Polyolefin microporous support gel polymer electrolyte with bicontinuous structure as well as preparation method and application of polyolefin microporous support gel polymer electrolyte
Through the dual continuous structure of polyolefin microporous support of gel polymer electrolyte, combined with the polymer electrolyte membrane interface layer and the polyolefin porous membrane support layer, the shortcomings of electrolyte conductivity and mechanical properties in lithium-ion batteries are solved, and high-efficiency lithium is achieved Ion migration and cell stability are improved.
Patent Information
- Application Number
- CN202411091244.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional lithium-ion batteries use organic liquid electrolytes and are flammable, and the solid polymer electrolyte has low room temperature conductivity and large electrode/electrolyte interface impedance, which limits their application, especially in terms of the flexibility and safety of high-power lithium-ion batteries. .
The double continuous structure polyolefin microporous support gel polymer electrolyte is prepared by immersion precipitation phase separation method, combining the polymer electrolyte membrane interface layer and the polyolefin porous membrane support layer to improve the conductivity and mechanical properties of the electrolyte and improve the electrode and Interface compatibility of electrolytes.
It achieves high ionic conductivity, excellent mechanical properties and electrochemical stability, effectively inhibit the growth of lithium dendrites, improves the life and safety of lithium batteries, and has a comprehensive performance that is better than commercial liquid electrolytes.
Smart Images

Figure CN118943478A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion battery polymer electrolytes, and in particular to a bicontinuous structure polyolefin microporous supported gel polymer electrolyte and a preparation method and application thereof. Background Art
[0002] The statements in this section merely provide background information related to the present disclosure and may not constitute prior art.
[0003] Lithium-ion batteries have the advantages of high energy density, long cycle life, safety and no leakage, low pollution and compliance with environmental protection requirements, which have aroused great interest and widespread attention from scientific researchers. However, traditional lithium-ion batteries usually use organic liquid electrolytes, and organic solvents have a series of disadvantages such as flammability. In addition, the uneven deposition of lithium ions is prone to produce lithium dendrites, which may pierce the diaphragm during long-term charge / discharge cycles, eventually causing internal short circuits in the battery.
[0004] In order to solve these problems, researchers have proposed solid polymer electrolytes to replace traditional liquid electrolytes. However, these solid polymer electrolytes have disadvantages such as low room temperature conductivity and large electrode / electrolyte interface impedance, which seriously limit the practical application of solid polymer electrolytes.
[0005] Compared with solid polymer electrolytes, gel polymer electrolytes (GPEs) have better electrode / electrolyte interface stability, higher ionic conductivity, and lower interfacial impedance at room temperature, and are therefore considered to be a very promising candidate electrolyte. GPE is a polymer electrolyte system with a certain network structure formed by a polymer matrix, a plasticizer, and an electrolyte salt by a certain method, which binds the liquid electrolyte in the polymer network structure to achieve the transmission of lithium ions. However, when the polymer matrix swells in the plasticizer, the mechanical strength of the GPE is reduced, far exceeding the range that the existing GPE can withstand, and cannot meet the flexibility, safety, and design requirements of high-power lithium-ion batteries. Therefore, it is still a huge challenge to design and prepare a GPE with high ionic conductivity, excellent mechanical properties, and the ability to inhibit the growth of lithium dendrites. Summary of the invention
[0006] The purpose of the present invention is to provide a bicontinuous structure polyolefin microporous supported gel polymer electrolyte and its preparation method and application in view of the problems existing in the prior art. The gel polymer electrolyte has excellent electrochemical and mechanical properties. The constructed bicontinuous structure can effectively improve the contact interface with the electrode, improve the life and safety of the lithium battery, thereby solving the above-mentioned problems.
[0007] The technical solution of the present invention is as follows:
[0008] A bicontinuous structure polyolefin microporous supported gel polymer electrolyte, comprising: 10-40wt% polymer electrolyte skeleton, 60-90wt% organic electrolyte;
[0009] The polymer electrolyte skeleton comprises: a support layer and a bicontinuous polymer electrolyte membrane interface layer; the organic electrolyte comprises: an organic solvent and a lithium salt.
[0010] Furthermore, the support layer is a polyethylene PE membrane, a polypropylene PP membrane, a polyimide PI membrane or a non-woven fabric membrane;
[0011] The bicontinuous polymer electrolyte membrane is prepared by an immersion precipitation phase separation method; wherein the polymer matrix is selected from a combination of two or more of polyvinylidene fluoride PVDF, polyvinylidene fluoride-hexafluoropropylene PVDF-HFP, polymethyl methacrylate PMMA, and polyethylene oxide PEO; the solvent is selected from a polar solvent, including one or more of N-methylpyrrolidone NMP, N,N-dimethylformamide DMF, tetrahydrofuran THF, dimethyl sulfoxide DMSO, and 1,4-epoxyhexacyclopentane; the non-solvent is selected from one or a combination of deionized water and anhydrous ethanol; the additive is selected from one of polyvinylpyrrolidone PVP, polyethylene oxide PEO, and polyethylene glycol PEG;
[0012] The organic solvent is selected from one or more combinations of ethylene carbonate EC, propylene carbonate PC, dimethyl carbonate DMC, diethyl carbonate DEC, ethyl methyl carbonate EMC, N,N-dimethylformamide DMF, 1,2-dimethoxyethane DME;
[0013] The lithium salt is selected from one of lithium hexafluorophosphate LiPF6, lithium perchlorate LiClO4, lithium tetrafluoroborate LiBF4, lithium hexafluoroarsenate LiAsF6, lithium trifluoromethanesulfonate LiOTf, lithium bis(trifluoromethanesulfonyl)imide LiTFSI, lithium dioxalatoborate LiBOB, lithium bis(fluorosulfonyl)imide LiFSI and lithium oxalatodifluoroborate LiDFOB.
