Energy storage cell and preparation method thereof

The ceramic diaphragm is prepared by high-speed airflow shear method and combined with thermal curing treatment, which solves the problem of insufficient mechanical strength of the electrode ears of lithium-ion batteries, improves the mechanical performance and safety of the battery cell, and avoids the risks of the electrode tears and welding.

CN118943500AActive Publication Date: 2024-11-12ZHEJIANG JINKO ENERGY STORAGE CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411217161.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The mechanical strength of existing lithium-ion batteries is insufficient, and tear is prone to occur, and there are problems of safety risks and poor pressure differential during welding.

Method used

The high-speed airflow shear method is used to mix the ceramic material with the adhesive to form a ceramic diaphragm, and the compaction density and mechanical properties of the positive electrode sheet are improved by thermal curing to avoid tearing the ears.

Benefits of technology

The mechanical strength of the electrode is improved, the tear of the electrode is avoided during welding, and the mechanical properties and safety of the battery cell are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943500A_ABST
    Figure CN118943500A_ABST
Patent Text Reader

Abstract

The embodiment of the invention relates to the field of energy storage, and provides an energy storage cell and a preparation method thereof, and the preparation method comprises the following steps: providing a current collector; a ceramic material and an adhesive are uniformly dispersed through high-speed airflow shearing to obtain mixed powder, the mass percent of the ceramic material is 80 wt%-98 wt%, and the mass percent of the adhesive is 2 wt%-20 wt%; rolling the mixed powder to obtain a ceramic diaphragm which is at least positioned at the tab part and the junction between the tab part and the active substance part; forming an active substance layer, wherein a first preset range is formed between the active substance layer and the ceramic diaphragm; carrying out thermocuring treatment, wherein a second preset range is formed between the active material layer subjected to thermocuring treatment and the ceramic diaphragm; the thermocuring treatment comprises the step of performing rolling treatment on the current collector containing the ceramic diaphragm and the active material layer at a preset temperature, so that the ceramic diaphragm is fixed on the current collector and the active material layer is fixed on the current collector.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present application relate to the field of energy storage, and in particular to an energy storage battery cell and a method for preparing the same. Background Art

[0002] In recent years, lithium-ion batteries have attracted great attention due to their excellent characteristics such as high energy density, high output voltage, low self-discharge rate, long service life, no memory effect and environmental friendliness. They have developed by leaps and bounds, their market share has continued to expand, and they have occupied a dominant position.

[0003] At present, single lithium batteries are mainly cylindrical, square and soft-pack. The methods adopted in the battery production process mainly include stacking and winding. The stacking method is generally die-cut and then cut and stacked, which has low production efficiency, low consistent precision, and low rate and cycle performance. The winding method has higher production efficiency. Generally, battery cells without die-cutting process adopt the post-process method of welding pole ears for drainage. In this process, the problem of pole ear alignment needs to be considered.

[0004] Among them, square batteries are mostly single-pole ear processes and multi-pole ear processes. The single-pole ear process is to connect the pole ear to the pole piece by ultrasonic welding before winding the pole piece, and then wind it into a battery through the welded pole ear drainage; the multi-pole ear process is to die-cut the pole piece. After die-cutting, it can be divided into two types: one is to stack the pieces after cutting, and the other is to directly wind. Both of them ultimately use the pole piece end as the pole ear for multi-pole ear super welding as the drainage terminal. Since the subsequent welding process requires the pole ear to be welded on the pole piece separately, and in this process, the pole ear is very easy to tear, and there is no effective full inspection and interception measures. After flowing out, it will cause safety risks to the battery cell and poor pressure difference between the battery cells in the module. Summary of the invention

[0005] The embodiments of the present application provide an energy storage battery cell and a method for preparing the same, which are at least beneficial to improving the mechanical strength of the tab.

[0006] According to some embodiments of the present application, on the one hand, the embodiments of the present application provide a method for preparing an energy storage battery cell, comprising: forming a diaphragm and a positive electrode sheet and a negative electrode sheet located on both sides of the diaphragm; the process steps for forming the positive electrode sheet include: providing a current collector, the current collector having two pole ear portions and an active material portion located between the two pole ear portions; forming a ceramic diaphragm, the ceramic diaphragm being located at least at the pole ear portion and the junction between the pole ear portion and the active material portion, and the process steps for forming the ceramic diaphragm include: uniformly dispersing a ceramic material and an adhesive by high-speed air flow shearing to obtain a mixed powder, wherein the mass percentage of the ceramic material is 80wt% to 98wt%, and the mass percentage of the adhesive is 2wt% to 20wt%; rolling the mixed powder to obtain the ceramic diaphragm; forming an active material layer, wherein the active material layer is located on the active material portion; wherein a first preset range is provided between the active material layer and the ceramic diaphragm; performing a heat curing treatment, wherein a second preset range is provided between the active material layer and the ceramic diaphragm after the heat curing treatment; the heat curing treatment comprises: performing a roller pressing treatment on the current collector including the ceramic diaphragm and the active material layer at a preset temperature so that the ceramic diaphragm is fixed to the current collector and the active material layer is fixed on the current collector; performing a die-cutting on the current collector corresponding to the pole ear portion according to preset parameters so that the pole ear portion of the current collector forms a pole ear; cutting the current collector to form two identical positive electrode sheets; and performing a winding treatment on the diaphragm, the positive electrode sheet and the negative electrode sheet.

