Ternary fluorine-containing organic lithium salt additive, electrolyte and lithium ion battery

By developing ternary fluorophosphimide lithium salt as an additive for lithium-ion batteries, the problem of insufficient research on binary or multivariate organic lithium salts in the existing technology has been solved, and the rapid transmission of lithium ions and the improvement of battery cycle life has been achieved. A CEI film with low interface impedance is formed, which alleviates hydrofluoric acid erosion and improves the electrochemical performance of the battery.

CN118943486APending Publication Date: 2024-11-12LIONGO (CHANGZHOU) NEW ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410971255.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

There are few researches on binary or multivariate organic lithium salts in the prior art, especially in lithium-ion batteries, which lead to the underdeveloped application prospects in electrolytes.

Method used

A ternary fluorine-containing organolithium salt additive, specifically a ternary fluorine-phosphorimide lithium salt, was developed. By nucleophilic substitution reaction between fluorine-chlorophosphate monomer and triamino monomer, and then substituted with a lithium source. The reaction preparation has excellent thermal stability and large anion radius, which enhances the dissociation ability of lithium ions, and forms a CEI film with low interface impedance on the positive electrode surface to alleviate the erosion of hydrofluoric acid on the positive electrode.

Benefits of technology

It improves the rapid transmission ability of lithium ions, enhances the conductivity of the electrolyte, extends the electrochemical cycle life of the lithium battery, reduces the loss of active lithium, and improves the overall electrochemical performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943486A_ABST
    Figure CN118943486A_ABST
Patent Text Reader

Abstract

The invention provides a ternary fluorine-containing organic lithium salt additive. The ternary fluorine-containing organic lithium salt additive has a structure as shown in a structural formula A, wherein M is Li, R1 is a fluorine atom or an oxygen atom, R2 is empty, methyl, n-propyl, allyl, 1, 2, 2-trifluoroethane, 1, 1, 1-trifluoroethane or perfluoroethane, and R3 is a hydrogen atom or methyl. Compared with the prior art, the ternary fluorine-containing organic lithium salt additive provided by the invention is a ternary fluorine phosphorimide organic lithium salt, and the lithium cations are easier to dissociate due to the special structural excellence of the ternary fluorine phosphorimide organic lithium salt, so that the rapid transmission capability of the lithium ions can be effectively improved; meanwhile, high-stability low-impedance interface protection films can be formed on the surfaces of the positive electrode and the negative electrode through induction respectively, so that erosion damage of hydrofluoric acid can be effectively relieved, the loss of active lithium is reduced, and the electrochemical cycle life of the lithium ion battery is prolonged. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of fluorine-containing organic lithium salts, and more specifically to a ternary fluorine-containing organic lithium salt additive, an electrolyte and a lithium ion battery. Background Art

[0002] Fluorinated organic lithium salts are important fluorinated organic ion compounds. They have important industrial application value in the fields of high-performance non-aqueous electrolyte materials for clean energy devices such as secondary batteries and supercapacitors, as well as new high-efficiency catalysts. Therefore, people have been committed to the synthesis and application research of new fluorinated organic lithium salts. At present, this type of research is mainly focused on monobasic salts (i.e., the molecule contains only one lithium cation), such as perfluoroalkylsulfonyl imide and its alkali metal salts, representative of which are lithium bis(trifluoromethylsulfonyl)imide (LiTFSI) and lithium bis(fluorosulfonyl)imide (LiFSI).

[0003] At present, most of the research focuses on the development of monobasic salts. In 1994, D.DdesMarteau synthesized a small molecule binary sodium salt containing two sulfonyl imide groups, and further polymerized it to obtain a polymer sodium salt with excellent site chemical properties; but its synthesis steps are complicated and not easy to industrialize. Patent CN1450052A provides a method for preparing a ternary sulfonyl imide metal salt using dichlorosulfonyl imide and sulfonamide alkali metal salt. The prepared ternary sulfonyl imide salt with a straight chain structure has high ionic conductivity and high electrochemical window; but the specific electrochemical properties are unknown. Patent CN116621739A provides a method for synthesizing a binary salt by adding a diol to an isocyanate; but this method has high requirements for the raw material sulfonyl isocyanate and has certain limitations.

[0004] In summary, the current research on new organic lithium salts is concentrated on monovalent salts, such as LiTFSI and LiFSI, while there are few reports on binary or polyvalent organic lithium salts, especially the application of binary, ternary or polyvalent organic lithium salts as electrolyte components in secondary lithium-ion batteries. Therefore, the development of preparation methods and application exploration of binary, ternary or polyvalent organic lithium salts has extremely high application prospects. Summary of the invention

[0005] In view of this, the object of the present invention is to provide a ternary fluorine-containing organic lithium salt additive, an electrolyte and a lithium ion battery. The ternary fluorine-containing organic lithium salt additive provided by the present invention is a ternary fluorophosphoryl imide lithium salt, which has excellent thermal stability and a larger anion radius. At the same time, the electron-withdrawing group contained at the end of the molecular chain makes lithium ions easy to dissociate, thereby enhancing the ion transmission selectivity, increasing the lithium ion migration number, and effectively improving the ability of lithium ions to quickly deintercalate under large current charging and discharging. At the same time, during the battery charging process, the P=O bond contained in the structure is easily oxidized by the positive electrode active material after lithium removal on the positive electrode plate. After P=O is oxidized, the remaining F ions are easily combined with lithium ions, thereby improving the problem of poor ion conductivity of the oxidation film product on the positive electrode surface, and forming a positive electrode interface solid electrolyte (CEI) film with low interface impedance; and because the radius of the F ions and the lithium ions are close, the binding energy is very strong, and they can be well covered on the surface of the positive electrode material, which can effectively alleviate the erosion of the positive electrode by the hydrofluoric acid generated by the decomposition of lithium hexafluorophosphate, thereby reducing the loss of active lithium, and effectively improving the electrochemical performance of the lithium battery. The present invention also provides a non-aqueous electrolyte containing the lithium salt additive and a lithium ion battery containing the non-aqueous electrolyte.

[0006] The present invention provides a ternary fluorine-containing organic lithium salt additive having a structure shown in structural formula A:

[0007]

[0008] Among them, M is Li, R1 is a fluorine atom or an oxygen atom, R2 is a vacancy, a methyl group, a n-propyl group, a propenyl group, a 1,2,2-trifluoroethane group, a 1,1,1-trifluoroethane group or a perfluoroethane group, and R3 is a hydrogen atom or a methyl group.

