Sulfur-chlorine-based solid electrolyte as well as preparation method and application thereof
Synthesis of thiochlorine-based solid electrolytes through high-energy ball milling method solves the problem of low conductivity of zirconium halide electrolytes, improves the cycle life and performance of all-solid-state batteries, and achieves efficient conductivity and low-cost production.
Patent Information
- Application Number
- CN202411067438.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-12
AI Technical Summary
The conductivity of zirconium-based halide solid electrolyte is low, resulting in slow lithium ion transmission speed, which in turn aggravates the internal resistance and performance decay of all-solid-state batteries, limiting the battery's service life and application potential.
The high-energy ball milling method is used to mix sulfide and metal halide to synthesize a thiochlorine-based solid electrolyte, which improves its room temperature ionic conductivity and is used in all-solid-state batteries.
It significantly improves the cycle life of all solid-state batteries, provides high-performance batteries development support, and reduces production costs.
Smart Images

Figure CN118943474A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries and relates to a sulfur-chlorine-based solid electrolyte and a preparation method and application thereof. Background Art
[0002] As the core component of all-solid-state batteries, solid electrolytes play a vital role in promoting the development of next-generation energy storage technologies. Among the many solid electrolyte materials, zirconium-based halide solid electrolytes have attracted much attention due to their unique physical and chemical properties. These materials have a wide electrochemical window, which means that they can remain stable over a wide voltage range, which is crucial for improving the energy density of all-solid-state batteries. In addition, zirconium-based halides can promote the formation of a good solid-solid contact interface between the electrode and the electrolyte, thereby ensuring efficient electron and ion transfer, which is the key to achieving high-performance all-solid-state batteries.
[0003] Zirconium-based halides also exhibit the advantages of being easy to prepare, with simple synthetic routes and significant cost-effectiveness, which makes large-scale production possible. These advantages not only help to reduce manufacturing costs, but also accelerate the commercialization of such batteries. However, despite the excellent performance of zirconium-based halide solid electrolytes in many aspects, their conductivity is usually low (less than 10 - 4 S / cm), which means that the transfer speed of lithium ions inside it is relatively slow. This low conductivity will cause the internal resistance of the battery to gradually increase during the cycle, which in turn accelerates the degradation rate of battery performance and limits the battery's service life and practical application potential. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a sulfur-chloride-based solid electrolyte and a preparation method and application thereof. The sulfur-chloride-based solid electrolyte is synthesized by mixing sulfide and metal halide by a high-energy ball milling method. The obtained sulfur-chloride-based solid electrolyte has high ionic conductivity and can be applied to all-solid-state batteries to improve their cycle life.
[0005] One object of the present invention is achieved by the following technical solutions:
[0006] A sulfur-chlorine-based solid electrolyte, the chemical formula of which is shown in Formula I:
[0007] Li x ZGar y Cl z Formula I,
[0008] Among them, 1≤x≤4, 0.5≤y≤2, 4≤z≤6.
[0009] Preferably, in the X-ray diffraction spectrum of the sulfur-chlorine-based solid electrolyte, an amorphous phase or a composite phase of a crystalline phase and an amorphous phase is presented, wherein the crystalline phase is lithium sulfide and / or lithium chloride.
[0010] Preferably, the raw materials for preparing the sulfur-chlorine-based solid electrolyte are lithium sulfide and zirconium chloride, or lithium chloride and zirconium sulfide.
[0011] Preferably, the room temperature ionic conductivity of the sulfur-chlorine-based solid electrolyte is 1×10 -4 ~3×10 -3 S / cm. More preferably, the room temperature ionic conductivity of the sulfur-chloride-based solid electrolyte is 6×10 -4 ~3×10 -3 S / cm, for example, can be 6×10 -4 ,7×10 -4 , 8×10 -4 ,9×10 -4 , 1×10 -3 , 1.5×10 -3 , 2×10 -3 , 2.5×10 -3 or 3×10 -3 The room temperature here is 10~40℃.