[0007] In some embodiments, the second preset range is 0.5 mm to 1.5 mm.

[0008] In some embodiments, the adhesive is one or more of polytetrafluoroethylene, polyhexafluoropropylene or polyvinylidene fluoride.

[0009] In some embodiments, the adhesive is a polytetrafluoroethylene material, the mass percentage of the ceramic material is 85wt% to 95wt%, and the mass percentage of the polytetrafluoroethylene material is 5wt% to 15wt%.

[0010] In some embodiments, the process parameters for uniformly dispersing the ceramic material and the adhesive by high-speed airflow shearing to obtain a mixed powder include: a feed flow rate of 100L / h to 2000L / h, an air flow velocity of 10m / s to 500m / s, and a temperature of 20°C to 60°C.

[0011] In some embodiments, the preset temperature is 60-130°C.

[0012] In some embodiments, the process steps for forming the active material layer include: uniformly dispersing the conductive agent, the active material and the adhesive by high-speed air flow shearing to obtain a conductive powder, the mass percentage of the conductive agent is 1wt% to 2wt%, the mass percentage of the active material is 95wt% to 97wt%, and the mass percentage of the adhesive is 1wt% to 4wt%; and roller pressing the conductive powder to obtain the active material layer.

[0013] In some embodiments, the process steps of performing the thermal curing treatment and the die-cutting include: die-cutting the current collector corresponding to the pole ear portion according to preset parameters so that the end of the current collector forms a pole ear; the ceramic diaphragm is located at the pole ear and at the junction between the pole ear and the active material portion; and performing the thermal curing treatment on the current collector.

[0014] According to some embodiments of the present application, on the other hand, the embodiments of the present application further provide an energy storage battery cell, comprising: a diaphragm, and a positive electrode sheet and a negative electrode sheet located on both sides of the diaphragm, the positive electrode sheet is prepared by the preparation method of the energy storage battery cell described in any of the above embodiments; the positive electrode sheet comprises a current collector, a ceramic diaphragm and an active material layer, the current collector has a pole ear and an active material portion, the ceramic diaphragm is located at least on the pole ear and at the junction between the pole ear and the active material portion; the active material layer is located on the active material portion, and there is a second preset range between the active material layer and the ceramic diaphragm.

[0015] In some embodiments, the ceramic diaphragm is also located on part of the active material portion, the distance of the ceramic diaphragm located in the active material portion along the first direction is a third preset distance, and the ratio of the third preset distance to the second preset distance is 5-20.

[0016] The technical solution provided by the embodiments of the present application has at least the following advantages:

[0017] The preparation method of the energy storage battery provided in the embodiment of the present application is to mix the ceramic material and the adhesive uniformly by high-speed airflow shearing, rather than using NMP (N-methylpyrrolidone, N-Methyl pyrrolidone) solution to dissolve the adhesive and disperse the ceramic material, which can avoid the safety problem of NMP solvent volatilization. Compared with the preparation of ceramic diaphragms by NMP solution, the high-speed airflow shearing method can be regarded as preparing ceramic diaphragms by dry process. In this process, the adhesive forms friction between adhesive molecules through high-speed shearing force, thereby producing fibers, which can coat the ceramic material and form a network structure, so as to have good mechanical properties, thereby improving the mechanical properties of the pole ear and avoiding the pole ear tearing. Secondly, the positive electrode sheet is formed by thermal curing treatment, that is, the current collector containing the ceramic diaphragm and the active material layer is rolled at a preset temperature, which can effectively improve the compaction density of the ceramic and active material layers in the positive electrode sheet, and can also further improve the winding degree of various substances in the pole ear and the active material layer, and improve the mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] One or more embodiments are exemplarily illustrated by the figures in the corresponding drawings. These exemplified descriptions do not constitute a limitation on the embodiments. Unless otherwise specified, the figures in the drawings do not constitute a scale limitation. In order to more clearly illustrate the embodiments of the present application or the technical solutions in the traditional technology, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 A flowchart corresponding to a method for preparing an energy storage cell provided in an embodiment of the present application;

[0020] Figure 2 to Figure 10 A schematic structural diagram corresponding to each step of forming a positive electrode sheet in a method for preparing an energy storage cell provided in an embodiment of the present application;

[0021] Fig.11 A top view of an energy storage cell that is being wound in a method for preparing an energy storage cell provided in an embodiment of the present application. DETAILED DESCRIPTION

[0022] As can be seen from the background technology, the mechanical strength of the tabs of current energy storage cells is poor and they are easily torn.