[0009] Preferably, the structural formula A is any one of the following formulas (I) to (VII):

[0010]

[0011] Preferably, the preparation method of the ternary fluorine-containing organic lithium salt additive comprises the following steps:

[0012] Firstly, a fluorine-containing chlorophosphoric acid monomer and a triamino monomer undergo a nucleophilic substitution reaction to prepare a ternary fluorophosphoryl imide compound, and then a substitution reaction is carried out with a lithium source to obtain a ternary fluorine-containing organic lithium salt additive.

[0013] The ternary fluorine-containing organic lithium salt additive accounts for 0.1% to 2% of the weight of the electrolyte.

[0014] The present invention also provides an electrolyte comprising a lithium salt, a non-aqueous organic solvent and an electrolyte additive; the electrolyte additive comprises the ternary fluorine-containing organic lithium salt additive described in the above technical solution.

[0015] Preferably, the other lithium salt is selected from one or more of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, and lithium difluorobis(oxalatophosphate);

[0016] The lithium salt accounts for 11% to 16% of the weight of the electrolyte.

[0017] Preferably, the non-aqueous organic solvent is an organic ester solvent and / or an ether solvent; the organic ester solvent is one or more of ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl trifluoroethyl carbonate, di(2,2,2-trifluoroethyl) carbonate, ethyl formate, ethyl acetate, propyl acetate, and propyl propionate; the ether solvent is one or more of dimethyl ether, diethyl ether, methyl ethyl ether, ethylene glycol dimethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, and 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether;

[0018] The non-aqueous organic solvent accounts for 78.7% to 84.5% of the electrolyte by weight.

[0019] Preferably, the electrolyte additive is the ternary fluorine-containing organic lithium salt additive and an auxiliary additive.

[0020] Preferably, the auxiliary additive is selected from vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, vinyl sulfate, divinyl sulfate, propylene sulfate, 1,3-propane sultone, 1,3-propylene sultone, 1,4-butane sultone, 2,4-butane sultone, phenyl methanesulfonate, methylene methanedisulfonate, N-phenylbis(trifluoromethanesulfonyl)imide, triallyl phosphate, tris(trimethylsilane)phosphate, trimethyl phosphite, phosphorous acid One or more of triphenyl ester, tris(2,2,2-trifluoroethyl)phosphite, tetramethylmethylene diphosphate, propargyl phosphate, (2-allylphenoxy)trimethylsilane, tris(trimethylsilyl)borate, 1,3,5-triallyl isocyanurate, isocyanoethyl methacrylate, hexamethylene diisocyanate, p-phenylene diisocyanate, 2,4-toluene diisocyanate, adiponitrile, succinonitrile, glutaronitrile, 1,3,6-hexanetrinitrile, and 1,2-bis(cyanoethoxy)ethane;

[0021] The auxiliary electrolyte additive accounts for 2% to 4.3% of the electrolyte weight.

[0022] The present invention also provides a lithium-ion battery, comprising: a positive electrode, a negative electrode, a separator and an electrolyte, wherein the electrolyte is the electrolyte described in the above technical solution.

[0023] Preferably, the active material of the positive electrode is selected from lithium cobalt oxide, lithium manganese oxide, ternary nickel cobalt manganese lithium, lithium nickel manganese oxide, lithium iron phosphate or lithium manganese iron phosphate;

[0024] The active material of the negative electrode is selected from artificial graphite, natural graphite, lithium titanate, metallic lithium, silicon-carbon composite material or silicon oxide;

[0025] The diaphragm is selected from polypropylene, polyethylene diaphragm or polyethylene diaphragm coated with aluminum oxide on one side.

[0026] The present invention provides a ternary fluorine-containing organic lithium salt additive having a structure shown in structural formula A:

[0027]

[0028] Among them, M is Li, R1 is a fluorine atom or an oxygen atom, R2 is a vacancy, a methyl group, a n-propyl group, a propenyl group, a 1,2,2-trifluoroethane group, a 1,1,1-trifluoroethane group or a perfluoroethane group, and R3 is a hydrogen atom or a methyl group.

[0029] Compared with the prior art, the ternary fluorine-containing organic lithium salt additive provided by the present invention is a ternary fluorophosphoryl imide organic lithium salt, which is used as an additive. Benefiting from its special structural advantages, it can make lithium cations easier to dissociate, and can effectively improve the ability of lithium ion rapid transmission. At the same time, the special structure it contains can also form a stable and low-impedance CEI film on the surface of the positive electrode, which can effectively alleviate the corrosion and damage of hydrofluoric acid to the positive electrode, thereby improving the electrochemical cycle life of the lithium-ion battery. DETAILED DESCRIPTION

[0030] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] The purpose of the present invention is to provide a ternary fluorophosphoryl imide organic lithium salt additive, which has a special structural advantage that can make lithium cations easier to dissociate, can effectively improve the ability of lithium ion rapid transmission, and can also form a highly stable and low-impedance CEI film on the surface of the positive electrode, which can effectively alleviate the corrosion and damage of hydrofluoric acid to the positive electrode, thereby improving the electrochemical cycle life of the lithium-ion battery.

[0032] To achieve the above object, the present invention adopts the following technical solutions:

[0033] In the first aspect, the present invention provides a ternary fluorine-containing organic lithium salt additive, specifically a ternary centrosymmetric fluorophosphorylimide organic lithium salt having a structure shown in structural formula A:

[0034]

[0035] Among them, M is Li, R1 is a fluorine atom or an oxygen atom, R2 is a vacancy, a methyl group, a n-propyl group, a propenyl group, a 1,2,2-trifluoroethane group, a 1,1,1-trifluoroethane group or a perfluoroethane group, and R3 is a hydrogen atom or a methyl group.

[0036] In the present invention, the structural formula A is preferably any one of the following formulas (I) to (VII):

[0037]

[0038] In the present invention, the preparation method of the ternary fluorine-containing organic lithium salt additive preferably comprises the following steps:

[0039] Firstly, a fluorine-containing chlorophosphoric acid monomer and a triamino monomer undergo a nucleophilic substitution reaction to prepare a ternary fluorophosphoryl imide compound, and then a substitution reaction is carried out with a lithium source to obtain a ternary fluorine-containing organic lithium salt additive.

[0040] The synthetic route is as follows:

[0041]

[0042] The present invention adopts the chemical preparation method of the ternary fluorine-containing organic lithium salt additive, which has a clear process route, mild conditions, easy control, and broad application prospects.