[0014] A method for preparing a bicontinuous structure polyolefin microporous supported gel polymer electrolyte comprises the following steps:
[0015] Step S1: preparing a bicontinuous polymer electrolyte membrane casting solution;
[0016] Step S2: Based on the casting solution prepared in step S1, a bicontinuous polymer electrolyte membrane is prepared by an immersion precipitation phase separation method;
[0017] Step S3: After vacuum drying the bicontinuous structure polymer electrolyte membrane obtained in step S2, immerse it in an electrolyte solution in a glove box for adsorption and gelation, and finally obtain a bicontinuous structure polyolefin microporous membrane-supported gel polymer electrolyte.
[0018] Furthermore, the step S1 comprises:
[0019] Step S11: dissolving the polymer matrix in a polar solvent according to a certain proportion to form a polymer solution;
[0020] Step S12: After adding additives and non-solvents into the polymer solution, sealing is performed;
[0021] Step S13: performing ultrasonic oscillation;
[0022] Step S14: placing the mixture in a water bath with magnetic stirring, and letting it stand to remove bubbles to obtain a casting solution.
[0023] Furthermore, the step S11 includes:
[0024] The polymer matrix is a combination of two or more of polyvinylidene fluoride PVDF, polyvinylidene fluoride-hexafluoropropylene PVDF-HFP, polymethyl methacrylate PMMA, and polyethylene oxide PEO;
[0025] The polar solvent is selected from one or more combinations of N-methylpyrrolidone NMP, N,N-dimethylformamide DMF, tetrahydrofuran THF, dimethyl sulfoxide DMSO, and 1,4-epoxyhexacyclic ring;
[0026] The step S12 comprises:
[0027] The additive is selected from one of polyvinyl pyrrolidone PVP, polyethylene oxide PEO and polyethylene glycol PEG;
[0028] The non-solvent is selected from deionized water and anhydrous ethanol or a combination of the two.
[0029] Furthermore, the step S2 comprises:
[0030] Step S21: uniformly coating the casting liquid on the support layer;
[0031] Step S22: staying for a period of time, then immersing in a non-solvent coagulation bath, and performing instantaneous phase transformation at room temperature to obtain a bicontinuous structure polymer electrolyte membrane.
[0032] Furthermore, the step S21 includes:
[0033] The supporting layer is a polyolefin microporous membrane, and the polyolefin microporous membrane is a biaxially oriented polyethylene PE diaphragm;
[0034] The step S22 comprises:
[0035] The non-solvent coagulation bath is one of deionized water and anhydrous ethanol or a combination of the two.
[0036] Furthermore, the step S3 comprises:
[0037] The electrolyte consists of lithium hexafluorophosphate LiPF6, ethylene carbonate EC, dimethyl carbonate DMC, and ethyl methyl carbonate EMC, wherein the volume ratio of EC:DMC:EMC is 1:1:1, and the molar concentration of lithium hexafluorophosphate LiPF6 is 1 mol / L.
[0038] A button cell comprises a bicontinuous structure polyolefin microporous supported gel polymer electrolyte located between a positive electrode material and a negative electrode material.
[0039] A polymer lithium ion battery cell comprises: the cell is assembled from a bicontinuous structure polyolefin microporous supported gel polymer electrolyte, a positive electrode material and a negative electrode material by a winding process.
[0040] Compared with the prior art, the present invention has the following beneficial effects:
[0041] 1. The present invention adopts an immersion precipitation phase separation method to coat a bicontinuous polymer electrolyte membrane on a polyolefin microporous membrane support material and immerse it in an electrolyte to prepare a three-layer gel polymer electrolyte. The polymer electrolyte membrane interface layer provides excellent conductivity and electrochemical properties, and the polyolefin porous membrane support layer provides excellent mechanical properties for the polymer electrolyte membrane. Compared with commercial liquid electrolytes, the bicontinuous structure polyolefin microporous membrane supported gel polymer electrolyte has good comprehensive performance, and the room temperature ionic conductivity reaches 1.2×10 -3 S / cm, the elongation at break is 142%, the electrochemical stability window can reach 5.2V, and the lithium ion migration number is as high as 0.90.