[0023] The embodiment of the present application provides a method for preparing an energy storage battery cell, which utilizes high-speed airflow to shear and disperse ceramic materials and adhesives, so that the mechanical strength of the ceramic diaphragm finally formed is greater to avoid the problem of tearing of the tabs.

[0024] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.

[0025] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0026] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists, A and B exist at the same time, and B exists. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0027] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).

[0028] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.

[0029] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.

[0030] In the accompanying drawings corresponding to the embodiments of the present application, the thickness and area of ​​the layer are magnified for better understanding and ease of description. When describing a component (such as a layer, film, region or substrate) on another component or on the surface of another component, the component can be "directly" located on the surface of another component, or there can be a third component between the two components. On the contrary, when describing a component on the surface of another component or when another component is formed or provided on the surface of a component, it means that there is no third component between the two components. In addition, when describing a component as "substantially" formed on another component, it means that the component is not formed on the entire surface (or front surface) of the other component, nor is it formed on a partial edge of the entire surface.

[0031] In the description of the embodiments of the present application, when a component "includes" another component, unless otherwise specified, other components are not excluded, and other components may be further included. In addition, when a component such as a layer, film, region, or plate is referred to as being "on / located on" another component, it may be "directly on" the other component (i.e., located on the surface of the other component with no other components between them), or another component may exist in between. In addition, when a component such as a layer, film, region, or plate is "directly located on" another component, or when a component such as a layer, film, region, or plate is located on the surface of another component, it means that no other components are located in between.

[0032] The terms used in the description of the various embodiments described herein are only used to describe specific embodiments and are not intended to be limiting. As used in the description of the various embodiments described and in the appended claims, "the part" is also intended to include plural forms unless the context clearly indicates otherwise. Among them, components include layers, films, regions, or panels. Thereby improving the yield of the battery cell.

[0033] Figure 1 This is a flow chart corresponding to a method for preparing an energy storage cell provided in one embodiment of the present application.

[0034] According to some embodiments of the present application, the present application provides a method for preparing an energy storage battery cell. Figure 1 The preparation method includes: forming a separator; forming a positive electrode sheet; forming a negative electrode sheet; assembling the positive electrode sheet, the negative electrode sheet and the separator, wherein the positive electrode sheet and the negative electrode sheet are respectively located on both sides of the separator; and performing a winding process on them.

[0035] The process steps for forming a positive electrode sheet include: providing a current collector, the current collector having two pole ear portions and an active material portion located between the two pole ear portions. The process steps for forming a positive electrode sheet include: forming a ceramic diaphragm, the ceramic diaphragm is at least located at the pole ear portion and the junction between the pole ear portion and the active material portion, and the process steps for forming a ceramic diaphragm include: uniformly dispersing a ceramic material and an adhesive by high-speed airflow shearing to obtain a mixed powder, wherein the mass percentage of the ceramic material is 80wt% to 98wt%, and the mass percentage of the adhesive is 2wt% to 20wt%; rolling the mixed powder to obtain a ceramic diaphragm. The process steps for forming a positive electrode sheet include: forming an active material layer, the active material layer is located on the active material portion; wherein there is a first preset range between the active material layer and the ceramic diaphragm. The process steps for forming the positive electrode sheet include: performing a heat curing treatment, wherein the active material layer after the heat curing treatment has a second preset range with the ceramic diaphragm; the heat curing treatment includes: performing a roller pressing treatment on the current collector including the ceramic diaphragm and the active material layer at a preset temperature so that the ceramic diaphragm is fixed to the current collector and the active material layer is fixed on the current collector. The process steps for forming the positive electrode sheet include: performing a die-cutting on the current collector corresponding to the pole ear according to preset parameters so that the pole ear portion of the current collector forms a pole ear. The process steps for forming the positive electrode sheet include: cutting the current collector and forming two identical positive electrode sheets.

[0036] The preparation method of the energy storage battery provided in the embodiment of the present application is to mix the ceramic material and the adhesive evenly by high-speed airflow shearing, rather than using NMP solution to dissolve the adhesive and disperse the ceramic material, which can avoid the safety problem of NMP solvent volatilization. Compared with the preparation of ceramic diaphragms by NMP solution, the high-speed airflow shearing method can be regarded as preparing ceramic diaphragms by dry process. In this process, the adhesive forms friction between adhesive molecules through high-speed shearing force, thereby producing fibers, which can coat the ceramic material and form a network structure, so as to have good mechanical properties, thereby improving the mechanical properties of the pole ear and avoiding the pole ear tearing. Secondly, the positive electrode sheet is formed by thermal curing treatment, that is, the current collector containing the ceramic diaphragm and the active material layer is rolled at a preset temperature, which can effectively improve the compaction density of the ceramic and active material layers in the positive electrode sheet, and can also further improve the winding degree of various substances in the pole ear and the active material layer, and improve the mechanical properties.