[0043] Compared with the prior art, the ternary fluorophosphoryl imide organic lithium salt additive provided by the present invention has a larger anion radius, so that lithium ions are easier to dissociate, and thus has excellent solubility in the electrolyte. When used as a lithium salt additive, it can effectively increase the number of lithium ion migration, increase the conductivity of the electrolyte, enhance the ability of lithium ion rapid deintercalation, and alleviate the concentration polarization phenomenon under high current; at the same time, the rich fluorine-containing groups contained in the structure enhance the electrochemical reduction and decomposition of the overall molecule, so that the SEI passivation layer rich in LiF can be preferentially decomposed on the negative electrode surface to be constructed in situ, and LiF exhibits high Young's modulus and high surface energy are used to homogenize the lithium ion flux, which significantly improves the stability of the negative electrode-electrolyte interface. In addition, after the P=O contained in the structure is oxidized, the remaining F ions are easily combined with lithium ions, thereby improving the problem of poor conductivity of the product ions of the oxidation film on the positive electrode surface and forming a CEI film with low interface impedance. And because the radius of F ions and lithium ions are close, the binding energy is very strong and they can be well covered on the surface of the positive electrode material, which can effectively alleviate the corrosion of the positive electrode by hydrofluoric acid produced by the decomposition of lithium hexafluorophosphate, thereby reducing the loss of active lithium and effectively improving the electrochemical performance of lithium batteries.

[0044] In a second aspect, the present invention further provides an electrolyte comprising a lithium salt, a non-aqueous organic solvent and an electrolyte additive, wherein the electrolyte additive comprises the ternary fluorine-containing organic lithium salt additive described in the above technical solution.

[0045] In the present invention, the other lithium salt is preferably selected from one or more of lithium hexafluorophosphate (LiPF6), lithium perchlorate (LiClO4), lithium tetrafluoroborate (LiBF4), lithium bis(oxalatoborate) (LiBOB), lithium difluorooxalatoborate (LiODFB), and lithium difluorobis(oxalatophosphate) (LiDODFP). The present invention has no particular restrictions on the source of the other lithium salt, and commercially available products known to those skilled in the art can be used.

[0046] In the present invention, the lithium salt preferably accounts for 11% to 16% of the weight of the electrolyte.

[0047] In the present invention, the non-aqueous organic solvent is preferably an organic ester solvent and / or an ether solvent; wherein the organic ester solvent is preferably one or more of ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl trifluoroethyl carbonate, di(2,2,2-trifluoroethyl) carbonate, ethyl formate, ethyl acetate, propyl acetate, and propyl propionate; the ether solvent is preferably one or more of dimethyl ether, diethyl ether, methyl ethyl ether, ethylene glycol dimethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, and 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether. The present invention has no special restrictions on the source of the non-aqueous organic solvent, and commercially available products known to those skilled in the art can be used.

[0048] In the present invention, the non-aqueous organic solvent preferably accounts for 78.7% to 84.5% of the weight of the electrolyte.

[0049] In the present invention, the electrolyte additives are the ternary fluorine-containing organic lithium salt additive and the auxiliary additive.

[0050] In the present invention, the auxiliary additive is preferably selected from vinylene carbonate, vinyl ethylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, vinyl sulfate, disulfate, propylene sulfate, 1,3-propane sultone, 1,3-propylene sultone, 1,4-butane sultone, 2,4-butane sultone, phenyl methanesulfonate, methylene methanedisulfonate, N-phenylbis(trifluoromethanesulfonyl)imide, triallyl phosphate, tris(trimethylsilane)phosphate, trimethyl phosphite ... One or more of triphenyl phosphate, tris(2,2,2-trifluoroethyl)phosphite, tetramethylmethylene diphosphate, propargyl phosphate, (2-allylphenoxy)trimethylsilane, tris(trimethylsilane)borate, 1,3,5-triallyl isocyanurate, isocyanoethyl methacrylate, hexamethylene diisocyanate, p-phenylene diisocyanate, 2,4-toluene diisocyanate, adiponitrile, succinonitrile, glutaronitrile, 1,3,6-hexanetrinitrile, and 1,2-bis(cyanoethoxy)ethane. The present invention has no particular restrictions on the source of the electrolyte additive, and commercially available products known to those skilled in the art can be used.

[0051] In the present invention, the ternary fluorine-containing organic lithium salt additive preferably accounts for 0.1% to 2% of the weight of the electrolyte; the auxiliary additive preferably accounts for 2% to 4.3% of the weight of the electrolyte.

[0052] In a third aspect, the present invention further provides a lithium-ion battery, comprising: a positive electrode, a negative electrode, a separator and an electrolyte, wherein the electrolyte is the electrolyte described in the above technical solution.

[0053] In the present invention, the lithium ion battery is a lithium ion battery containing the electrolyte described in the above technical solution.

[0054] In the present invention, the active material of the positive electrode is preferably selected from lithium cobalt oxide, lithium manganese oxide, ternary nickel cobalt manganese lithium, nickel manganese oxide, lithium iron phosphate or lithium iron manganese phosphate, and more preferably ternary nickel cobalt manganese lithium (NCM811). The present invention has no special restrictions on the source of the active material of the positive electrode, and commercially available products known to those skilled in the art can be used.

[0055] In the present invention, the active material of the negative electrode is preferably selected from artificial graphite, natural graphite, lithium titanate, metallic lithium, silicon-carbon composite material or silicon oxide, and more preferably artificial graphite. The present invention has no particular restriction on the source of the active material of the negative electrode, and commercially available products well known to those skilled in the art can be used.

[0056] In the present invention, the diaphragm is preferably selected from polypropylene, polyethylene diaphragm or polyethylene diaphragm coated with aluminum oxide on one side, more preferably polyethylene diaphragm coated with aluminum oxide on one side. The present invention has no particular limitation on the source of the diaphragm, and commercial products known to those skilled in the art can be used.

[0057] Compared with the prior art, the lithium ion battery made using the electrolyte provided by the present invention has better electrochemical performance, which is specifically manifested in that the electrochemical performance of the lithium ion battery in the voltage range of 3.0V to 4.2V is greatly improved.

[0058] In order to further illustrate the present invention, the following examples are provided for detailed description. In the following examples of the present invention, if no specific conditions are specified, the reaction is carried out according to conventional conditions or conditions recommended by the manufacturer, and if no manufacturer is specified for the reagents or instruments used, all of them are conventional products that can be purchased commercially.

