO: It is a perovskite material with high ionic conductivity. It has important application potential in all-solid-state lithium-ion batteries. Its crystal structure is a tetragonal perovskite structure with good chemical stability and high ionic conductivity. However, there are some challenges in its preparation process, such as disordered growth and arrangement of crystals, and high sintering temperature. LAGP: It is a solid electrolyte material with high ionic conductivity and belongs to the NASICON structure. It has excellent chemical stability, a wider electrochemical window and is non-flammable.

[0039] In one embodiment of the present application, the structural formula of LATP is Li 1+x Al x Ti 2-x (PO4)3, where the value of X is usually in the range of 0≤x≤0.5, such as X=0.1, 0.2, 0.3, 0.4, 0.5. Changes within this range affect the crystal structure and conductivity characteristics of the material. In practical applications, adjusting the value of X can optimize the performance of the material, making it more suitable as a component of a battery or other electronic device. As X increases, the number of aluminum atoms increases, while the number of titanium atoms decreases accordingly. This structure is characterized by a three-dimensional skeleton formed by the connection of TiO6 octahedrons and PO4 tetrahedrons with common vertices. The connection mode of each TiO6 octahedron and PO=tetrahedron determines the crystal structure of the entire material. In the chemical composition of this material, the ratio of aluminum to titanium is adjusted by the value of x to achieve specific physical and chemical properties. When x is within this range, LATP has better ionic conductivity, better crystal structure stability, and good chemical stability.

[0040] Taking into account the stability of the crystal structure and the charge balance, the range of X is ≤ 0.5. 1+x Al x Ti 2-xIn the structure of (PO4)3, each PO4 tetrahedral unit carries a negative charge, and Li + 、Al 3+ and Ti 4+ They carry positive charges of +1, +3, and +4, respectively. In order to maintain the electrical neutrality of the entire structure, the positive and negative charges must offset each other. If the X value is too large, it means that the number of aluminum ions increases, while the number of titanium ions decreases, which will result in insufficient total positive charge and cannot completely offset the negative charge of the PO4 tetrahedral unit, thereby destroying the charge balance and stability of the crystal. In addition, the increase in the X value may also affect other properties of the material, such as thermal stability, mechanical strength, and electrical conductivity. Therefore, in order to ensure that the material has good comprehensive properties, the range of X is usually limited to a certain range, usually not exceeding 0.5.

[0041] In one embodiment according to the present application, LATP is Li 1.5 Al 0.5 Ti 1.5 (PO4)3、Li 1.4 Al 0.4 Ti 1.6 (PO4)3 or Li 1.3 Al 0.3 Ti 1.7 (PO4)3, LLZO is Li7La3Zr2O 12 LLTO is Li 0.5 La 0.5 TiO3 or Li 0.33 La 0.557 TiO3, LAGP for Li 1.5 Al 0.5 Ge 1.5 (PO4)3, the selection of the above-mentioned solid electrolyte materials makes the performance of the solid electrolyte coating 2 better and can form a denser thermal stability protective layer 3.

[0042] The thickness H1 of the solid electrolyte coating 2 and the thickness H2 of the base film 1 satisfy the relationship: H1 / H2≥10%; the surface density w1 of the solid electrolyte coating 2 and the surface density w2 of the base film 1 satisfy the relationship: w1 / w2≥50%. These requirements are intended to ensure that the solid electrolyte coating 2 can effectively cover the base film 1 and provide sufficient ion conduction channels, thereby optimizing the performance of the solid electrolyte diaphragm. After satisfying the above relationship, the generated thermal stability protective layer 3 can provide sufficient support for the diaphragm.

[0043] In one embodiment of the present application, the thickness of the solid electrolyte coating 2 is 0.5-5 μm, and the surface density is 2-4 g / m 2 The thickness of the base film 1 is 4 to 10 μm, and the surface density is 1.8 to 3.8 g / m 2When the thickness and surface density of the solid electrolyte coating 2 and the base film 1 are within the above ranges, the solid electrolyte separator has good thermal stability and lithium ion conductivity.