[0037] According to the appearance classification, the prepared energy storage cells can be divided into square cells, round cells or soft-pack cells. According to the capacity classification, the energy storage cells can be divided into 50Ah, 100Ah, 150Ah, 200Ah, 280Ah, 306Ah, 314Ah, 500+Ah, 800+Ah and 1000+Ah and other models. According to the chemical composition and working principle of the cell, the energy storage cell can be a lithium-ion battery, a lead-acid battery, a sodium-ion battery or a nickel-metal hydride battery. The embodiment of the present application takes the preparation method of a lithium-ion battery as an example. Those skilled in the art can replace the lithium ions in the positive electrode sheet, the negative electrode sheet and the electrolyte with corresponding metal ions according to actual needs. For example, in sodium ion batteries, the lithium transition metal oxide of the positive electrode active material is replaced by any of the corresponding layered metal oxides (such as NaFeO2), polyanion compounds (NaFePO4) and Prussian blue compound systems (such as NaMnFe(CN)6-zH2O), and the electrolyte is replaced by any of the organic liquid electrolyte, solid composite electrolyte or solid electrolyte.

[0038] The following will describe the various embodiments of the present application in detail with reference to the accompanying drawings. However, it will be appreciated by those skilled in the art that in the various embodiments of the present application, many technical details are provided in order to enable the reader to better understand the present application. However, even without these technical details and various changes and modifications based on the following embodiments, the technical solution claimed in the present application can be implemented.

[0039] Figure 2 to Figure 10 This is a schematic structural diagram corresponding to each step of preparing a positive electrode sheet in a method for preparing an energy storage cell provided in an embodiment of the present application.

[0040] Figure 2 A top view corresponding to a current collector is provided in a method for preparing an energy storage cell provided in an embodiment of the present application; Figure 3 for Figure 2 Section view along section A1-A2.

[0041] refer to Figure 2 and Figure 3 The preparation method for forming a positive electrode sheet includes: providing a current collector 10 , wherein the current collector 10 has two pole ear portions 12 and an active material portion 11 located between the two pole ear portions 12 .

[0042] In some embodiments, the current collector 10 can be aluminum foil, which is cheaper than copper foil. A dense oxide film is formed on the surface of the aluminum foil, and the oxide film is very thin, which can improve the corrosion resistance of the aluminum foil, and electrons can achieve conductivity through the tunnel effect.

[0043] In some embodiments, the current collector 10 may also be a composite current collector, which includes three stacked layers, the middle layer is organic, and the upper and lower layers are copper-plated and aluminum-plated. The organic material is PET (polyethylene terephthalate), PP (polypropylene), PI (polyimide), etc.

[0044] In some embodiments, the current collector 10 may also be a carbon-based current collector, that is, a conductive carbon layer is provided on the aluminum foil, and the conductive carbon layer may serve as a protective layer to effectively protect the current collector to prevent corrosion of the metal current collector, thereby increasing the life of the current collector; secondly, the conductive carbon layer itself has a low resistivity, so as not to generate excessive electrical losses.

[0045] The conductive carbon layer can be made of flake graphite, spherical graphite, small-size active particles, carbon nanotubes, graphene, etc. 2 / g) compared to flake graphite (specific surface area of ​​16m 2 / g) provides a larger surface area for contacting with lithium ion particles in the subsequently formed active material layer 120, and the corresponding positive electrode exhibits more excellent cyclic voltammetric characteristics and has better dispersibility in the slurry. Using active particles or carbon nanotubes, graphene, etc. with small particle sizes or even nanometer sizes as the conductive carbon layer can significantly improve the energy density, rate performance, etc. of lithium ion batteries.

[0046] It should be noted that the carbon-based current collector may be expressed as the upper and lower surfaces of the aluminum foil are coated with a conductive carbon layer, or may be expressed as the surface of part of the aluminum foil is covered with a conductive carbon layer. Part of the surface of the aluminum foil covered with a conductive carbon layer may include the aluminum foil corresponding to the active material part 11 having a conductive carbon layer, the aluminum foil corresponding to part of the active material part 11 having a conductive carbon layer, the aluminum foil corresponding to the active material part 11 and the subsequent ceramic diaphragm having a conductive carbon layer, etc.

[0047] In addition, in other embodiments, for example, the current collector of the positive electrode sheet in a sodium ion battery may also be aluminum foil.

[0048] The active material portion 11 is a region for forming an active material layer. The active material particles in the active material layer are carriers for oxidation reaction in the battery cell.

[0049] The pole ear portion 12 is an area for forming a pole ear in the future. The pole ear is a metal conductor that leads the positive electrode of the energy storage battery cell out of the battery cell. The pole ear is the contact point between the positive electrode sheet and the external contact component when the battery cell is charged and discharged. The external contact component can be a pole.