[0059] Example 1

[0060] (1) Preparation of compound (I), the specific steps are as follows:

[0061]

[0062] Under nitrogen atmosphere, anhydrous THF (300 mL) was added to a clean and dry 1000 mL three-necked flask equipped with a magnetic rotor, and then the flask was placed in an ice-water bath, stirring was started, and after THF dropped to 0°C, butyl triamine (4.12 g, 40.00 mmol) was added, and then a constant pressure dropping funnel was used to slowly add 200 mL of anhydrous THF solution pre-frozen to 0°C containing (2-methyl) fluorochlorophosphate (17.15 g, 130.00 mmol). After the addition was completed, the ice-water bath was removed and the resulting mixture was stirred at room temperature for 12 h. The residue was purified by a short pad of flash silica gel chromatography, the eluent was a mixture of n-hexane / dichloromethane (volume ratio 1:1), the solvent was removed by rotary evaporation, and anhydrous magnesium sulfate was used to dry to obtain a ternary fluorophosphorimide intermediate with a yield of 92.5%. TOF-SIMS (m / z): calcd.for C7H 19 F3N3O6P3[M+1] + ,391.04,found 391.05.

[0063] Under nitrogen atmosphere, add 150 mL of anhydrous ethanol and 150 mL of ethyl acetate to a clean and dry 500 mL three-necked flask equipped with a magnetic rotor, and then start stirring. Then place the flask in a low-temperature reactor, and after cooling to about 0°C, add the intermediate (19.55 g, 50.00 mmol) and lithium carbonate (11.84 g, 160.00 mmol) prepared in the previous step to the solution, and react for 12 hours after the addition is completed. After the reaction is completed, the reaction solution is concentrated by vacuum distillation until the volume is reduced by half, and then 100 mL of anhydrous dichloromethane is added to the reaction solution, and the solid is filtered and washed three times with 20 mL of anhydrous dichloromethane. After drying, the target ternary fluorophosphoryl imide organic lithium salt compound (I) is obtained in the form of a white powder with a yield of 82.7%. TOF-SIMS (m / z): calcd.for C7H 16 F3N3O6P3Li3[M+1] + ,409.07,found409.11.

[0064] (2) Prepare the electrolyte 1 sample, the specific steps are as follows:

[0065] In an argon glove box with a water and oxygen content of ≤0.1ppm, ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC) are uniformly mixed in a volume ratio of 10:10:40:40 to obtain an organic solvent, and then lithium hexafluorophosphate (LiPF6) is slowly added to the organic solvent. After complete dissolution, fluoroethylene carbonate (FEC), 1,3-propane sultone (PS), vinyl sulfate (DTD) and compound (I) are added, and the electrolyte 1 is obtained after stirring. The amount of LiPF6, organic solvent, FEC, PS, DTD and compound (I) used is 11%, 84%, 2%, 1%, 1% and 1% of the total mass of the electrolyte, respectively.

[0066] (3) Prepare the experimental battery 1 sample, the specific steps are as follows:

[0067] Preparation of positive electrode sheet: The positive electrode material 8 series nickel cobalt manganese oxide (NCM811), conductive agent carbon black (SuperP) and carbon nanotubes (CNT, 5% by mass NMP solution) binder polyvinylidene fluoride (PVDF, 5% by mass NMP solution) are weighed and mixed in a mass ratio of 97:0.7:0.8:1.5. After mixing, an appropriate amount of NMP is added to control the theoretical solid content to 65%. The positive electrode slurry is homogenized using a planetary homogenizer, and the positive electrode slurry is evenly coated on an aluminum foil with a thickness of 13 μm. After drying, rolling and cutting, a 50 mm × 70 mm positive electrode sheet is obtained.

[0068] Preparation of diaphragm: A polyethylene diaphragm coated with aluminum oxide on one side was used as the isolation membrane and was placed in a dry room with a dew point of -35°C for 72 hours before use.

[0069] Preparation of negative electrode sheet: artificial graphite (capacity 355 mAh g -1 ), conductive agent SuperP, thickener sodium carboxymethyl cellulose (CMC, deionized water solution with a solid content of 1.5%), binder styrene butadiene rubber (SBR, deionized water solution with a solid content of 48%) are mixed at a mass ratio of 95:1:1.5:2.5, and deionized water is added after mixing. The theoretical solid content is controlled to be 52%, and the negative electrode slurry is obtained by homogenization using a planetary homogenizer, and the negative electrode slurry is evenly coated on a copper foil with a thickness of 17μm. After drying, rolling, and cutting, a 52mm×72mm negative electrode sheet is obtained. The N / P ratio of the positive and negative electrodes is 1.1.

[0070] Preparation of battery: The battery was made in a dry room with an ambient dew point of ≤-35°C, the separator was folded in a Z shape, the positive electrode sheet and the negative electrode sheet were placed on each side, there were 12 layers of positive electrode sheets and 13 layers of negative electrode sheets, the positive electrode, separator and negative electrode were aligned and stacked in order to obtain an electrode group, and then the electrode group was fixed with polyimide tape and the ear was welded, and then placed in an aluminum-plastic film, and then vacuum-baked at 90°C for 12 hours, and after cooling, the above-prepared electrolyte 1 was injected, and finally after vacuum packaging, high-temperature infiltration, formation, aging, secondary sealing and capacity division, an experimental battery 1 with a capacity of about 2.5Ah was obtained.

[0071] Example 2

[0072] The specific steps for preparing compound (II) are as follows:

[0073]

[0074] Under nitrogen atmosphere, add anhydrous THF (300 mL) to a clean and dry 1000 mL three-necked flask equipped with a magnetic rotor, then place the flask in an ice-water bath, start stirring, and add 2-(aminomethyl)-2-methyl-1,3-propanediamine (4.69 g, 40.00 mmol) after THF drops to 0°C, and then slowly add 200 mL of anhydrous THF solution containing (2-n-propyl) fluorochlorophosphate (20.87 g, 130.00 mmol) pre-chilled to 0°C using a constant pressure dropping funnel. After the addition is complete, remove the ice-water bath and stir the resulting mixture at room temperature for 12 h. The residue is purified by flash silica gel chromatography on a short pad, the eluent is a mixture of n-hexane / dichloromethane (volume ratio 1:1), the solvent is removed by rotary evaporation, and anhydrous magnesium sulfate is used to dry to obtain a ternary fluorophosphorimide intermediate with a yield of 91.8%. TOF-SIMS(m / z):calcd.for C 14 H 33 F3N3O6P3[M+1] + ,489.15,found489.18.