[0012] Another object of the present invention is achieved by the following technical solutions:
[0013] The method for preparing the above-mentioned sulfur-chlorine-based solid electrolyte comprises step 1 or step 2:
[0014] Step 1: according to the stoichiometric ratio of elements in the sulfur-chlorine-based solid electrolyte, raw materials including Li, Zr, S, and Cl are weighed, mixed, and ball-milled to obtain a sulfur-chlorine-based solid electrolyte;
[0015] Step 2: According to the stoichiometric ratio of elements in the sulfur-chlorine-based solid electrolyte, raw materials including Li, Zr, S, and Cl are weighed and uniformly mixed, and then ground after heat treatment to obtain a sulfur-chlorine-based solid electrolyte.
[0016] Preferably, the raw material containing Li, Zr, S and Cl is lithium sulfide and zirconium chloride, or lithium chloride and zirconium sulfide.
[0017] Preferably, the ball milling conditions of step 1 include: a ball-to-material ratio of 1 to 60:1, a rotation speed of 400 to 1000 rpm, and a time of 10 to 50 hours.
[0018] Preferably, the uniform mixing method in step 2 includes one or more of mechanical stirring, ball milling, roller milling, and grinding, and the mixing time is 0.1 to 24 hours.
[0019] Preferably, the heat treatment conditions in step 2 include: under vacuum or inert atmosphere, the heat treatment temperature is 80 to 250° C., more preferably 120 to 200° C., and the heat treatment time is 1 to 10 hours, more preferably 1 to 6 hours.
[0020] Preferably, the sulfur-chlorine-based solid electrolyte cannot come into contact with water and / or oxygen during the preparation process.
[0021] The third object of the present invention is achieved by the following technical solutions:
[0022] A composite positive electrode material comprises the sulfur-chlorine-based solid electrolyte, a positive electrode active material and a conductive agent.
[0023] Preferably, the mass ratio of the sulfur-chloride-based solid electrolyte, the positive electrode active material and the conductive agent is 90-70:10-30:1-6.
[0024] Preferably, the positive electrode active material is LiFePO4, LiCoO2, LiNiO2, LiMn2O4, LiNi 0.8 Co 0.1 Mn 0.1 O2 and LiNi 0.6 Co 0.2 Mn 0.2 One or more of O2.
[0025] Preferably, the conductive agent is one or more of Super-P, superconducting carbon black, acetylene black and Ketjen black.
[0026] The fourth object of the present invention is achieved by the following technical solutions:
[0027] An all-solid-state lithium secondary battery comprises a positive electrode, a negative electrode and an electrolyte, wherein the electrolyte comprises the above-mentioned sulfur-chlorine-based solid electrolyte.
[0028] Preferably, the electrolyte includes the above-mentioned sulfur-chloride-based solid electrolyte and sulfide solid electrolyte.
[0029] Preferably, the positive electrode comprises the composite positive electrode material
[0030] Preferably, the negative electrode is any one of Li, Li-In alloy and Si.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] 1. The sulfur-chlorine-based solid electrolyte provided by the present invention presents an amorphous phase or a composite phase of a crystalline phase (the crystalline phase is the raw material phase)-amorphous phase, has a high room temperature ionic conductivity, and shows good electrical conductivity performance.
[0033] 2. The present invention uses a simple high-energy ball milling method to mix sulfide and metal chloride to synthesize sulfur-chloride-based solid electrolyte. The preparation method is very simple and practical, and also reduces production costs.