[0044] In one embodiment of the present application, the base film 1 is a polyolefin or a modified polyolefin material, such as PP, PE, PP / PE / PP.

[0045] In one embodiment of the present application, the porosity of the base film 1 is 20% to 40%, the air permeability is 180 to 300 sec / 100 cc, the needle puncture strength is greater than or equal to 200 gf, and the longitudinal tensile strength is greater than or equal to 2000 kgf / cm 2 , transverse tensile strength greater than or equal to 1800kgf / cm 2 , the longitudinal elongation is greater than or equal to 30%, the transverse elongation is greater than or equal to 30%, and the melting point is greater than or equal to 135°C. Matching the base film 1 and the solid electrolyte coating 2 can improve the solid electrolyte membrane and ensure that it has stable performance and reliable mechanical support during use.

[0046] Specifically, the solid electrolyte coating 2 further includes a water-based binder or an oil-based binder with a mass fraction of 5% to 20%, the water-based binder is one or more of PMMA, PAA, SBR, and CMC, and the oil-based binder is PVDF.

[0047] like Figure 2 As shown, the solid electrolyte membrane includes a first state and a second state. The first state is the state of the solid electrolyte membrane before formation, and the second state is the state of the solid electrolyte membrane after formation. In the second state, a dense thermal stability protective layer 3 is formed on the surface of the solid electrolyte membrane.

[0048] In a high temperature environment (≥110°C), the dense thermal stability protective layer 3 will play a self-supporting role for the diaphragm, inhibit the thermal shrinkage deformation of the diaphragm, and greatly reduce the thermal shrinkage rate of the diaphragm, so that the probability of internal short circuit caused by thermal deformation of the diaphragm is greatly reduced. At the same time, since the short circuit caused by the thermal shrinkage deformation of the diaphragm that is easy to occur at lower temperatures is solved, the cause of thermal runaway of the battery is transformed into the thermal decomposition and oxygen release reaction of the positive electrode that requires a higher temperature, so that the thermal runaway safety margin can be increased from 130°C to 150°C.

[0049] like Figure 3 and Figure 4As shown, the ceramic-coated diaphragm experienced thermal runaway at 130°C for 1h, and the ceramic coating and the base membrane 1 were damaged to varying degrees. However, the solid electrolyte coating diaphragm had a dense thermal stability protective layer 3 that was self-supporting, which suppressed the thermal shrinkage deformation of the diaphragm and greatly reduced the thermal shrinkage rate of the diaphragm. Although the solid electrolyte coating 2 and the base membrane 1 were damaged to varying degrees at 130°C for 1h, the thermal stability protective layer 3 remained intact, greatly reducing the probability of internal short circuit caused by thermal deformation of the diaphragm, and the thermal runaway temperature was increased to 150°C.

[0050] According to a second aspect of the present application, the present application provides a battery formation method for improving the thermal stability of the above-mentioned solid electrolyte membrane, comprising the following steps:

[0051] Step 1: Under a preset heating temperature and pressure, a voltage in the range of 4.0 to 5.0 V is applied to the electrodes of the battery to be formed, and the battery is charged at a first charging rate for a first preset time;

[0052] Step 2: Under a preset heating temperature and pressure, a voltage in the range of 4.0 to 5.0 V is applied to the electrodes of the battery to be formed, and the battery is charged at a second charging rate for a second preset time;

[0053] Step 3: Under a preset heating temperature and pressure, a voltage in the range of 4.0 to 5.0 V is applied to the electrodes of the battery to be formed, and the battery is charged at a third charging rate for a third preset time;

[0054] Among them, the battery is placed for a preset placement time between adjacent steps, the second charging rate is greater than the first charging rate, and the third charging rate is greater than the second charging rate. Using a lower charging rate in the first step helps to avoid material damage, improve molding efficiency, and ensure that the chemical process inside the battery can be fully carried out. As the molding process proceeds, gradually increasing the charging rate can help further activate the battery material and promote the reaction inside the battery, so that the generated thermal stability protective layer 3 has better compactness.