[0075] Under nitrogen atmosphere, add 150 mL of anhydrous ethanol and 150 mL of ethyl acetate to a clean and dry 500 mL three-necked flask equipped with a magnetic rotor, and then start stirring. Then place the flask in a low-temperature reactor, and after cooling to about 0°C, add the intermediate (24.46 g, 50.00 mmol) and lithium carbonate (11.84 g, 160.00 mmol) prepared in the previous step to the solution, and react for 12 hours after the addition is completed. After the reaction is completed, the reaction solution is concentrated by vacuum distillation until the volume is reduced by half, and then 100 mL of anhydrous dichloromethane is added to the reaction solution, and the solid is filtered and washed three times with 20 mL of anhydrous dichloromethane. After drying, the target ternary fluorophosphoryl imide organic lithium salt compound (II) is obtained in a white powdery form, with a yield of 83.1%. TOF-SIMS (m / z): calcd.for C 14 H 30 F3N3O6P3Li3[M+1] + ,507.18,found507.20.

[0076] Electrolyte 2 and experimental battery 2 were prepared according to the method of Example 1, except that the additives added to electrolyte 2 were FEC, PS, ethylene carbonate (VC) and compound (II), wherein the usage amounts of LiPF6, organic solvent, FEC, PS, VC and compound (II) were 12%, 83.5%, 2%, 1%, 0.5% and 1% of the total mass of the electrolyte, respectively.

[0077] Example 3

[0078] The specific steps for preparing compound (III) are as follows:

[0079]

[0080] Under nitrogen atmosphere, anhydrous THF (300 mL) was added to a clean and dry 1000 mL three-necked flask equipped with a magnetic rotor, and then the flask was placed in an ice-water bath, stirring was started, and after THF dropped to 0°C, butyl triamine (4.12 g, 40.00 mmol) was added, and then a constant pressure dropping funnel was used to slowly add 200 mL of anhydrous THF solution pre-frozen to 0°C containing difluorochlorophosphorus (15.59 g, 130.00 mmol). After the addition was completed, the ice-water bath was removed and the resulting mixture was stirred at room temperature for 12 h. The residue was purified by flash silica gel chromatography on a short pad, the eluent was a mixture of n-hexane / dichloromethane (volume ratio 1:1), the solvent was removed by rotary evaporation, and anhydrous magnesium sulfate was used to dry to obtain a ternary fluorophosphorimide intermediate with a yield of 89.7%. TOF-SIMS (m / z): calcd.for C4H 10 F6N3O3P3[M+1] +,354.98,found355.02.

[0081] Under nitrogen atmosphere, add 150 mL of anhydrous ethanol and 150 mL of ethyl acetate to a clean and dry 500 mL three-necked flask equipped with a magnetic rotor, and then start stirring. Then place the flask in a low-temperature reactor, and after cooling to about 0°C, add the intermediate (17.75 g, 50.00 mmol) and lithium carbonate (11.84 g, 160.00 mmol) prepared in the previous step to the solution, and react for 12 hours after the addition is completed. After the reaction is completed, the reaction solution is concentrated by vacuum distillation until the volume is reduced by half, and then 100 mL of anhydrous dichloromethane is added to the reaction solution, and the solid is filtered and washed three times with 20 mL of anhydrous dichloromethane. After drying, the target ternary fluorophosphoryl imide organic lithium salt compound (III) is obtained in the form of a white powder with a yield of 82.7%. TOF-SIMS (m / z): calcd.for C4H7F6N3O6P3Li3[M+1] + ,373.01,found373.05.

[0082] Electrolyte 3 and experimental battery 3 were prepared according to the method of Example 1, except that the additives added to electrolyte 3 were FEC, PS, 1,3,6-hexanetricarbonitrile (HTCN) and compound (III), wherein the usage amounts of LiPF6, organic solvent, FEC, PS, HTCN and compound (III) were 12%, 83.5%, 2%, 1%, 0.5% and 1% of the total mass of the electrolyte, respectively.

[0083] Example 4

[0084] The specific steps for preparing compound (IV) are as follows:

[0085]

[0086] Under nitrogen atmosphere, anhydrous THF (300 mL) was added to a clean and dry 1000 mL three-necked flask equipped with a magnetic rotor, and then the flask was placed in an ice-water bath, stirring was turned on, and after THF dropped to 0°C, butyltriamine (4.12 g, 40.00 mmol) was added, and then a constant pressure dropping funnel was used to slowly add 200 mL of anhydrous THF solution pre-frozen to 0°C containing (2-propenyl) fluorochlorophosphate (20.60 g, 130.00 mmol). After the addition was completed, the ice-water bath was removed and the resulting mixture was stirred at room temperature for 12 h. The residue was purified by a short pad of rapid silica gel chromatography, the eluent was a mixture of n-hexane / dichloromethane (volume ratio 1:1), the solvent was removed by rotary evaporation, and anhydrous magnesium sulfate was used to dry to obtain a ternary fluorophosphorimide intermediate with a yield of 90.4%. TOF-SIMS (m / z): calcd.for C 13 H25 F3N3O6P3[M+1] + ,469.09,found 469.12.

[0087] Under nitrogen atmosphere, add 150 mL of anhydrous ethanol and 150 mL of ethyl acetate to a clean and dry 500 mL three-necked flask equipped with a magnetic rotor, and then start stirring. Then place the flask in a low-temperature reactor, and after cooling to about 0°C, add the intermediate (23.45 g, 50.00 mmol) and lithium carbonate (11.84 g, 160.00 mmol) prepared in the previous step to the solution, and react for 12 hours after the addition is completed. After the reaction is completed, the reaction solution is concentrated by vacuum distillation until the volume is reduced by half, and then 100 mL of anhydrous dichloromethane is added to the reaction solution, and the solid is filtered and washed three times with 20 mL of anhydrous dichloromethane. After drying, the target ternary fluorophosphoryl imide organic lithium salt compound (IV) is obtained in a white powdery form, with a yield of 81.8%. TOF-SIMS (m / z): calcd.for C 13 H 22 F3N3O6P3Li3[M+1] + ,487.12,found487.14.

[0088] Electrolyte 4 and experimental battery 4 were prepared according to the method of Example 1, except that the additives added to electrolyte 4 were FEC, DTD, propargyl phosphate (TPP) and compound (IV), wherein the usage amounts of LiPF6, organic solvent, FEC, DTD, TPP and compound (IV) were 12%, 83.8%, 2%, 1%, 0.2% and 1% of the total mass of the electrolyte, respectively.