[0042] 2. The bicontinuous structure constructed by the present invention provides an effective channel for the diffusion and migration of lithium ions in the electrolyte, with a liquid absorption rate of up to 210%, so that the gel polymer electrolyte has high ionic conductivity; the polymer electrolyte membrane with a bicontinuous structure is tightly attached to both sides of the polyolefin microporous membrane, effectively improving the interface compatibility between the electrolyte and the electrode; the gel polymer electrolyte supported by the polyolefin microporous membrane with a bicontinuous structure obtained by the immersion phase separation technology can effectively inhibit the growth of lithium dendrites and promote stable battery circulation.
[0043] 3. The method and production process of the present invention are simple, and the raw materials are cheap and easily available, which provides conditions for industrial production and realizes the decoupling of mechanical properties and electrochemical properties. Compared with the prior art, the technical solution of the present invention can better solve the problems of harsh preparation conditions of gel polymer electrolytes and difficulty in achieving both mechanical strength and electrochemical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 SEM of the bicontinuous structured polyolefin microporous membrane-supported gel polymer electrolyte of Experiments 1-3;
[0045] Figure 2 is the bulk impedance value of the bicontinuous structure polyolefin microporous membrane supported gel polymer electrolyte at 25°C in Experiments 1-3;
[0046] Figure 3 The linear sweep voltammogram of the bicontinuous structure polyolefin microporous membrane supported gel polymer electrolyte of Experiment 1-3 at a scan rate of 0.1 mV / s;
[0047] Figure 4 Polarization curves of lithium symmetric cells assembled with bicontinuous polyolefin microporous membrane-supported gel polymer electrolytes in Experiment 1-3. The inset shows the impedance changes of the symmetric cells before and after polarization.
[0048] Figure 5 The stress-strain curves of the bicontinuous structured polyolefin microporous membrane-supported gel polymer electrolyte of Experiments 1-3. DETAILED DESCRIPTION
[0049] It should be noted that relational terms such as "first" and "second" are used only to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0050] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0051] Embodiment 1
[0052] This embodiment proposes a bicontinuous structure polyolefin microporous supported gel polymer electrolyte, which has a thickness of 11-13 μm and is prepared by gelling the modified polyolefin microporous membrane as a matrix in an electrolyte; wherein the bicontinuous structure of polyvinylidene fluoride PVDF-polymethyl methacrylate PMMA-polyethylene glycol PEG interface layer is tightly attached to both sides of the polyolefin microporous membrane, effectively improving the interface compatibility between the electrolyte and the electrode. Compared with commercial liquid electrolytes, the gel polymer electrolyte prepared by the present invention has excellent comprehensive performance, the electrochemical stability window can reach 5.2V, and the lithium ion migration number can reach 0.90.
[0053] That is, the bicontinuous structure polyolefin microporous supported gel polymer electrolyte is prepared by gelling a modified polyolefin microporous membrane in an electrolyte solution as a polymer skeleton; the modified polyethylene microporous membrane consists of three layers, including a polyolefin microporous membrane support layer and a bicontinuous structure polymer electrolyte membrane interface layer.
[0054] The polyolefin microporous membrane maintains a certain mechanical support effect and has good electrochemical stability; the interface layer of the bicontinuous structure of polyvinylidene fluoride PVDF-polymethyl methacrylate PMMA-polyethylene glycol PEG polymer electrolyte membrane obtained by the immersion precipitation phase separation method is tightly attached to both sides of the polyolefin microporous membrane, which not only ensures high ionic conductivity, but also effectively improves the interface compatibility between the electrolyte and the electrode; after the gel polymer electrolyte is assembled into a battery, electrochemical tests show that compared with commercial liquid lithium-ion batteries, the gel polymer electrolyte has higher lithium-ion batteries, better mechanical properties and electrochemical stability.
[0055] The above-mentioned bicontinuous structure polyolefin microporous supported gel polymer electrolyte is prepared by the following method:
[0056] Step S1: preparing a bicontinuous polymer electrolyte membrane casting solution;
[0057] Step S2: Based on the casting solution prepared in step S1, a bicontinuous polymer electrolyte membrane is prepared by an immersion precipitation phase separation method;
[0058] Step S3: After vacuum drying the bicontinuous structure polymer electrolyte membrane obtained in step S2, immerse it in an electrolyte solution in a glove box for adsorption and gelation, and finally obtain a bicontinuous structure polyolefin microporous membrane-supported gel polymer electrolyte.
[0059] In this embodiment, specifically, step S1 includes:
[0060] Step S11: dissolving polyvinylidene fluoride (PVDF) and polymethyl methacrylate (PMMA) in N-methylpyrrolidone (NMP) solvent in a proportion to form a polymer solution;
[0061] Step S12: After adding additives and non-solvents into the polymer solution, sealing is performed;
[0062] Step S13: performing ultrasonic oscillation;
[0063] Step S14: placing the mixture in a water bath with magnetic stirring, and letting it stand to remove bubbles to obtain a casting solution.