[0055] Specifically, the heating temperature is 70-90°C, the pressurization pressure is 0.3-2MPa, the first charging rate range is 0.1-0.5C, the second charging rate range is 0.5-1.5C, the third charging rate range is 1-3C, the first preset time range is 1-3min, the second preset time range is 2-4min, the third preset time range is 20-30min, and the shelf time is 5-60s.

[0056] The formation conditions for forming the dense thermal stability protective layer 3 are: temperature 80°C ± 10°C, pressure 0.3-2MPa, example - 2C rate fast charging battery, the process is shown in Table 1:

[0057] Table 1

[0058]

[0059] Preparation method of diaphragm:

[0060] 1) Select a suitable solid electrolyte and prepare it into an oil-based or water-based coating slurry.

[0061] 2) The coating slurry is evenly coated on the surface of the base film PE by a coating process to form a solid electrolyte coating.

[0062] 3) The coated diaphragm is dried, heat treated and other processes are performed to ensure a close bond between the coating and the diaphragm.

[0063] 4.) The prepared coated diaphragm is applied to the lithium battery and subjected to the formation process. During this process, the solid electrolyte coating reacts with the electrolyte to form a dense, thermally stable protective layer.

[0064] 5) Performing performance tests on the prepared lithium battery, including thermal stability test, thermal abuse safety test and electrochemical performance test, etc., to verify the actual effect of the present invention.

[0065] Preferably, the components of the electrolyte selected during formation of the battery of the present application are: 1) lithium salt: the main component of the electrolyte, which is responsible for providing lithium ions. Such as lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium pentafluorophosphate (LiPF5), lithium difluorophosphate (LiPF2), etc.; 2) organic solvent: organic solvent is another important component of the electrolyte, which plays the role of dissolving lithium salts and providing lithium ion transmission medium. Commonly used organic solvents include carbonates (such as vinyl acetate (EC), ethyl acrylate (EMC), dimethyl carbonate (DMC), ethylene carbonate (DEC), etc.); 3) additives: in order to improve the performance and safety of the battery, some additives are usually added to the electrolyte. These additives can be film-forming additives, overcharge protection agents, flame retardants, etc., such as succinonitrile, adiponitrile, 1,3,6-hexanetrinitrile, etc., which can form a protective film on the electrode surface, inhibit side reactions, and improve the cycle life and safety of the battery.

[0066] The present invention is further described in detail below in conjunction with specific embodiments.

[0067] Example 1

[0068] Follow these steps to prepare the battery:

[0069] 1. Prepare positive electrode slurry and negative electrode slurry respectively;

[0070] 2. Coat the positive electrode slurry on the surface of the positive electrode collector, and then dry, roll and cut in sequence to obtain a positive electrode sheet; coat the negative electrode slurry on the surface of the negative electrode collector, and then dry, roll and cut in sequence to obtain a negative electrode sheet.

[0071] 3. 90wt% solid electrolyte Li 1.5 Al 0.5 Ti 1.5 (PO4)3 and 10wt% of aqueous binder PMMA were mixed to prepare a coating slurry, and the coating slurry was evenly coated on the surface of the base film PE by a coating process to form a solid electrolyte coating. The coated diaphragm was dried, heat treated and other processes were performed to ensure the close combination of the coating and the diaphragm to obtain a solid electrolyte diaphragm, wherein the thickness of the solid electrolyte coating was 3um and the surface density was 3g / m 2 The thickness of the base film is 7um and the surface density is 2.5g / m 2 .

[0072] 4. Battery preparation: The above-mentioned positive electrode sheet, solid electrolyte membrane, and negative electrode sheet are wound or stacked to produce a bare battery cell, which is then packaged and injected with electrolyte to produce a lithium-ion battery.

[0073] The electrolyte comprises lithium salt - LiPF6, 1.1 mol / L; solvent - ethyl acrylate (EMC): dimethyl carbonate (DMC): diethyl carbonate (DEC) = 5:3:2; additive: adiponitrile.