[0050] In some embodiments, two pole ears can be formed at both ends of the current collector 10, and finally cut to form two identical positive electrode sheets, so that two pole ear portions 12 are defined at both ends of the current collector 10. In other embodiments, a current collector can be cut to form multiple positive electrode sheets, and the active material portion 11 and the pole ear portion can be arranged at intervals according to a certain size ratio, and the pole ear portion is subsequently die-cut to form the corresponding pole ear.

[0051] In some embodiments, the boundary line and size relationship between the pole ear portion 12 and the active material portion 11 are not limited in the embodiments of the present application, and those skilled in the art can set them according to specific needs. In one example, the length of the active material portion 11 can be 55 mm, and the length of the pole ear portion 12 can be 3 mm.

[0052] Figure 4 A top view corresponding to the formation of a ceramic diaphragm 110 in the method for preparing an energy storage cell provided in one embodiment of the present application; Figure 5 for Figure 4 Section view along section A1-A2.

[0053] refer to Figure 4 and Figure 5 The process steps of forming the positive electrode sheet include: forming a ceramic diaphragm 110 , and the ceramic diaphragm 110 is at least located at the pole ear portion 12 and the junction between the pole ear portion 12 and the active material portion 11 .

[0054] When the pole ear is welded, that is, the pole ear and the adapter are welded, the pole ear needs to be assisted in welding by making the welding surface perpendicular to the extension direction of the positive electrode sheet. During this process, the pole ear is deformed to a large extent and there is welding stress, which makes the pole ear prone to tearing. In the positive electrode sheet provided in the embodiment of the present application, a ceramic diaphragm 110 is formed. The ceramic diaphragm 110 is located at the pole ear portion 12 and at the junction of the pole ear portion 12 and the active material portion 11. The mechanical strength of the ceramic diaphragm 110 sheared by the high-speed airflow is high, which can enhance the mechanical strength of the pole ear and effectively avoid the problem of the pole ear tearing during the welding process.

[0055] The process steps for forming the ceramic diaphragm 110 include: uniformly dispersing the ceramic material and the adhesive by high-speed airflow shearing to obtain a mixed powder. In this way, the adhesive is fiberized based on the shearing force of the high-speed airflow, and the fibrous adhesive is dispersed in the entire system, and a three-dimensional network structure is formed based on the adhesion between the adhesive and the adhesive. The three-dimensional network structure can not only construct pores, but also enhance the mechanical properties. Ceramic materials can fill the pores to prevent ceramic materials from agglomerating with each other and affecting the final insulation effect. The three-dimensional network structure enhances the mechanical properties, and the ceramic diaphragm 110 located at the junction of the ear portion 12 and the active material portion 11 subsequently has a higher mechanical strength, thereby avoiding the problem of the ear tearing during the welding process.

[0056] Secondly, high-speed airflow shearing disperses the ceramic material, and utilizes high-speed airflow to promote the collision between ceramic material particles. The shearing effect of the airflow impacting the ceramic material and the impact and shearing of the ceramic material and other components promote the crushing of the ceramic material, thereby causing the ceramic material to be broken from large particles to small particles, and from large particle sizes to small particle sizes. The final ceramic crushed product has a smaller average particle size, a narrower particle size distribution, and a smooth and regular particle surface, thereby increasing the compaction density of the final ceramic diaphragm 110.

[0057] The ceramic material and the adhesive are sheared by high-speed airflow, that is, the ceramic diaphragm 110 is formed by a dry process, which is also called a solvent-free process (Solvent-Free, SF). The dry process can not only reduce the solvent drying step, but also reduce the preparation cost, improve production efficiency and reduce environmental pollution. The dry process can also reduce the thickness of the ceramic diaphragm 110, thereby reducing the thickness of the electrode layer of the positive electrode sheet in the battery cell, thereby improving the energy density of the battery.

[0058] Before the high-speed airflow shearing treatment, the process also includes: pre-treating the ceramic material and the adhesive until there is no obvious agglomerate in the mixed species. The pre-treatment is slow stirring first, followed by high-temperature aging. The linear speed of slow stirring is less than 5m / s. The aging temperature of high-temperature aging is 40℃~50℃, and the aging time is 48h~96h. After slow stirring, high-temperature aging can make the ceramic material and the adhesive undergo the process of opening and stretching the polymer molecular chain, avoiding the adverse effects such as molecular chain interruption and functional group destruction caused by the high-speed shearing process.

[0059] It should be noted that the main principle of high-speed airflow shearing treatment is to suck the material into the airflow through a high-speed rotating centrifuge, and under the action of high-pressure gas, it is accelerated, sheared, ground and processed.

[0060] In some embodiments, the process parameters for uniformly dispersing the ceramic material and the binder by high-speed airflow shearing to obtain a mixed powder include: feed flow rate, airflow velocity and temperature, among which the feed flow rate is ≤2000L / h, the airflow velocity is ≤500m / s, and the temperature is 20°C to 60°C. The mixture composed of the ceramic material and the binder is absorbed in a device, and the feed flow rate of the inert gas is controlled to be ≤2000L / h and the airflow velocity is ≤500m / s, the turbine speed is 300rpm / min to 650rpm / min, the airflow crushing time is 3min to 15min, and the reaction temperature is 20°C to 60°C to form a mixed powder.