[0064] In this embodiment, specifically, step S11 includes:
[0065] The mass ratio of polyvinylidene fluoride PVDF and polymethyl methacrylate PMMA is 5-7:5-3;
[0066] The mass percentage of N-methylpyrrolidone NMP solvent is 89-91%;
[0067] The step S12 comprises:
[0068] The additive is polyethylene glycol PEG-400, which accounts for 30-40% of the polymer solution by mass;
[0069] The non-solvent is anhydrous ethanol, accounting for 3-5% of the polymer solution by mass;
[0070] The addition amount of polyvinylidene fluoride PVDF, polymethyl methacrylate PMMA and polyethylene glycol PEG-400 is 6-8% of the mass of N-methylpyrrolidone NMP solvent and anhydrous ethanol; that is, the mass concentration of the casting solution is 6-8%;
[0071] The step S13 comprises:
[0072] Ultrasonic oscillation for 30 min;
[0073] The step S14:
[0074] The mixture is stirred magnetically in a water bath at 40-60°C for 4-6 hours, the stirring speed is controlled at 400-500 r / min, and the standing time is 12-24 hours; preferably, the mixture is stirred magnetically in a water bath at 40-60°C for 4 hours, and the standing time is 24 hours.
[0075] It should be noted that the weight percentages of the raw materials in the casting solution are as follows:
[0076] Polymethyl methacrylate PMMA 2-4%, polyvinylidene fluoride PVDF 2-6%, N-methylpyrrolidone NMP 89-91%, polyethylene glycol PEG 0.1-2%, anhydrous ethanol 1-3%.
[0077] In this embodiment, specifically, step S2 includes:
[0078] Step S21: using a 9 μm polyolefin microporous membrane as a support material, and uniformly coating the casting liquid on the polyolefin microporous membrane; it should be noted that a thin support body can achieve strong mechanical properties with controllable thickness;
[0079] Step S22: staying for a period of time, then immersing in a non-solvent coagulation bath, and performing instantaneous phase transformation at room temperature to obtain a bicontinuous structure polymer electrolyte membrane.
[0080] In this embodiment, specifically, step S21 includes:
[0081] The gap between the casting blades is 5-10 μm; in this embodiment, the gap between the casting blades is 10 μm;
[0082] The step S22 comprises:
[0083] The residence time is 5min;
[0084] The non-solvent coagulation bath is deionized water, the coagulation bath phase transition time is 12-24 hours, and the coagulation bath temperature is maintained at 25°C; preferably, the coagulation bath phase transition time is 24 hours, and the coagulation bath temperature is 25°C.
[0085] In this embodiment, specifically, step S3 includes:
[0086] The vacuum drying temperature is 60-80°C and the drying time is 12-24h;
[0087] The whole gelation process was carried out in a glove box, with an oxygen content of 0.1-1.0 ppm and a water content of 0.01-0.05 ppm; the gelation time was 4 h;
[0088] The electrolyte consists of lithium hexafluorophosphate LiPF6, ethylene carbonate EC, dimethyl carbonate DMC, and ethyl methyl carbonate EMC, wherein the volume ratio of EC:DMC:EMC is 1:1:1, and the molar concentration of lithium hexafluorophosphate LiPF6 is 1 mol / L.
[0089] Embodiment 2
[0090] This embodiment is an application of a bicontinuous structure polyolefin microporous supported gel polymer electrolyte in a button cell proposed by the present invention.
[0091] Specifically, this embodiment provides a button-type battery, including: a bicontinuous structure polyolefin microporous supported gel polymer electrolyte located between a positive electrode material and a negative electrode material.
[0092] It should be noted that the positive electrode material includes LiCoO2, LiMnO4 or LiFePO4; and the negative electrode material is artificial graphite.
[0093] That is, the positive electrode material, the bicontinuous structure polyolefin microporous supported gel polymer electrolyte and the negative electrode material are assembled into a button battery in a glove box in sequence.
[0094] The button battery can be used in electronic products such as electronic dictionaries, watches, calculators, etc.
[0095] Embodiment 3
[0096] This embodiment is an application of a bicontinuous structure polyolefin microporous supported gel polymer electrolyte in a polymer lithium ion battery proposed by the present invention.
[0097] Specifically, this embodiment provides a polymer lithium-ion battery, including: a battery cell and a protection circuit;
[0098] The battery core is assembled from a double-continuous structure polyolefin microporous supported gel polymer electrolyte, a positive electrode material and a negative electrode material by a winding process.
[0099] Furthermore, the preparation process of the battery cell is as follows:
[0100] The bicontinuous structure polyolefin microporous supported gel polymer electrolyte, positive electrode material and negative electrode material are assembled into a battery cell by a winding process;
[0101] Spot weld the positive electrode with an aluminum tab and spot weld the negative electrode with a nickel tab, then dry the battery cell in a vacuum drying oven at 65-75°C for 15-20 hours and take it out;
[0102] The dried battery cell is placed in an aluminum-plastic film bag, which is then sealed with a vacuum sealer. A small air bag is reserved in the bag during sealing. The bag is allowed to stand for 5-8 hours before being formed. After the formation is completed, the gas generated by the formation enters the air bag and is sealed again to obtain a soft-pack polymer lithium-ion battery.