[0074] 5. Battery formation: The lithium-ion battery is formed according to the above-mentioned battery formation method to obtain a finished lithium-ion battery.

[0075] Example 2

[0076] The difference from Example 1 is that 80 wt% of the solid electrolyte Li 1.5 Al 0.5 Ti 1.5 (PO4)3 and 20 wt% of aqueous binder PMMA were mixed to prepare a coating slurry.

[0077] The other steps are the same as those in Example 1 and will not be described in detail in this example.

[0078] Example 3

[0079] The difference from Example 1 is that 80 wt% of the solid electrolyte Li 1.5 Al 0.5 Ti 1.5 (PO4)3, 3wt% solid electrolyte Li7La3Zr2O 12 , 3wt% solid electrolyte Li 0.5 La0.5 TiO3, 4wt% solid electrolyte Li 1.5 Al 0.5 Ge 1.5 (PO4)3 and 10 wt% of aqueous binder PMMA were mixed to prepare a coating slurry.

[0080] The other steps are the same as those in Example 1 and will not be described in detail in this example.

[0081] Example 4

[0082] The difference from Example 1 is that the thickness of the solid electrolyte coating is 2um and the surface density is 2g / m 2 The thickness of the base film is 9um and the surface density is 3g / m 2 .

[0083] The other steps are the same as those in Example 1 and will not be described in detail in this example.

[0084] Comparative Example 1

[0085] Follow these steps to prepare the battery:

[0086] 1. Prepare positive electrode slurry and negative electrode slurry respectively;

[0087] 2. Coat the positive electrode slurry on the surface of the positive electrode collector, and then dry, roll and cut in sequence to obtain a positive electrode sheet; coat the negative electrode slurry on the surface of the negative electrode collector, and then dry, roll and cut in sequence to obtain a negative electrode sheet.

[0088] 3. 90 wt% of boehmite and 10 wt% of water-based binder PMMA were mixed to prepare a coating slurry, and the coating slurry was evenly coated on the surface of the base film PE by a coating process to form a ceramic coating. The coated diaphragm was dried, heat treated and other processes were performed to ensure that the coating and the diaphragm were tightly bonded to obtain a ceramic diaphragm, wherein the thickness of the ceramic coating was 3 um and the surface density was 3 g / m 2 The thickness of the base film is 7um and the surface density is 2.5g / m 2 .

[0089] 4. Battery preparation: The above positive electrode sheet, separator, and negative electrode sheet are wound or stacked to produce a bare cell, which is then packaged and injected with electrolyte to produce a lithium-ion battery.

[0090] The electrolyte comprises lithium salt - LiPF6, 1.1 mol / L; solvent - ethyl acrylate (EMC): dimethyl carbonate (DMC): diethyl carbonate (DEC) = 5:3:2; additive: adiponitrile.

[0091] 5. Battery formation: The lithium-ion battery is formed according to the above-mentioned battery formation method to obtain a finished lithium-ion battery.

[0092] Comparative Example 2

[0093] The difference from Comparative Example 1 is that 30 wt% of the solid electrolyte Li 1.5 Al 0.5 Ti 1.5 (PO4)3 and 70wt% of aqueous binder PMMA are mixed to prepare a coating slurry, and the coating slurry is evenly coated on the surface of the base film PE by a coating process to form a solid electrolyte coating. The coated diaphragm is dried, heat treated and other processes are performed to ensure that the coating and the diaphragm are tightly combined to obtain a solid electrolyte diaphragm, wherein the thickness of the solid electrolyte coating is 3um and the surface density is 3g / m 2 The thickness of the base film is 7um and the surface density is 2.5g / m 2 .

[0094] The other structures are the same as those in Comparative Example 1, and will not be described in detail in this comparative example.