[0061] In some embodiments, the feed flow rate can be controlled to be 100 L / h to 2000 L / h, the air flow velocity can be controlled to be 10 m / s to 500 m / s, and the temperature can be controlled to be 20° C. to 60° C.

[0062] In some embodiments, the feed flow rate can be controlled to be 500 L / h to 2000 L / h, and the air flow velocity can be controlled to be 100 m / s to 500 m / s.

[0063] The mass percentage of the ceramic material is 80wt% to 98wt%, and the mass percentage of the adhesive is 2wt% to 20wt%. The mass percentage of the adhesive and the ceramic material can make the structure of the final ceramic diaphragm relatively stable, and the ceramic material will not detach during the battery charging and discharging cycle. When the content of the adhesive is lower than 2wt%, the bonding and contact tightness of the components cannot be guaranteed; when the content of the adhesive is higher than 20wt%, the content of the ceramic material will be reduced, and the ceramic material, which mainly acts as an insulator, may not be able to form a sufficient thickness and cover the pole ear, thereby causing a short circuit problem between the positive electrode and the negative electrode.

[0064] In some embodiments, the adhesive is one or more of polytetrafluoroethylene (PTFE), polyhexafluoropropylene (PHTP), or polyvinylidenefluoride (PVDF). Fluorinated ethylene adhesives have excellent adhesion, insulation, and mechanical strength. The bond energy of carbon-fluorine bonds is large, which can prevent the functional group decomposition of the adhesive during high-speed airflow shearing, or even failure.

[0065] In some embodiments, the adhesive is a polytetrafluoroethylene material, the mass percentage of the ceramic material is 85wt% to 95wt%, and the mass percentage of the polytetrafluoroethylene material is 5wt% to 15wt%. The polytetrafluoroethylene material has a low van der Waals force and is loosely stacked. Under the action of external shear force, it changes from agglomerates to fibrils, and the fibrils present a three-dimensional network structure and bond the ceramic material. The pores in the fibrillated three-dimensional network structure can accommodate the ceramic material, thereby preventing the ceramic material from falling off the current collector 10, and avoiding the phenomenon of rapid discharge or even burning caused by the short circuit between the positive and negative electrodes.

[0066] The ceramic material may be any one or more of oxides (such as boehmite, aluminum oxide, zirconium oxide), carbides (such as silicon carbide, boron carbide), and nitrides (such as silicon nitride).

[0067] The mixed powder is subjected to roller pressing to obtain a ceramic diaphragm 110. In this way, the ceramic diaphragm 110 can be compacted, the contact performance between the ceramic material and the fiberized adhesive in the ceramic diaphragm 110 can be improved, and the ceramic material can be prevented from falling off. The ceramic diaphragm 110 after roller pressing can be used as a self-supporting film, and the self-supporting film can have a certain strength so that it will not be damaged in subsequent process steps and battery cycle charging and discharging processes.

[0068] In some embodiments, the process parameters of the roller pressing process are roller speed ≤ 100 m / min; main roller pressure ≤ 300 t; roller gap 100 μm to 300 μm, and roller pressing time 10 min to 50 min. The speed and pressure of the roller pressing are controlled so that the mixed powder is rolled into a ceramic diaphragm within a certain period of time.

[0069] Figure 6 A top view corresponding to the formation of an active material layer 120 in the method for preparing an energy storage cell provided in one embodiment of the present application; Figure 7 for Figure 6 Section view along section A1-A2.

[0070] The process steps for forming the positive electrode sheet include: forming an active material layer 120, wherein the active material layer 120 is located on the active material portion 11; wherein, there is a first preset range between the active material layer 120 and the ceramic diaphragm 110, that is, the active material layer 120 and the ceramic diaphragm 110 are spaced apart, and there is a certain gap between the two. This gap can prevent the active material layer 120 and the ceramic diaphragm 110 from abutting against each other during the subsequent thermal curing treatment, and thereby prevent the materials between the active material layer 120 and the ceramic diaphragm 110 from mixing.

[0071] In some embodiments, the first preset range is 0.6 mm to 1.8 mm. The value of the first preset range can make a smaller area used as an empty foil area within the limited size of the positive electrode sheet, and a larger area is provided with an active material layer and used as the area where the oxidation reaction of the final positive electrode sheet occurs, thereby improving the energy density of the battery.

[0072] The first preset range may be 0.6 mm, 0.9 mm, 1.1 mm, 1.3 mm, 1.5 mm or 1.8 mm.

[0073] The active material layer 120 may be composed of a positive electrode active material, a conductive agent, and a first binder.

[0074] The positive electrode active material may be lithium cobalt oxide, lithium iron phosphate or lithium manganese oxide.