[0103] It should be noted that the positive electrode material includes LiCoO2, LiMnO4 or LiFePO4; and the negative electrode material is artificial graphite.
[0104] Embodiment 4
[0105] In order to verify the effect of the present invention, the following comparative experiment was carried out in this embodiment.
[0106] Experiment 1:
[0107] A method for preparing a bicontinuous structure polyolefin microporous membrane supported gel polymer electrolyte comprises the following steps:
[0108] (1) Preparation of bicontinuous polymer electrolyte membrane casting solution
[0109] 1.5 g of polyvinylidene fluoride PVDF and 1.5 g of polymethyl methacrylate PMMA were mixed and dissolved in 37.5 g of N-methylpyrrolidone NMP solvent, 0.9 g of polyethylene glycol PEG-400 was added as an additive, and 1.125 g of anhydrous ethanol was added as a non-solvent. After sealing, ultrasonic oscillation was performed for 30 minutes, and then placed in a 45°C water bath with magnetic stirring for 6 hours, and allowed to stand for 12 hours to remove bubbles to obtain a casting solution.
[0110] (2) Preparation of bicontinuous polymer electrolyte membrane using immersion phase separation technology
[0111] A 9μm polyolefin microporous membrane was used as the supporting material, the casting knife gap was adjusted to 10μm, the polymer membrane casting liquid was evenly coated on the polyolefin microporous membrane, left for 5 minutes, and then immersed in deionized water and subjected to instantaneous phase inversion at room temperature to obtain a bicontinuous structure polymer electrolyte membrane with a thickness of 13μm.
[0112] SEM observations show that the polymer electrolyte film exhibits an obvious bicontinuous structure and is connected in all directions in space, which is conducive to efficient material transport and diffusion within the material, thereby improving the utilization rate of active sites within the material. It not only ensures that the membrane has a high liquid absorption rate, but also makes a great contribution to improving liquid retention capacity.
[0113] (3) After vacuum drying the bicontinuous polymer electrolyte membrane obtained in step (2), immersing it in an electrolyte in a glove box for adsorption and gelation, finally obtaining a bicontinuous polyolefin microporous membrane-supported gel polymer electrolyte. The electrolyte consists of LiPF6, ethylene carbonate EC, dimethyl carbonate DMC, and ethyl methyl carbonate EMC, wherein the volume ratio of EC:DMC:EMC is 1:1:1, and the molar concentration of LiPF6 is 1 mol / L.
[0114] Figure 2 The prepared bicontinuous structure polyolefin microporous membrane supported gel polymer electrolyte is sandwiched between stainless steel electrodes and the AC impedance spectrum curve is obtained by testing at room temperature. Because stainless steel blocking electrodes are used, there is no electrochemical reaction, so the arc part representing the electrochemical reaction in the impedance spectrum can be regarded as infinite in diameter, so it is shown as an approximate diameter in the figure. The room temperature ionic conductivity of the prepared bicontinuous structure polyolefin microporous membrane supported gel polymer electrolyte is 1.2×10 -3 S / cm.
[0115] Figure 3 The test results of linear sweep voltammetry of the bicontinuous structure polyolefin microporous membrane-supported gel polymer electrolyte (stainless steel is used as the working positive electrode, metallic lithium is used as the negative electrode and the reference electrode, and the gel polymer electrolyte is sandwiched therein), and its electrochemical stability window is 5.2V.
[0116] Figure 4 Polarization curve of lithium symmetric battery assembled with bicontinuous polyolefin microporous membrane supporting gel polymer electrolyte. The inset shows the impedance change of the symmetric battery before and after polarization. The figure shows that the PMMA / PVDF / PEG conductive interface layer can accelerate the charge transfer at the gel polymer electrolyte / metal electrode interface, effectively improving the interfacial compatibility between the electrolyte and the electrode. At the same time, it can be calculated that the lithium ion migration number can reach 0.90.
[0117] Figure 5 The stress-strain curve of the bicontinuous structure polyolefin microporous membrane supporting the gel polymer electrolyte. It can be seen from the figure that with the introduction of the interface layer of the bicontinuous structure polymer electrolyte membrane, the pores are connected to each other, which is conducive to the improvement of the tensile properties.
[0118] Specifically, during the preparation of the bicontinuous structure polymer electrolyte, the phase inversion temperature was maintained at 25° C. and the phase inversion time was 12 h.
[0119] Experiment 2:
[0120] A method for preparing a bicontinuous structure polyolefin microporous membrane supported gel polymer electrolyte comprises the following steps:
[0121] (1) Preparation of bicontinuous polymer electrolyte membrane casting solution
[0122] 2.1 g of polyvinylidene fluoride PVDF and 0.9 g of polymethyl methacrylate PMMA were mixed and dissolved in 37.5 g of N-methylpyrrolidone NMP solvent, 0.9 g of polyethylene glycol PEG-400 was added as an additive, and 1.125 g of anhydrous ethanol was added as a non-solvent. After sealing, the mixture was ultrasonically oscillated for 30 min, then placed in a 45°C water bath with magnetic stirring for 6 h, and allowed to stand for 12 h to remove bubbles to obtain a casting solution.