[0095] Comparative Example 3

[0096] The difference from Comparative Example 1 is that 90 wt% of the solid electrolyte Li 1.5 Al 0.5 Ti 1.5 (PO4)3 and 10wt% of aqueous binder PMMA are mixed to prepare a coating slurry, and the coating slurry is evenly coated on the surface of the base film PE by a coating process to form a solid electrolyte coating. The coated diaphragm is dried, heat treated and other processes are performed to ensure that the coating and the diaphragm are tightly combined to obtain a solid electrolyte diaphragm, wherein the thickness of the solid electrolyte coating is 0.5um and the surface density is 0.5g / m 2 The thickness of the base film is 10um and the surface density is 3.8g / m 2 .

[0097] The other structures are the same as those in Comparative Example 1, and will not be described in detail in this comparative example.

[0098] Test methods and results

[0099] 1. DC resistance DCR test

[0100] A: Test 25℃ DCR ​​(high and low temperature box test)

[0101] 1) 25℃ rest 30min;

[0102] 2) Charge at 8A constant current to 4.2V at 25℃; then charge at 6A constant current constant voltage to 4.50V, CV to 0.02C;

[0103] 3) rest 15 minutes;

[0104] 4) 0.1C DC to 3.4V; this step gets the actual capacity;

[0105] 5) rest 15 minutes;

[0106] 6) Charge at 8A constant current at 25℃ to 4.2V; then charge at 6A constant current and constant voltage to 4.50V, CV to 0.02C; in this step, the current is calculated using the actual capacity;

[0107] 7) rest 15 minutes;

[0108] 8) 0.1C DC 10s (200ms stepping), in this step, the current is calculated using the actual capacity;

[0109] 9) 1C DC 1s (10ms stepping); in this step, the current is calculated using the specified capacity;

[0110] 10) 0.1C DC 60min; in this step, the current is calculated using the actual capacity;

[0111] 11) 1C DC 1s (10ms stepping); in this step, the current is calculated using the specified capacity;

[0112] 12) Repeat steps 10-11 10 times in total; the minimum voltage is set to 2.5V;

[0113] B: After the 25℃ DCR ​​test, continue to test the 10℃ DCR

[0114] Test 10℃ DCR ​​(high and low temperature box test)

[0115] 1) 10℃ rest for 60min;

[0116] 2) 10℃, 1.0C constant current and constant voltage charge to 4.50V, CV to 0.02C;

[0117] 3) rest 15 minutes;

[0118] 4) 0.1C DC to 3.4V; this step gets the actual capacity;

[0119] 5) rest 15 minutes;

[0120] 6) Charge at 10℃ with 1.0C constant current and constant voltage to 4.50V, CV to 0.02C; in this step, the current is calculated using the actual capacity;

[0121] 7) rest 15 minutes;

[0122] 8) 0.1C DC 10s (200ms stepping), in this step, the current is calculated using the actual capacity;

[0123] 9) 1C DC 1s (10ms stepping); in this step, the current is calculated using the specified capacity;

[0124] 10) 0.1C DC 60min; in this step, the current is calculated using the actual capacity;

[0125] 11) 1C DC 1s (10ms stepping); in this step, the current is calculated using the specified capacity;

[0126] 12) Repeat steps 10-11 10 times in total; the minimum voltage is set to 2.5V;

[0127] C: After the 10℃ DCR ​​test, continue to test the 0℃ DCR

[0128] Test 0℃ DCR ​​(high and low temperature box test)

[0129] 1) 0℃ rest for 60min;

[0130] 2) Charge at 0.7C constant current to 4.2V at 0℃; then charge at 0.5C constant current and constant voltage to 4.50V, CV to 0.02C;

[0131] 3) rest for 30 minutes;

[0132] 4) 0.1C DC to 3.4V; this step gets the actual capacity;

[0133] 5) rest for 30 minutes;

[0134] 6) Charge at 0.7C constant current to 4.2V at 0℃; then charge at 0.5C constant current and constant voltage to 4.50V; in this step, the current is calculated using the actual capacity;

[0135] 7) rest for 30 minutes;