[0075] Conductive agents collect microcurrents between active materials and between active materials and current collectors to reduce the contact resistance of electrodes. Conductive agents can include traditional conductive agents (such as carbon black, conductive graphite, and carbon fiber, etc.) and new conductive agents (such as carbon nanotubes, graphene, and mixed conductive slurries thereof, etc.).

[0076] The main function of the first adhesive is to ensure that the active material particles and the active particles and the current collector have a certain bonding strength during the use of the battery, and is conducive to the formation of SEI (Solid Electrolyte Interphase) film. The first adhesive can be an oily adhesive, such as PVDF; or an aqueous adhesive, such as natural cellulose.

[0077] In some embodiments, the process steps for forming the active material layer 120 include: dissolving 85wt% to 95wt% of the positive electrode active material, 5wt% to 10wt% of the conductive agent and 2wt% to 10wt% of the first binder in N-methylpyrrolidone solvent according to the mass ratio, stirring for 10h to 15h under the conditions of vacuum degree of -0.07Mpa to -0.08Mpa and stirring speed of 1000rpm to 3500rpm to obtain a mixture, sieving the mixture, controlling the mesh specification to 160 mesh, and filtering the mixture through the secondary stage to prepare the positive electrode slurry, coating the positive electrode slurry on the current collector, and drying to form the active material layer 120. During the mixing process, the temperature of the slurry is controlled not to be higher than 40°C, and the discharge temperature is controlled at 23±5°C. Coating on the current collector of 15μm to 20μm at a coating rate of 5m / min to 8m / min.

[0078] In other embodiments, the process steps for forming the active material layer 120 include: uniformly dispersing the conductive agent, the active material and the adhesive by high-speed air flow shearing to obtain a conductive powder, wherein the mass percentage of the conductive agent is 1wt% to 2wt%, the mass percentage of the active material is 95wt% to 97wt%, and the mass percentage of the adhesive is 1wt% to 4wt%; and rolling the conductive powder to obtain the active material layer 120. The active material layer 120 is prepared by a dry process, and the prepared active material layer has a high compaction density, thereby having a high battery capacity. When the content of the adhesive is less than 1wt%, the bonding and contact tightness of each component cannot be guaranteed; when the content of the adhesive is higher than 4wt%, it will cause a lower battery capacity, resulting in a lower overall energy density of the battery, and is not conducive to the cycle stability of the battery. When the content of the active material is lower than 95wt%, the capacity of the battery will be reduced, resulting in a lower overall energy density that does not meet the current energy demand; when the content of the active material is higher than 97wt%, it is not conducive to the cycle stability of the battery. When the content of the conductive agent is lower than 1wt%, a complete conductive network cannot be formed, which is not conducive to the transmission of electrons / ions and the capacity of the electrode material cannot be fully utilized; when the content of the conductive additive is higher than 2wt%, it will lead to a lower overall energy density of the battery.

[0079] It should be noted that the first adhesive in the active material layer is different from the adhesive of the ceramic diaphragm. In other embodiments, the adhesive in the active material layer is the same as the adhesive of the ceramic diaphragm. In other embodiments, the adhesive in the active material layer is one or more of the above-mentioned polytetrafluoroethylene material, polyhexafluoropropylene or polyvinylidene fluoride.

[0080] Figure 8 A cross-sectional view of an energy storage cell after heat curing treatment in a method for preparing the energy storage cell provided in one embodiment of the present application.

[0081] The process steps for forming the positive electrode sheet include: performing a heat curing treatment, wherein the active material layer 120 after the heat curing treatment has a second preset range with the ceramic diaphragm 110; the heat curing treatment includes: performing a roller pressing treatment on the current collector 10 including the ceramic diaphragm 110 and the active material layer 120 at a preset temperature, so that the ceramic diaphragm 110 is fixed to the current collector 10 and the active material layer 120 is fixed on the current collector 10. The heat curing treatment may be a high-temperature calendering composite process. The use of a high-temperature calendering composite process to form the positive electrode sheet can effectively improve the compaction density of the ceramic diaphragm and the active material layer in the positive electrode sheet, and can also further improve the degree of winding of various substances in the ceramic diaphragm and various substances in the active material layer, thereby improving the mechanical properties.

[0082] In some embodiments, the second preset range is 0.5 mm to 1.5 mm. The active material layer 120 and the materials in the ceramic diaphragm 110 will not agglomerate, and the particles of the ceramic diaphragm 110 are stably connected as transmission links, establishing a good ion transmission channel and conductive network, thereby improving the electrochemical performance of the electrode.

[0083] It should be noted that the gap between the ceramic diaphragm after heat curing and the active material layer may be slightly smaller than that between the ceramic diaphragm and the active material layer after heat curing, for example, from 0.6mm to 0.5mm. Correspondingly, the thickness of the ceramic diaphragm after heat curing may be slightly smaller than that of the ceramic diaphragm after heat curing; the thickness H4 of the active material layer after heat curing may be slightly smaller than the thickness H3 of the active material layer after heat curing.