[0123] (2) Preparation of bicontinuous polymer electrolyte membrane using immersion precipitation phase separation method
[0124] A 9μm polyolefin microporous membrane was used as the supporting material, the casting knife gap was adjusted to 10μm, the casting liquid was evenly coated on the polyolefin microporous membrane, left for 5 minutes, and then immersed in deionized water and subjected to instantaneous phase inversion at room temperature to obtain a bicontinuous structure gel polymer electrolyte membrane with a thickness of 13μm.
[0125] (3) After the obtained bicontinuous structure polymer electrolyte membrane is vacuum dried, it is immersed in an electrolyte in a glove box for adsorption and gelation, and finally a bicontinuous structure polyolefin microporous membrane supported gel polymer electrolyte is obtained. The electrolyte is composed of LiPF6, ethylene carbonate EC, dimethyl carbonate DMC, and ethyl methyl carbonate EMC, wherein the volume ratio of EC:DMC:EMC is 1:1:1, and the molar concentration of LiPF6 is 1 mol / L.
[0126] Experiment 3:
[0127] A method for preparing a bicontinuous structure polyolefin microporous membrane supported gel polymer electrolyte comprises the following steps:
[0128] (1) Preparation of bicontinuous polymer electrolyte membrane casting solution
[0129] 1.8 g of polyvinylidene fluoride PVDF and 1.2 g of polymethyl methacrylate PMMA were mixed and dissolved in 37.5 g of N-methylpyrrolidone NMP solvent, 0.9 g of polyethylene glycol PEG-400 was added as an additive, and 1.125 g of anhydrous ethanol was added as a non-solvent. After sealing, ultrasonic oscillation was performed for 30 minutes, and then placed in a 45°C water bath with magnetic stirring for 6 hours, and allowed to stand for 12 hours to remove bubbles to obtain a casting solution.
[0130] (2) Preparation of bicontinuous polymer electrolyte membrane using immersion precipitation phase separation method
[0131] A 9μm polyolefin microporous membrane was used as the supporting material, the casting knife gap was adjusted to 10μm, the casting liquid was evenly coated on the polyolefin microporous membrane, left for 5 minutes, and then immersed in deionized water and subjected to instantaneous phase inversion at room temperature to obtain a bicontinuous structure polymer electrolyte membrane with a thickness of 13μm.
[0132] (3) After the obtained bicontinuous polymer electrolyte membrane is vacuum dried, it is immersed in an electrolyte in a glove box for adsorption and gelation, and finally a cavity porous structure polyolefin microporous membrane supported gel polymer electrolyte is obtained. The electrolyte is composed of LiPF6, ethylene carbonate EC, dimethyl carbonate DMC, and ethyl methyl carbonate EMC, wherein the volume ratio of EC:DMC:EMC is 1:1:1, and the molar concentration of LiPF6 is 1 mol / L.
[0133] Comparative Example 4:
[0134] As a comparison with Experiment 1, a liquid electrolyte was selected to assemble a lithium symmetrical battery: the battery shell was 2023 type, the negative electrode shell was opened upward and laid flat on the panel; the spring sheet was placed in the negative electrode shell; the gasket was clamped and placed on the spring sheet, and then the graphite pole piece was clamped and placed in the middle of the gasket; the polyolefin microporous membrane was clamped to cover the graphite pole piece, and 1M LiPF6, ethylene carbonate EC, dimethyl carbonate DMC and ethyl methyl carbonate EMC were added dropwise with a pipette, wherein the volume ratio of EC: DMC: EMC was 1:1:1. (At this time, there were two differences between Comparative Example 1 and Experiments 1-3: (1) it did not contain a polymer electrolyte membrane interface layer; (2) the electrolyte existed only in liquid form, not in gel form); the lithium metal negative electrode was clamped and placed in the middle of the polyolefin microporous membrane, the positive electrode shell was clamped with tweezers to cover it, and a button battery packaging machine was used to press it to obtain a button battery, and the amount of electrolyte added to the button battery was 60μL.
[0135] Comparative Example 5:
[0136] A method for preparing a dense pore structure polyolefin microporous membrane supported gel polymer electrolyte comprises the following steps:
[0137] (1) Preparation of dense pore structure polymer electrolyte membrane casting solution
[0138] 3 g of polyvinylidene fluoride (PVDF) was dissolved in 37.5 g of N-methylpyrrolidone (NMP) solvent, 0.9 g of polyethylene glycol (PEG-400) was added as an additive, and 1.125 g of anhydrous ethanol was added as a non-solvent. The mixture was sealed and ultrasonically oscillated for 30 min. The mixture was then placed in a 45°C water bath and magnetically stirred for 6 h. The mixture was allowed to stand for 12 h to remove bubbles, and the casting solution was obtained.