[0034] 3. The sulfur-chlorine-based solid electrolyte of the present invention is applied to all-solid-state batteries, which can effectively improve the cycle life of the batteries and provide strong support for the development of high-performance all-solid-state batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 X-ray diffraction patterns of the sulfur-chlorine-based solid electrolytes prepared in Example 1, Example 2, Example 4 and Example 5;
[0036] Figure 2 is the room temperature AC impedance diagram of the Li2ZrSCl4 electrolyte of Example 1;
[0037] Figure 3 is Li of Example 2 1.6 ZGar 0.8 Room temperature AC impedance diagram of Cl4 electrolyte;
[0038] Figure 4 This is the LCO / Li2ZrSCl4-Li6PS5Cl / Li-In battery cycle diagram of Example 1;
[0039] Figure 5 This is a charge and discharge curve diagram of the LCO / Li2ZrSCl4-Li6PS5Cl / Li-In battery of Example 1;
[0040] Figure 6 is the LCO / Li of Example 2 1.6 ZGar 0.8 Cl4-Li6PS5Cl / Li-In battery cycle diagram;
[0041] Figure 7 is the X-ray diffraction pattern of the Li2ZrCl6 solid electrolyte of Comparative Example 1;
[0042] Figure 8 The room temperature AC impedance diagram of the Li2ZrCl6 solid electrolyte of Comparative Example 1;
[0043] Fig. 9 Li2ZrS x Cl 6-2x X-ray diffraction pattern of solid electrolyte;
[0044] Fig.10 Li2ZrS 0.05 Cl 5.9 Room temperature AC impedance diagram of the solid electrolyte. DETAILED DESCRIPTION
[0045] The technical scheme of the present invention is further described below by specific examples and accompanying drawings. It should be understood that the specific examples described herein are only used to help understand the present invention and are not intended for specific limitations of the present invention. The accompanying drawings used herein are only for better illustrating the disclosure of the present invention and do not have a limiting effect on the scope of protection. If not otherwise specified, the raw materials used in the embodiments of the present invention are all commonly used raw materials in the art, and the methods used in the embodiments are all conventional methods in the art.
[0046] Example 1
[0047] Li2S and ZrCl4 were weighed in molar ratio and poured into an agate ball mill jar, and ZrO2 balls were added. The ball-to-material ratio was 50:1, the ball mill speed was 500 rpm, and the ball milling time was 24 h to obtain a sulfur-chloride-based solid electrolyte with a chemical formula of Li2ZrSCl4. Its ionic conductivity at room temperature (30°C) was 1.41 mS / cm.
[0048] The X-ray diffraction pattern of Li2ZrSCl4 electrolyte is shown in Figure 1 , presenting a composite phase dominated by an amorphous phase and a small amount of a crystalline phase, the crystalline phase being the raw material Li2S phase and the LiCl phase obtained by ball milling.
[0049] The room temperature AC test impedance diagram of Li2ZrSCl4 electrolyte is shown in Figure 2 .
[0050] The all-solid-state principle battery was assembled with Li-In alloy as the negative electrode, LiCoO2 (LCO) as the positive electrode material, and sulfide solid electrolytes Li6PS5Cl and Li2ZrSCl4 as electrolytes for battery charge and discharge tests. The battery was activated at 0.1C, and the first cycle coulomb efficiency was 96.4%. Figure 5 shown. Figure 4 This is the battery cycle diagram of Li-In / Li6PS5Cl-Li2ZrSCl4 / LCO. After activation, a 0.3C long cycle test was performed. After 50 cycles, there was still 119.1mAh g -1 The specific capacity and capacity retention rate are 93.4%.
[0051] The above processes were all carried out in a water-free (<0.1 ppm) and oxygen-free (<0.1 ppm) glove box.
[0052] Example 2
[0053] Li2S and ZrCl4 were weighed in molar ratio and poured into an agate ball mill, and ZrO2 balls were added. The ball-to-material ratio was 50:1, the ball mill speed was 500 rpm, and the ball milling time was 24 h to obtain a chemical formula of Li 1.6 ZGar0.8 The ionic conductivity of the Cl4-sulfur-chlorine-based solid electrolyte is 1.39 mS / cm at room temperature (30°C).
[0054] Li 1.6 ZGar 0.8 The X-ray diffraction pattern of Cl4 electrolyte is shown in Figure 1 , presenting a composite phase dominated by an amorphous phase and a small amount of a crystalline phase, the crystalline phase being the raw material Li2S and the LiCl phase obtained by ball milling.