[0089] Example 5

[0090] The specific steps for preparing compound (V) are as follows:

[0091]

[0092] Under nitrogen atmosphere, add anhydrous THF (300 mL) to a clean and dry 1000 mL three-necked flask equipped with a magnetic rotor, then place the flask in an ice-water bath, start stirring, and add 2-(aminomethyl)-2-methyl-1,3-propanediamine (4.69 g, 40.00 mmol) after THF drops to 0°C, and then slowly add 200 mL of anhydrous THF solution containing (1,1,2-trifluoroethyl) fluorochlorophosphate (26.06 g, 130.00 mmol) pre-chilled to 0°C using a constant pressure dropping funnel. After the addition is complete, remove the ice-water bath and stir the resulting mixture at room temperature for 12 h. The residue is purified by flash silica gel chromatography on a short pad, the eluent is a mixture of n-hexane / dichloromethane (volume ratio 1:1), the solvent is removed by rotary evaporation, and anhydrous magnesium sulfate is used to dry to obtain a ternary fluorophosphoryl imide intermediate with a yield of 88.4%. TOF-SIMS(m / z):calcd.for C 11 H 18 F 12 N3O6P3[M+1] + ,609.02,found 609.03.

[0093] Under nitrogen atmosphere, add 150 mL of anhydrous ethanol and 150 mL of ethyl acetate to a clean and dry 500 mL three-necked flask equipped with a magnetic rotor, and then start stirring. Then place the flask in a low-temperature reactor, and after cooling to about 0°C, add the intermediate (30.45 g, 50.00 mmol) and lithium carbonate (11.84 g, 160.00 mmol) prepared in the previous step to the solution, and react for 12 hours after the addition is completed. After the reaction is completed, the reaction solution is concentrated by vacuum distillation until the volume is reduced by half, and then 100 mL of anhydrous dichloromethane is added to the reaction solution, the solid is filtered, and then washed with 20 mL of anhydrous dichloromethane. After drying, the target ternary fluorophosphoryl imide organic lithium salt compound (V) is obtained in the form of a white powder with a yield of 80.2%. TOF-SIMS (m / z): calcd.for C 11 H 15 F 12 N3O6P3Li3[M+1] + ,627.05,found 627.09.

[0094] Electrolyte 5 and experimental battery 5 were prepared according to the method of Example 1, except that the additives added to electrolyte 5 were FEC, tris(trimethylsilyl)phosphate (TMSP) and compound (V), wherein the usage amounts of LiPF6, organic solvent, FEC, TMSP and compound (V) were 13%, 83.5%, 2%, 0.5% and 1% of the total mass of the electrolyte, respectively.

[0095] Example 6

[0096] The specific steps for preparing compound (VI) are as follows:

[0097]

[0098] Under nitrogen atmosphere, anhydrous THF (300 mL) was added to a clean and dry 1000 mL three-necked flask equipped with a magnetic rotor, and then the flask was placed in an ice-water bath and stirred. After THF dropped to 0°C, 4.12 g, 40.00 mmol, was added, and then a constant pressure dropping funnel was used to slowly add 200 mL of anhydrous THF solution pre-frozen to 0°C containing (2,2,2-trifluoroethyl) fluorochlorophosphate (26.06 g, 130.00 mmol). After the addition was completed, the ice-water bath was removed and the resulting mixture was stirred at room temperature for 12 h. The residue was purified by a short pad of flash silica gel chromatography, the eluent was a mixture of n-hexane / dichloromethane (volume ratio 1:1), the solvent was removed by rotary evaporation, and anhydrous magnesium sulfate was used to dry to obtain a ternary fluorophosphorimide intermediate with a yield of 87.2%. TOF-SIMS (m / z): calcd.for C 10 H 16 F 12 N3O6P3[M+1] + ,595.01,found 595.04.

[0099] Under nitrogen atmosphere, add 150 mL of anhydrous ethanol and 150 mL of ethyl acetate to a clean and dry 500 mL three-necked flask equipped with a magnetic rotor, and then start stirring. Then place the flask in a low-temperature reactor, and after cooling to about 0°C, add the intermediate (29.75 g, 50.00 mmol) and lithium carbonate (11.84 g, 160.00 mmol) prepared in the previous step to the solution, and react for 12 hours after the addition is completed. After the reaction is completed, the reaction solution is concentrated by vacuum distillation until the volume is reduced by half, and then 100 mL of anhydrous dichloromethane is added to the reaction solution, the solid is filtered, and then washed with 20 mL of anhydrous dichloromethane. After drying, the target ternary fluorophosphoryl imide organic lithium salt compound (VI) is obtained in the form of a white powder with a yield of 78.7%. TOF-SIMS (m / z): calcd.for C7H 16 F3N3O6P3Li3[M+1] + ,613.03,found 613.06.

[0100] Electrolyte 6 and experimental battery 6 were prepared according to the method of Example 1, except that the lithium salt added to electrolyte 6 was lithium tetrafluoroborate (LiBF4) and compound (VI), the organic solvent was propylene carbonate (PC), diethyl carbonate (DEC), propyl propionate (PP), di(2,2,2-trifluoroethyl) carbonate (TFEC), the volume ratio was 25:30:35:10, and the additives were FEC, tri(2,2,2-trifluoroethyl) phosphite (TEFP) and compound (VI), wherein the usage amounts of LiBF4, organic solvent, FEC, TEFP and compound (VI) were 11%, 84.5%, 3%, 0.5% and 1% of the total mass of the electrolyte, respectively.

[0101] Example 7

[0102] The specific steps for preparing compound (VII) are as follows:

[0103]

[0104] Under nitrogen atmosphere, anhydrous THF (300 mL) was added to a clean and dry 1000 mL three-necked flask equipped with a magnetic rotor, and then the flask was placed in an ice-water bath, stirring was turned on, and after THF dropped to 0°C, butyl triamine (4.12 g, 40.00 mmol) was added, and then a constant pressure dropping funnel was used to slowly add 200 mL of anhydrous THF solution pre-frozen to 0°C containing (perfluoroethyl) fluorochlorophosphate (30.74 g, 130.00 mmol). After the addition was completed, the ice-water bath was removed and the resulting mixture was stirred at room temperature for 12 h. The residue was purified by a short pad of rapid silica gel chromatography, the eluent was a mixture of n-hexane / dichloromethane (volume ratio 1:1), the solvent was removed by rotary evaporation, and anhydrous magnesium sulfate was used to dry to obtain a ternary fluorophosphorimide intermediate with a yield of 85.5%. TOF-SIMS (m / z): calcd.for C 10 H 10 F 18 N3O6P3[M+1] + ,702.95,found 702.99.