[0139] (2) Preparation of dense pore structure gel polymer electrolyte membrane by immersion precipitation phase separation method
[0140] A 9μm polyolefin microporous membrane was used as the supporting material, the casting knife gap was adjusted to 10μm, the casting liquid was evenly coated on the polyolefin microporous membrane, left for 5 minutes, and then immersed in deionized water, and an instantaneous phase inversion was performed at room temperature to obtain a dense pore structure polymer electrolyte membrane with a thickness of 13μm.
[0141] (3) After the obtained dense pore structure polymer electrolyte membrane is vacuum dried, it is immersed in an electrolyte in a glove box for adsorption and gelation, and finally a dense pore structure polyolefin microporous membrane supported gel polymer electrolyte is obtained. The electrolyte is composed of LiPF6, ethylene carbonate EC, dimethyl carbonate DMC, and ethyl methyl carbonate EMC, wherein the volume ratio of EC:DMC:EMC is 1:1:1, and the molar concentration of LiPF6 is 1 mol / L.
[0142] Comparative Example 6:
[0143] A method for preparing a cavity porous structure polyolefin microporous membrane supported gel polymer electrolyte comprises the following steps:
[0144] (1) Preparation of casting solution for porous polymer electrolyte membrane
[0145] 2.7 g of polyvinylidene fluoride PVDF and 0.3 g of polymethyl methacrylate PMMA were mixed and dissolved in 37.5 ml of N-methylpyrrolidone NMP solvent, 0.9 g of polyethylene glycol PEG-400 was added as an additive, and 1.125 g of anhydrous ethanol was added as a non-solvent. After sealing, ultrasonic oscillation was performed for 30 minutes, and then placed in a 45°C water bath with magnetic stirring for 6 hours, and allowed to stand for 12 hours to remove bubbles to obtain a casting solution.
[0146] (2) Preparation of porous polymer electrolyte membranes using immersion precipitation phase separation method
[0147] A 9μm polyolefin microporous membrane was used as the supporting material, the casting knife gap was adjusted to 10μm, the casting liquid was evenly coated on the polyolefin microporous membrane, left for 5 minutes, and then immersed in deionized water and subjected to instantaneous phase inversion at room temperature to obtain a 13μm thick cavity porous structure polymer electrolyte membrane.
[0148] After the obtained cavity porous structure polymer electrolyte membrane is vacuum dried, it is immersed in the electrolyte in the glove box for adsorption and gelation, and finally a cavity porous structure polyolefin microporous membrane supported gel polymer electrolyte is obtained. The electrolyte is composed of LiPF6, ethylene carbonate EC, dimethyl carbonate DMC, and ethyl methyl carbonate EMC, wherein the volume ratio of EC: DMC: EMC is 1:1:1, and the molar concentration of LiPF6 is 1 mol / L.
[0149] The electrochemical performance of the bicontinuous polyolefin microporous membrane-supported gel polymer electrolyte prepared in the above experiments 1-3 and the electrolyte prepared in comparative examples 4-6 was tested, and the results of the electrolyte liquid retention, AC internal resistance and ionic conductivity are shown in Table 1:
[0150] Table 1 Comparison results of electrolyte retention, AC internal resistance and ionic conductivity
[0151]
[0152]
[0153] From the comparison of the test results, it can be seen that compared with the gel polymer electrolyte without a bicontinuous structure, the bicontinuous structure gel polymer electrolyte described in Experiments 1-3 has significantly improved the electrolyte retention capacity, and the ion conductivity and lithium ion migration number have been greatly improved; Figure 5As shown, compared with the commercial polyolefin microporous membrane liquid electrolyte prepared in Comparative Example 4, the dense pore structure gel polymer electrolyte prepared in Comparative Example 5, and the cavity porous structure gel polymer electrolyte prepared in Comparative Example 6, the electrochemical performance of the dual continuous structure gel polymer electrolyte prepared in Experiments 1-3 is also significantly improved.
[0154] The above-mentioned embodiments only express the specific implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the protection scope of the present application. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the technical solution concept of the present application, and these all belong to the protection scope of the present application.
[0155] This background section is provided to generally present the context of the invention, and the work of the presently named inventors, the work to the extent described in this background section, and aspects of this section that did not constitute prior art at the time of application are neither explicitly nor implicitly admitted to be prior art to the present invention.
Claims
1. A bicontinuous structure polyolefin microporous supported gel polymer electrolyte, characterized in that: The components include: 10-40wt% polymer electrolyte skeleton, 60-90wt% organic electrolyte; The polymer electrolyte skeleton comprises: a support layer and a bicontinuous polymer electrolyte membrane interface layer; the organic electrolyte comprises: an organic solvent and a lithium salt.