[0136] 8) 0.1C DC 10s (200ms stepping), in this step, the current is calculated using the actual capacity;

[0137] 9) 1C DC 1s (10ms stepping); in this step, the current is calculated using the specified capacity;

[0138] 10) 0.1C DC 60min; in this step, the current is calculated using the actual capacity;

[0139] 11) 1C DC 1s (10ms stepping); in this step, the current is calculated using the specified capacity;

[0140] 12) Repeat steps 10-11 10 times in total; the minimum voltage is set to 2.5V;

[0141] Note: For ranges exceeding 5A, the stepping rate cannot reach 10ms

[0142] Judgment criteria: 25℃<50mΩ, 10℃<100mΩ, 0℃<140mΩ;

[0143] Table 2

[0144]

[0145]

[0146] From the comparison of Examples 1 and 2 and Comparative Example 2, it can be seen that when the proportion of the solid electrolyte in the solid electrolyte coating decreases, the DC impedance of the battery increases. This is because the solid state has a higher ionic conductivity, and the impedance increases when the content of the solid electrolyte decreases.

[0147] From the comparison between Examples 1 and 3, it can be seen that when part of the solid electrolyte Li 1.5 Al 0.5 Ti 1.5 (PO4)3 is replaced by solid electrolyte Li7La3Zr2O 12 , Li 0.5 La 0.5 TiO3、Li 1.5 Al 0.5 Ge 1.5 (PO4)3, the battery impedance decreases, this is because these substances have high ionic conductivity, and Li 1.5 Al 0.5 Ti 1.5 Although (PO4)3 is conducive to the formation of a dense thermally stable protective layer, its ionic conductivity is lower than that of the above-mentioned solid electrolyte. The overall conductivity of the diaphragm can be improved by replacing the solid electrolyte components.

[0148] 2. Thermal abuse Hotbox test

[0149] 1) Fully charge the battery: charge to 4.2V at 8A constant current; then charge to 4.50V at 6A constant current constant voltage, CV to 0.02C; record OCV and IMP before the test, check the appearance and take photos;

[0150] 2) Heat the battery cell at a rate of 5°C / min±2°C / min to X°C±2°C and maintain for 60 min, recording the surface temperature rise and voltage of the battery cell; where X is 130, 135, 140, 145, 150, and 155, respectively;

[0151] 3) After the test, record OCV, IMP, check the appearance and take photos;

[0152] 4) Pass criteria: The battery does not catch fire, explode or emit smoke.

[0153] Table 3

[0154]

[0155]

[0156] By comparing Examples 1 and 4 with Comparative Example 3, it can be seen that when the thickness and surface density of the solid electrolyte coating are too small relative to the thickness and surface density of the base film, the boundary safety temperature of the battery thermal runaway decreases. This is because the thickness and surface density of the solid electrolyte coating are small, and the support effect of the thermal stability protective layer generated after the battery is formed is poor. When the stress of the thermal shrinkage deformation of the thick base film is too large, the thermal stability protective layer cannot provide sufficient support and cannot suppress the shrinkage of the base film, and the battery short-circuits after the base film shrinks due to heat.

[0157] By comparing Example 1 and Comparative Example 2, it can be seen that when the solid electrolyte content of the solid electrolyte coating is too low, the boundary safety temperature of the battery thermal runaway is low. This is because the thermal stability protective layer generated after the battery formation due to too little solid electrolyte content is not dense enough, and the thermal stability protective layer will have holes, and cannot provide insulation effect after the base film is destroyed, so the boundary safety temperature of the battery thermal runaway is low.