[0105] Under nitrogen atmosphere, add 150 mL of anhydrous ethanol and 150 mL of ethyl acetate to a clean and dry 500 mL three-necked flask equipped with a magnetic rotor, and then start stirring. Then place the flask in a low-temperature reactor, and after cooling to about 0°C, add the intermediate (20 g, 50.00 mmol) and lithium carbonate (11.84 g, 160.00 mmol) prepared in the previous step to the solution, and react for 12 hours after the addition is completed. After the reaction is completed, the reaction solution is concentrated by vacuum distillation until the volume is reduced by half, and then 100 mL of anhydrous dichloromethane is added to the reaction solution, the solid is filtered, and then washed with 20 mL of anhydrous dichloromethane. After drying, the target ternary fluorophosphoryl imide organic lithium salt compound (VII) is obtained in the form of a white powder with a yield of 75.9%. TOF-SIMS (m / z): calcd.for C 10 H7F 18 N3O6P3Li3[M+1] + ,720.97 found 720.99.

[0106] Electrolyte 7 and experimental battery 7 were prepared according to the method of Example 1, except that the lithium salts added to electrolyte 7 were LiPF6 and lithium perchlorate (LiClO4), the organic solvents were propylene carbonate (PC), ethyl methyl carbonate (EMC), and methyl trifluoroethyl carbonate (FEMC), and the volume ratio was 30:60:10, and the additives were FEC, PS, tris(trimethylsilyl)borate (TMSB) and compound (VII), wherein the usage amounts of LiPF6, LiClO4, organic solvent, FEC, PS, TMSB and compound (VII) were 8%, 8%, 78.7%, 2%, 2%, 0.3% and 1% of the total mass of the electrolyte, respectively.

[0107] Example 8

[0108] Electrolyte 8 and experimental battery 8 were prepared according to the method of Example 1, except that the lithium salts added to electrolyte 8 were LiPF6 and LiFSI, the organic solvents were propylene carbonate (PC), ethyl methyl carbonate (EMC), 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether (F-EAE), the volume ratio was 30:50:20, and the additives were FEC, 1,3,5-triallyl isocyanurate (TAIC) and compound (III), wherein the usage amounts of LiPF6, LiFSI, organic solvent, FEC, TAIC and compound (III) were 10%, 5%, 83.4%, 1%, 0.5% and 0.1% of the total mass of the electrolyte, respectively.

[0109] Example 9

[0110] Electrolyte 9 and experimental battery 9 were prepared according to the method of Example 1, except that the lithium salt added to electrolyte 9 was lithium bis(oxalatoborate) (LiBOB) and lithium difluorooxalatoborate (LiODFB), and the additives were FEC, PS and compound (III), wherein the usage amounts of LiBOB, LiODFB, organic solvent, FEC, PS and compound (III) were 5%, 8%, 83%, 1%, 1% and 2% of the total mass of the electrolyte, respectively.

[0111] Example 10

[0112] The electrolyte 10 and the experimental battery 10 are prepared according to the method of Example 1, except that the additives added to the electrolyte 10 are FEC and compound (III), wherein the usage amounts of LiPF6, organic solvent, FEC and compound (III) are 13%, 84%, 2% and 1% of the total mass of the electrolyte, respectively.

[0113] Comparative Example 1

[0114] The electrolyte 11 and the experimental battery 11 are prepared according to the method of Example 1, except that the additives added to the electrolyte 11 are FEC and LiTFSI, wherein the usage amounts of LiPF6, organic solvent, FEC and LiTFSI are 13%, 84%, 2% and 1% of the total mass of the electrolyte respectively.

[0115] Comparative Example 2

[0116] The electrolyte 12 and the experimental battery 12 are prepared according to the method of Example 1, except that the additives added to the electrolyte 12 are FEC and LiFSI, wherein the usage amounts of LiPF6, organic solvent, FEC and LiFSI are 13%, 84%, 2% and 1% of the total mass of the electrolyte, respectively.

[0117] The electrolyte compositions and contents of Examples 1 to 10 and Comparative Examples 1 to 2 are shown in Table 1.

[0118] Table 1 Electrolyte compositions of various embodiments and comparative examples

[0119]

[0120]

[0121]

[0122] The lithium ion batteries prepared in Examples 1 to 10 and Comparative Examples 1 to 2 were subjected to room temperature cycle performance test, low temperature cycle performance test and rate cycle performance test, respectively, and the test conditions are as follows:

[0123] Battery cycle test at room temperature:

[0124] The prepared lithium-ion battery was placed in a constant temperature room at an ambient temperature of 25°C, with a current of 1C and a voltage of 4.2V, and constant current and constant voltage charging to a cut-off current of 0.05C, and then discharged at a constant current of 1C to a voltage of 3V, and cycled for 1000 cycles, and the capacity retention rate was recorded. Single battery: nth cycle capacity retention rate (%) = (nth cycle discharge capacity / first cycle discharge capacity) × 100%, 5 samples were tested for each example, and the average value was taken.

[0125] Battery rate cycle test:

[0126] The prepared lithium-ion battery was placed in a constant temperature room at an ambient temperature of 25°C, and charged to 4.2V at a constant current of 3C, then charged at a constant voltage of 4.2V to a cut-off current of 0.05C, and then discharged at a constant current of 1C to a voltage of 3V, and cycled for 1000 cycles, and the capacity retention rate was recorded. Single battery: nth cycle capacity retention rate (%) = (nth cycle discharge capacity / first cycle discharge capacity) × 100%, 5 samples were tested for each example, and the average value was taken.

[0127] DC resistance (DCR) test:

[0128] The prepared lithium-ion battery was initially charged to 100% SOC, then discharged at a constant current of 1C for 30 minutes, and the SOC was adjusted to 50%. After being left for 2 hours, the voltage value V0 was recorded, and then the constant current was discharged at a current of 3C (the actual value was recorded as I0) for 10 seconds, and the voltage value V1 was recorded. DCR = (V0-V1) / I0, recorded as R0. The battery after 1000 cycles was tested with the same operation to obtain R1. DCR growth rate = (R1-R0) × 100% / R0. Five samples were tested in each example and the average value was taken.