2. The bicontinuous structure polyolefin microporous supported gel polymer electrolyte according to claim 1, characterized in that: The supporting layer is a polyethylene PE diaphragm, a polypropylene PP diaphragm, a polyimide PI diaphragm or a non-woven fabric diaphragm; The bicontinuous polymer electrolyte membrane is prepared by an immersion precipitation phase separation method; wherein the polymer matrix is selected from a combination of two or more of polyvinylidene fluoride PVDF, polyvinylidene fluoride-hexafluoropropylene PVDF-HFP, polymethyl methacrylate PMMA, and polyethylene oxide PEO; the solvent is selected from a polar solvent, including one or more of N-methylpyrrolidone NMP, N,N-dimethylformamide DMF, tetrahydrofuran THF, dimethyl sulfoxide DMSO, and 1,4-epoxyhexacyclopentane; the non-solvent is selected from one or a combination of deionized water and anhydrous ethanol; the additive is selected from one of polyvinylpyrrolidone PVP, polyethylene oxide PEO, and polyethylene glycol PEG; The organic solvent is selected from one or more combinations of ethylene carbonate EC, propylene carbonate PC, dimethyl carbonate DMC, diethyl carbonate DEC, ethyl methyl carbonate EMC, N,N-dimethylformamide DMF, 1,2-dimethoxyethane DME; The lithium salt is selected from one of lithium hexafluorophosphate LiPF6, lithium perchlorate LiClO4, lithium tetrafluoroborate LiBF4, lithium hexafluoroarsenate LiAsF6, lithium trifluoromethanesulfonate LiOTf, lithium bis(trifluoromethanesulfonyl)imide LiTFSI, lithium dioxalatoborate LiBOB, lithium bis(fluorosulfonyl)imide LiFSI and lithium oxalatodifluoroborate LiDFOB.
3. A method for preparing a bicontinuous structure polyolefin microporous supported gel polymer electrolyte, characterized in that: The steps include: Step S1: preparing a bicontinuous polymer electrolyte membrane casting solution; Step S2: Based on the casting solution prepared in step S1, a bicontinuous polymer electrolyte membrane is prepared by an immersion precipitation phase separation method; Step S3: After vacuum drying the bicontinuous structure polymer electrolyte membrane obtained in step S2, immerse it in an electrolyte solution in a glove box for adsorption and gelation, and finally obtain a bicontinuous structure polyolefin microporous membrane-supported gel polymer electrolyte.
4. The method for preparing a bicontinuous structure polyolefin microporous supported gel polymer electrolyte according to claim 3, characterized in that: The step S1 comprises: Step S11: dissolving the polymer matrix in a polar solvent according to a certain proportion to form a polymer solution; Step S12: After adding additives and non-solvents into the polymer solution, sealing is performed; Step S13: performing ultrasonic oscillation; Step S14: placing the mixture in a water bath with magnetic stirring, and letting it stand to remove bubbles to obtain a casting solution.
5. The method for preparing a bicontinuous structure polyolefin microporous supported gel polymer electrolyte according to claim 4, characterized in that: The step S11 comprises: The polymer matrix is a combination of two or more of polyvinylidene fluoride PVDF, polyvinylidene fluoride-hexafluoropropylene PVDF-HFP, polymethyl methacrylate PMMA, and polyethylene oxide PEO; The polar solvent is selected from one or more combinations of N-methylpyrrolidone NMP, N,N-dimethylformamide DMF, tetrahydrofuran THF, dimethyl sulfoxide DMSO, and 1,4-epoxyhexacyclic ring; The step S12 comprises: The additive is selected from one of polyvinyl pyrrolidone PVP, polyethylene oxide PEO and polyethylene glycol PEG; The non-solvent is selected from deionized water and anhydrous ethanol or a combination of the two.
6. The method for preparing a bicontinuous structure polyolefin microporous supported gel polymer electrolyte according to claim 3, characterized in that: The step S2 comprises: Step S21: uniformly coating the casting liquid on the support layer; Step S22: staying for a period of time, then immersing in a non-solvent coagulation bath, and performing instantaneous phase transformation at room temperature to obtain a bicontinuous structure polymer electrolyte membrane.
7. The method for preparing a bicontinuous structure polyolefin microporous supported gel polymer electrolyte according to claim 6, characterized in that: The step S21 comprises: The supporting layer is a polyolefin microporous membrane, and the polyolefin microporous membrane is a biaxially oriented polyethylene PE diaphragm; The step S22 comprises: The non-solvent coagulation bath is one of deionized water and anhydrous ethanol or a combination of the two.
8. The method for preparing a bicontinuous structure polyolefin microporous supported gel polymer electrolyte according to claim 3, characterized in that: The step S3 comprises: The electrolyte consists of lithium hexafluorophosphate LiPF6, ethylene carbonate EC, dimethyl carbonate DMC, and ethyl methyl carbonate EMC, wherein the volume ratio of EC:DMC:EMC is 1:1:1, and the molar concentration of lithium hexafluorophosphate LiPF6 is 1 mol / L.
9. A button battery, characterized in that: include: The bicontinuous structure polyolefin microporous supported gel polymer electrolyte is located between the positive electrode material and the negative electrode material.
10. A polymer lithium-ion battery cell, characterized in that: include: The battery core is assembled from a double-continuous structure polyolefin microporous supported gel polymer electrolyte, a positive electrode material and a negative electrode material by a winding process.
Citation Information
Cited By
Polyimide modified nanofiber diaphragm composite gel polymer electrolyte and preparation method thereof
CN119742432A
High-temperature polymer lithium ion battery and preparation method thereof