[0158] 3. Cycle test

[0159] 1) 23℃ cycle

[0160] (1) Test the initial voltage, internal resistance and thickness of the battery cell at 23±2℃;

[0161] (2) At 23±2℃, charge at 8A constant current to 4.2V; then charge at 6A constant current constant voltage to 4.50V, CV to 0.02C, and record the cell voltage, internal resistance, and thickness;

[0162] (3) At 23±2℃, place for 2h; discharge at 0.2C constant current to 3.0V, place for 10min, charge at 8A constant current to 4.2V; then charge at 6A constant current constant voltage to 4.50V, CV to 0.02C, place for 10min; (4) At 23±2℃, discharge at 0.2C constant current to 3.0V, as 0.2C discharge capacity D0, place for 10min; (5) At 23±2℃, charge at 8A constant current to 4.2V; then charge at 6A constant current constant voltage to 4.50V, CV to 0.02C, place for 10min;

[0163] (6) At 23±2℃, discharge at 0.7C constant current to 3.0V, which is taken as 0.7C discharge capacity D1', and leave for 10min;

[0164] (7) Repeat steps 5 to 6; after 49 cycles at 0.7C, charge to 4.2V at 8A constant current; then charge to 4.50V at 6A constant current and constant voltage, CV to 0.02C, and record the voltage, internal resistance, and thickness of the fully charged cell;

[0165] (8) At 23±2°C, discharge at 0.2C to 3.0V, which is the discharge capacity D50 of the 50th 0.2C cycle; (9) Repeat this process for a total of 1000 cycles;

[0166] (10) For the first 500 times of the test, the cell's full-charge voltage, internal resistance, and thickness are tested every 50 times. From 500 to 1000 times, the cells are tested every 100 times. Full-charge EIS is tested at the 100th / 300th / 500th / 800th / 1000th times.

[0167] 2) 45℃ cycle

[0168] (1) Test the initial voltage, internal resistance and thickness of the battery cell at 45±2℃;

[0169] (2) At 45±2℃, charge at 8A constant current to 4.2V; then charge at 6A constant current constant voltage to 4.50V, CV to 0.02C, and record the cell voltage, internal resistance, and thickness;

[0170] (3) At 45±2℃, discharge at 0.2C constant current to 3.0V, which is taken as 0.2C discharge capacity D0, and leave for 10min;

[0171] (4) 45±2℃, 8A cc to 4.2V, 1C cc to 4.3V, 0.8C to 4.48V, 0.6C to4.53VFFC cv to 0.164C, leave for 10 min;

[0172] (5) At 45±2℃, discharge at 0.7C constant current to 3.0V, which is the 0.7C discharge capacity D1', and leave it for 10min;

[0173] (6) Repeat steps 4 to 5; after 49 cycles at 0.7C, fully charge the battery using standard charging conditions (cut-off current 0.05C); record the voltage, internal resistance, and thickness of the fully charged cell;

[0174] (7) At 45±2℃, discharge at 0.2C to 3.0V, which is the discharge capacity D50 of the 50th 0.2C cycle; (8) Repeat this process for a total of 1000 cycles

[0175] (9) For the first 300 times of the test, the cell's full-charge voltage, internal resistance, and thickness are tested every 50 times. From 300 to 1000 times, the cells are tested every 100 times. Full-charge EIS is tested at the 100th / 300th / 500th / 800th / 1000th times.

[0176] Table 4

[0177]

[0178] According to the comparison between Examples 1-4 and Comparative Examples 1-3, it can be seen that when the DC impedance of the battery decreases, the battery has a better cycle capacity retention rate.

[0179] The above description shows and describes several preferred embodiments of the present invention, but as before, it should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the invention concept of this article through the above teachings or the technology or knowledge of the relevant field. And the changes and modifications made by those skilled in the art do not depart from the spirit and scope of the present invention, and should be within the scope of protection of the claims attached to the present invention.

Claims

1. A solid electrolyte membrane, characterized in that: It comprises a base film (1) and a solid electrolyte coating (2) coated on at least one surface of the base film (1); The solid electrolyte coating (2) comprises a solid electrolyte, and the solid electrolyte accounts for 80% to 95% by mass of the solid electrolyte coating (2); The solid electrolyte is LATP, or a mixture of LATP and at least one of LLZO, LLTO and LAGP.