[0129] The battery performance test results of the lithium ion batteries prepared in Examples 1 to 10 and Comparative Examples 1 to 2 are shown in Table 2:

[0130] Table 2 Statistical table of electrical properties of batteries in various embodiments and comparative examples

[0131]

[0132]

[0133] It can be seen from the performance test data of lithium ion batteries corresponding to Examples 1 to 10 and Comparative Examples 1 to 2 that after using the ternary fluorine-containing organic lithium salt additive provided by the present invention, the lithium ion battery exhibits a higher cycle life and better rate performance. This is due to the use of the ternary fluorine phosphorimide organic lithium salt provided by the present invention as a lithium salt additive, which can effectively increase the number of lithium ion migrations and enhance the ability of lithium ion rapid deintercalation. At the same time, the rich fluorine-containing groups contained in the structure enhance the electrochemical reduction decomposition of the overall molecule, so that the in-situ construction of a LiF-rich SEI passivation layer can be preferentially decomposed on the negative electrode surface. In addition, the P=O contained in the structure is easily oxidized on the highly active positive electrode surface, so the remaining F ions are easily combined with lithium ions to participate in film formation, thereby improving the problem of poor ion conductivity of the oxidation film product on the positive electrode surface, and forming a CEI film with low interface impedance. And because the radius of the F ions and lithium ions is close, the binding energy is very strong, and they can be well covered on the surface of the positive electrode material, which can effectively alleviate the erosion of the positive electrode by hydrofluoric acid, thereby reducing the loss of active lithium, and effectively improving the electrochemical performance of the lithium battery. At the same time, the change of the internal DC impedance before and after the battery cycle is intuitively shown through DCR monitoring. The results show that the growth of the DC internal resistance of the lithium ion batteries of Examples 1 to 10 is significantly suppressed compared with that of the lithium ion batteries of Comparative Examples 1 to 2. On the one hand, this is because the ternary fluorine-containing organic lithium salt additive provided by the present invention induces the generation of more fluorine-containing phases at the positive and negative electrode interfaces, respectively, so that the interface film has a higher ionic conductivity; on the other hand, the generated interface protection film is more solid and stable, and is not easy to break during the cycle. The interface film will not proliferate to cause an increase in impedance, and thus exhibits a lower internal resistance growth rate.

[0134] In summary, the above description of the disclosed embodiments enables professionals and technicians in the field to implement or use the present invention. Various modifications to these embodiments will be apparent to professionals and technicians in the field, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but will conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A ternary fluorine-containing organic lithium salt additive, characterized in that: It has the structure shown in structural formula A: Among them, M is Li, R1 is a fluorine atom or an oxygen atom, R2 is a vacancy, a methyl group, a n-propyl group, a propenyl group, a 1,2,2-trifluoroethane group, a 1,1,1-trifluoroethane group or a perfluoroethane group, and R3 is a hydrogen atom or a methyl group.

2. The ternary fluorine-containing organic lithium salt additive according to claim 1, characterized in that: The structural formula A is specifically any one of the following formulas (I) to (VII):

3. The ternary fluorine-containing organic lithium salt additive according to claim 1, characterized in that: The preparation method of the ternary fluorine-containing organic lithium salt additive comprises the following steps: Firstly, a fluorine-containing chlorophosphoric acid monomer and a triamino monomer undergo a nucleophilic substitution reaction to prepare a ternary fluorophosphoryl imide compound, and then a substitution reaction is carried out with a lithium source to obtain a ternary fluorine-containing organic lithium salt additive.

4. An electrolyte comprising a lithium salt, a non-aqueous organic solvent and an electrolyte additive, characterized in that: The electrolyte additive comprises the ternary fluorine-containing organic lithium salt additive according to any one of claims 1 to 3.

5. The electrolyte according to claim 4, characterized in that The lithium salt is selected from one or more of lithium hexafluorophosphate, lithium perchlorate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, and lithium difluorobis(oxalatophosphate); The lithium salt accounts for 11% to 16% of the weight of the electrolyte.

6. The electrolyte according to claim 4, characterized in that The non-aqueous organic solvent is an organic ester solvent and / or an ether solvent; the organic ester solvent is one or more of ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl trifluoroethyl carbonate, di(2,2,2-trifluoroethyl) carbonate, ethyl formate, ethyl acetate, propyl acetate, and propyl propionate; the ether solvent is one or more of dimethyl ether, diethyl ether, methyl ethyl ether, ethylene glycol dimethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, and 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether; The non-aqueous organic solvent accounts for 78.7% to 84.5% of the weight of the electrolyte.

7. The electrolyte according to claim 4, characterized in that The electrolyte additives are the ternary fluorine-containing organic lithium salt additive and auxiliary additives; The ternary fluorine-containing organic lithium salt additive accounts for 0.1% to 2% of the weight of the electrolyte.

8. The electrolyte according to claim 7, characterized in that The auxiliary additive is selected from vinylene carbonate, ethylene carbonate, fluoroethylene carbonate, difluoroethylene carbonate, vinyl sulfate, diethylene sulfate, propylene sulfate, 1,3-propane sultone, 1,3-propylene sultone, 1,4-butane sultone, 2,4-butane sultone, phenyl methanesulfonate, methylene disulfonate, N-phenyl bis(trifluoromethanesulfonyl)imide, triallyl phosphate, tris(trimethylsilyl)phosphate, trimethyl phosphite, triphenyl phosphite one or more of ester, tris(2,2,2-trifluoroethyl)phosphite, tetramethylmethylene diphosphate, propargyl phosphate, (2-allylphenoxy)trimethylsilane, tris(trimethylsilyl)borate, 1,3,5-triallyl isocyanurate, isocyanoethyl methacrylate, hexamethylene diisocyanate, p-phenylene diisocyanate, 2,4-toluene diisocyanate, adiponitrile, succinonitrile, glutaronitrile, 1,3,6-hexanetrinitrile, and 1,2-bis(cyanoethoxy)ethane; The auxiliary additive accounts for 2% to 4.3% of the weight of the electrolyte.

9. A lithium ion battery comprising: A positive electrode, a negative electrode, a separator and an electrolyte, wherein the electrolyte is the electrolyte according to any one of claims 4 to 8.

10. The lithium ion battery according to claim 9, characterized in that: The active material of the positive electrode is selected from lithium cobalt oxide, lithium manganese oxide, ternary nickel cobalt manganese lithium, lithium nickel manganese oxide, lithium iron phosphate or lithium manganese iron phosphate; The active material of the negative electrode is selected from artificial graphite, natural graphite, lithium titanate, metallic lithium, silicon-carbon composite material or silicon oxide; The diaphragm is selected from polypropylene, polyethylene diaphragm or polyethylene diaphragm coated with aluminum oxide on one side.