[0055] Li 1.6 ZGar 0.8 The room temperature AC test impedance diagram of Cl4 electrolyte is shown in Figure 3 .
[0056] An all-solid-state principle battery was assembled with Li-In alloy as the negative electrode, LiCoO2 (LCO) as the positive electrode material, and sulfide solid electrolytes Li6PS5Cl and Li2ZrSCl4 as electrolytes for battery charge and discharge tests. Figure 6 Li-In / Li6PS5Cl-Li 1.6 ZGar 0.8 Battery cycle diagram of Cl4 / LCO. The battery was tested at 0.1C. After 50 cycles, the capacity retention rate was 82%.
[0057] The above processes were all carried out in a water-free (<0.1 ppm) and oxygen-free (<0.1 ppm) glove box.
[0058] Example 3
[0059] LiCl and ZrS2 were weighed in molar ratio and poured into an agate ball mill jar, and ZrO2 balls were added. The ball-to-material ratio was 50:1, the ball mill speed was 500 rpm, and the ball milling time was 24 h to obtain a sulfur-chloride-based solid electrolyte with a chemical formula of Li2ZrS2Cl2. Its ionic conductivity at room temperature (30°C) was 0.8 mS / cm.
[0060] The X-ray diffraction spectrum of the sulfur-chlorine-based solid electrolyte shows a composite phase mainly composed of an amorphous phase and a small amount of a crystalline phase, and the crystalline phase is the raw material LiCl phase.
[0061] Example 4
[0062] Li2S and ZrCl4 were weighed in molar ratio and poured into an agate ball mill, and ZrO2 balls were added. The ball-to-material ratio was 50:1, the ball mill speed was 500 rpm, and the ball milling time was 24 h to obtain a chemical formula of Li 1.2 ZGar 0.6 The ionic conductivity of the Cl4-sulfur-chlorine-based solid electrolyte is 0.86 mS / cm at room temperature (30°C).
[0063] Li1.2 ZGar 0.6 The X-ray diffraction pattern of Cl4 electrolyte is shown in Figure 1 , presenting a composite phase dominated by an amorphous phase and a small amount of a crystalline phase, the crystalline phase being the raw material Li2S and the LiCl phase obtained by ball milling.
[0064] Example 5
[0065] Li2S and ZrCl4 were weighed in molar ratio and poured into an agate ball mill, and ZrO2 balls were added. The ball-to-material ratio was 50:1, the ball mill speed was 500 rpm, and the ball milling time was 24 h to obtain a chemical formula of Li 2.4 ZGar 1.2 The ionic conductivity of the Cl4-sulfur-chlorine-based solid electrolyte is 0.75 mS / cm at room temperature (30°C).
[0066] Li 2.4 ZGar 1.2 The X-ray diffraction pattern of Cl4 electrolyte is shown in Figure 1 , presenting a composite phase dominated by an amorphous phase and a small amount of a crystalline phase, the crystalline phase being the raw material Li2S and the LiCl phase obtained by ball milling.
[0067] Example 6
[0068] Li2S and ZrCl4 were weighed in molar ratio and poured into an agate ball mill, and ZrO2 balls were added. The ball-to-material ratio was 50:1, the ball mill speed was 500 rpm, and the ball milling time was 24 h to obtain a chemical formula of Li 0.4 ZGar 0.2 The ionic conductivity of the Cl4-sulfur-chlorine-based solid electrolyte is 0.7 mS / cm at room temperature (30°C).
[0069] Li 0.4 ZGar 0.2 The X-ray diffraction pattern of the Cl4 electrolyte shows a composite phase dominated by an amorphous phase and a small amount of a crystalline phase, and the crystalline phase is the raw material Li2S and the LiCl phase obtained by ball milling.