2. The solid electrolyte membrane according to claim 1, characterized in that: The thickness H1 of the solid electrolyte coating (2) and the thickness H2 of the base film (1) satisfy the relationship: H1 / H2≥10%; the surface density w1 of the solid electrolyte coating (2) and the surface density w2 of the base film (1) satisfy the relationship: w1 / w2≥50%.

3. The solid electrolyte membrane according to claim 2, characterized in that: The solid electrolyte coating (2) has a thickness of 0.5 to 5 μm and a surface density of 2 to 4 g / m 2 The base film (1) has a thickness of 4 to 10 μm and a surface density of 1.8 to 3.8 g / m 2 .

4. The solid electrolyte membrane according to claim 1, characterized in that: The structural formula of the LATP is Li 1+ x Al x Ti 2-x (PO4)3, where x ranges from 0 to 0.

5.

5. The solid electrolyte membrane according to claim 4, characterized in that: The LATP is Li 1.5 Al 0.5 Ti 1.5 (PO4)3、Li 1.4 Al 0.4 Ti 1.6 (PO4)3 or Li 1.3 Al 0.3 Ti 1.7 (PO4)3, the LLZO is Li7La3Zr2O 12 , the LLTO is Li 0.5 La 0.5 TiO3 or Li 0.33 La 0.557 TiO3, the LAGP is Li 1.5 Al 0.5 Ge 1.5 (PO4)3.

6. The solid electrolyte membrane according to claim 1, characterized in that: The base film (1) is made of polyolefin or modified polyolefin material.

7. The solid electrolyte membrane according to claim 1, characterized in that: The base film (1) has a porosity of 20% to 40%, an air permeability of 180 to 300 sec / 100 cc, a needle puncture strength greater than or equal to 200 gf, and a longitudinal tensile strength greater than or equal to 2000 kgf / cm 2 , transverse tensile strength greater than or equal to 1800kgf / cm 2 , the longitudinal elongation is greater than or equal to 30%, the transverse elongation is greater than or equal to 30%, and the melting point is greater than or equal to 135°C.

8. The solid electrolyte membrane according to claim 1, characterized in that: The solid electrolyte coating (2) further comprises a water-based binder or an oil-based binder with a mass fraction of 5% to 20%, wherein the water-based binder is one or more of PMMA, PAA, SBR, and CMC, and the oil-based binder is PVDF.

9. The solid electrolyte membrane according to claim 1, characterized in that: The solid electrolyte membrane includes a first state and a second state, wherein the first state is the state of the solid electrolyte membrane before formation, and the second state is the state of the solid electrolyte membrane after formation. In the second state, a dense thermal stability protective layer (3) is formed on the surface of the solid electrolyte membrane.

10. A battery formation method for improving the thermal stability of the solid electrolyte membrane according to any one of claims 1 to 9, characterized in that: The following steps are involved: Step 1: Under a preset heating temperature and pressure, a voltage in the range of 4.0 to 5.0 V is applied to the electrodes of the battery to be formed, and the battery is charged at a first charging rate for a first preset time; Step 2: Under a preset heating temperature and pressure, a voltage in the range of 4.0 to 5.0 V is applied to the electrodes of the battery to be formed, and the battery is charged at a second charging rate for a second preset time; Step 3: Under a preset heating temperature and pressure, a voltage in the range of 4.0 to 5.0 V is applied to the electrodes of the battery to be formed, and the battery is charged at a third charging rate for a third preset time; Wherein, the battery is preset to be left for a predetermined time between adjacent steps, the second charging rate is greater than the first charging rate, and the third charging rate is greater than the second charging rate.

Citation Information

Patent Citations

  • High-voltage polymer lithium ion battery high-temperature formation process

    CN109616709A

  • Ionic-electronic conductor composite film and preparation method thereof and lithium battery

    CN109638202A

  • High temperature type high voltage lithium ion battery and manufacturing method thereof

    CN110474085A

Cited By

  • Diaphragm and preparation method and application thereof

    CN121394773A

  • An llto-based solid-state electrolyte separator and a method of preparing the same

    CN122931240A