[0070] Example 7
[0071] Li2S and ZrCl4 were weighed in molar ratio and poured into a wall breaking machine for stirring at a speed of 7000 rpm for 15 seconds. Then, the mixture was poured into a quartz tube, vacuum-sealed, and heated in a muffle furnace at 200°C for 5 hours. After grinding, a product with the chemical formula of Li 2.4 ZGar 1.2 The ionic conductivity of the Cl4-sulfur-chlorine-based solid electrolyte is 0.75 mS / cm at room temperature (30°C).
[0072] Li 2.4 ZGar 1.2The X-ray diffraction pattern of the Cl4 electrolyte shows a composite phase dominated by an amorphous phase and a small amount of a crystalline phase, and the crystalline phase is the raw material Li2S phase.
[0073] Comparative Example 1
[0074] LiCl and ZrCl4 were weighed in molar ratio and poured into an agate ball mill, and ZrO2 balls were added. The ball-to-material ratio was 50:1, the ball mill speed was 500 rpm, and the ball milling time was 24 h. The above process was carried out in a glove box without water (<0.1 ppm) and oxygen (<0.1 ppm). A solid electrolyte with the chemical formula of Li2ZrCl6 was obtained, and its ionic conductivity at room temperature (30 ° C) was 0.3 mS / cm. The AC impedance spectrum is shown in the figure. Figure 8 shown.
[0075] The X-ray diffraction pattern of Li2ZrCl6 electrolyte is shown in Figure 7 , Li2ZrCl6 material has the same physical phase as monoclinic Li3YCl6.
[0076] Comparative Example 2
[0077] LiCl, ZrCl4 and Li2S were weighed in molar ratio and poured into an agate ball mill, and ZrO2 balls were added. The ball-to-material ratio was 50:1, the ball mill speed was 500 rpm, and the ball milling time was 24 h. The above process was carried out in a glove box without water (<0.1 ppm) and oxygen (<0.1 ppm), and the chemical formula of Li2ZrS was obtained. 0.05 Cl 5.9 The solid electrolyte has an ionic conductivity of 0.58 mS / cm at room temperature (30°C). The AC impedance spectrum is shown in Fig.10 shown.
[0078] Li2Zr 0.05 Cl 5.9 The X-ray diffraction pattern of the electrolyte is shown in Fig. 9 , Li2ZrS doped with S x Cl 6-2x The solid electrolyte still retains the characteristic peaks of Li2ZrCl6.
[0079] Comparative Example 3
[0080] LiCl, ZrCl4 and Li2S were weighed in molar ratio and poured into an agate ball mill, and ZrO2 balls were added. The ball-to-material ratio was 50:1, the ball mill speed was 500 rpm, and the ball milling time was 24 h. The above process was carried out in a glove box without water (<0.1 ppm) and oxygen (<0.1 ppm), and the chemical formula of Li2ZrS was obtained. 0.1 Cl 5.8 The solid electrolyte has an ionic conductivity of 0.28mS / cm at room temperature (30°C).
[0081] Li2Zr 0.1 Cl 5.9 The X-ray diffraction pattern of the electrolyte is shown in Fig. 9 , Li2ZrS doped with S x Cl 6-2x The solid electrolyte still retains the characteristic peaks of Li2ZrCl6.
[0082] Comparative Example 4
[0083] LiCl, ZrCl4 and Li2S were weighed in molar ratio and poured into an agate ball mill, and ZrO2 balls were added. The ball-to-material ratio was 50:1, the ball mill speed was 500 rpm, and the ball milling time was 24 h. The above process was carried out in a glove box without water (<0.1 ppm) and oxygen (<0.1 ppm), and the chemical formula of Li2ZrS was obtained. 0.2 Cl 5.6 The solid electrolyte has an ionic conductivity of 0.56 mS / cm at room temperature (30°C).
[0084] Li2Zr 0.2 Cl 5.6 The X-ray diffraction pattern of the electrolyte is shown in Fig. 9 , Li2ZrS doped with S x Cl 6-2x The solid electrolyte still retains the characteristic peaks of Li2ZrCl6.
[0085] The various aspects, embodiments, and features of the present invention should be considered to be illustrative in all aspects and not limiting of the present invention, the scope of which is defined solely by the claims. Other embodiments, modifications, and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.
[0086] In the preparation method of the present invention, the order of each step is not limited to the order listed. For those skilled in the art, without creative work, the order of each step is also within the protection scope of the present invention. In addition, two or more steps or actions can be performed simultaneously.
[0087] Finally, it should be noted that the specific embodiments described herein are merely examples of the present invention, and are not intended to limit the implementation methods of the present invention. A person skilled in the art of the present invention may make various modifications or supplements to the specific embodiments described, or replace them in a similar manner. It is not necessary and impossible to provide all examples of all implementation methods here. However, these obvious changes or modifications derived from the essential spirit of the present invention still fall within the scope of protection of the present invention, and interpreting them as any additional limitation is contrary to the spirit of the present invention.
Claims
1. A sulfur-chlorine-based solid electrolyte, characterized in that: Its chemical formula is shown in Formula I: Li x ZrS y Cl z Formula I Among them, 1≤x≤4, 0.5≤y≤2, 4≤z≤6.
2. A sulfur-chlorine-based solid electrolyte according to claim 1, characterized in that: In the X-ray diffraction spectrum of the sulfur-chlorine-based solid electrolyte, an amorphous phase or a composite phase of a crystalline phase and an amorphous phase is presented, wherein the crystalline phase is lithium sulfide and / or lithium chloride.
3. A sulfur-chlorine-based solid electrolyte according to claim 1, characterized in that: The raw materials for preparing the sulfur-chlorine-based solid electrolyte are lithium sulfide and zirconium chloride, or lithium chloride and zirconium sulfide.
4. A sulfur-chlorine-based solid electrolyte according to claim 1, characterized in that: The room temperature ionic conductivity of the sulfur-chloride-based solid electrolyte is 1×10 -4 ~3×10 -3 S / cm.
5. The method for preparing the sulfur-chlorine-based solid electrolyte according to claim 1, characterized in that: Includes step 1 or step 2: Step 1: according to the stoichiometric ratio of elements in the sulfur-chlorine-based solid electrolyte, raw materials including Li, Zr, S, and Cl are weighed, mixed, and ball-milled to obtain a sulfur-chlorine-based solid electrolyte; Step 2: According to the stoichiometric ratio of elements in the sulfur-chlorine-based solid electrolyte, raw materials including Li, Zr, S, and Cl are weighed and uniformly mixed, and then ground after heat treatment to obtain a sulfur-chlorine-based solid electrolyte.
6. The preparation method according to claim 5, characterized in that: The raw material containing Li, Zr, S and Cl is lithium sulfide and zirconium chloride, or lithium chloride and zirconium sulfide; And / or, the ball milling conditions of step 1 include: a ball-to-material ratio of 1 to 60:1, a rotation speed of 400 to 1000 rpm, and a time of 10 to 50 hours.
7. The preparation method according to claim 5, characterized in that: The uniform mixing method in step 2 includes one or more of mechanical stirring, ball milling, roller milling, and grinding, and the mixing time is 0.1 to 24 hours; And / or, the heat treatment conditions in step 2 include: under vacuum or inert atmosphere, the heat treatment temperature is 80 to 250° C., and the heat treatment time is 1 to 10 hours.
8. A composite positive electrode material, characterized in that: The invention comprises the sulfur-chlorine-based solid electrolyte as claimed in claim 1, a positive electrode active material and a conductive agent.
9. An all-solid-state lithium secondary battery, characterized in that: The invention comprises a positive electrode, a negative electrode and an electrolyte, wherein the electrolyte comprises the sulfur-chlorine-based solid electrolyte as claimed in claim 1.
10. The all-solid-state lithium secondary battery according to claim 9, characterized in that: The positive electrode comprises the composite positive electrode material as claimed in claim 8; And / or, the negative electrode is any one of Li, Li-In alloy and Si.
Citation Information
Cited By
Sulfide-based solid electrolyte and all-solid-state battery including the same
EP4826823A1