[0084] In some embodiments, the ceramic diaphragm extends to the active material portion, the distance of the ceramic diaphragm 110 located in the active material portion 11 along the first direction is a third preset distance, and the ratio between the third preset distance and the second preset distance is 5 to 20. The ratio between the third preset distance and the second preset distance can be 5, 6, 8, 10, 13, 16, 18 or 20.

[0085] The third preset distance L3 ranges from 0 mm to 1 mm. L3 may be 0 mm, 0.1 mm, 0.3 mm, 0.6 mm, 0.8 mm or 1 mm.

[0086] The preset distance L0 between the ceramic diaphragm and the end of the pole lug is in the range of 10 mm to 35 mm. The preset distance L0 between the ceramic diaphragm and the end of the pole lug may be 10 mm, 15 mm, 21 mm, 26 mm, 33 mm or 35 mm.

[0087] In some embodiments, the preset temperature is 60° C. to 130° C. At this temperature, the mobility of the particles in each film layer of the positive electrode sheet is adjusted, so that the particles move relative to each other, and under a certain pressure, a more compact and stable structure is formed, thereby increasing the compaction density, and allowing the lithium ions in the active material layer to dissolve in the electrolyte, thereby increasing the battery capacity.

[0088] Fig. 9 A top view corresponding to the formation of a pole ear in a method for preparing an energy storage cell provided in one embodiment of the present application.

[0089] The process steps for forming the positive electrode sheet include: die-cutting the current collector 10 corresponding to the pole ear portion 12 according to preset parameters, so that the pole ear portion 12 of the current collector 10 forms a pole ear.

[0090] Fig.10A top view corresponding to a positive electrode sheet formed in a method for preparing an energy storage cell provided in an embodiment of the present application.

[0091] The process steps for forming the positive electrode sheet include: cutting the current collector 10 and forming two identical positive electrode sheets.

[0092] In other embodiments, the process steps of performing heat curing and die cutting include: die cutting the current collector 10 corresponding to the pole ear portion 12 according to preset parameters so that the end of the current collector 10 forms a pole ear; the ceramic diaphragm 110 is located at the pole ear and the junction between the pole ear and the active material portion 11; and heat curing the current collector 10. In this way, the current collector is first die cut to form the pole ear, and then heat cured, which can avoid damage to the ceramic diaphragm during the die cutting process, thereby ensuring the stability of the final ceramic diaphragm.

[0093] The preparation method comprises: forming a negative electrode sheet.

[0094] The negative electrode sheet 2 includes a negative electrode current collector and a negative electrode active material layer, and the negative electrode active layer is located on the negative electrode current collector. A portion of the negative electrode current collector is cut into the shape of a tab and serves as a negative electrode tab.

[0095] The negative electrode current collector may be copper foil, which has low electrical conductivity and can have high electron transmission capacity, and copper foil has weak lithium insertion capacity and captures fewer lithium ions, thereby effectively reducing the loss of lithium ions. In other embodiments, the negative electrode current collector may also be a foam copper current collector, a copper mesh current collector, and a three-dimensional nano copper array current collector.

[0096] In some embodiments, the negative electrode active material layer may be composed of a negative electrode active material, a conductive agent, and a binder. The negative electrode active material may be carbon material and non-carbon material: carbon-based materials include graphite materials (natural graphite, artificial graphite, and mesophase carbon spheres) and other carbon-based materials (hard carbon, soft carbon, and graphene); non-carbon-based materials may be subdivided into titanium-based materials, silicon-based materials, tin-based materials, nitrides, and metallic lithium, etc.

[0097] The conductive agent is similar to that of the positive electrode active material layer, and the adhesive for the negative electrode is similar to that for the positive electrode, mainly including oil-based PVDF, water-based CMC, PAMAC, polyvinyl alcohol (PVA), sodium alginate, etc., which will not be repeated here.

[0098] The process steps for forming the negative electrode sheet include: providing a negative electrode current collector; preparing a negative electrode slurry, and coating the negative electrode slurry on a negative electrode current collector of 15 μm to 20 μm at a speed of 5 m / min to 8 m / min, and die-cutting a portion of the negative electrode current collector according to preset parameters so that the end of the current collector forms a negative electrode ear; cutting the current collector to form two identical negative electrode sheets 2.

[0099] In some embodiments, the preparation step of the negative electrode slurry includes: dissolving 85wt% to 95wt% of the negative electrode active material, 5wt% to 15wt% of the conductive agent and 2wt% to 10wt% of the binder in N-methylpyrrolidone solvent according to the mass ratio, stirring for 12h to 18h under the conditions of vacuum degree of -0.07Mpa to -0.08Mpa and stirring speed of 1000rpm to 3000rpm to obtain a mixture, sieving the mixture, controlling the mesh specification to 0 mesh, and filtering it through secondary filtering to prepare the negative electrode slurry.

[0100] Fig.11 A top view of an energy storage cell that is being wound in a method for preparing an energy storage cell provided in an embodiment of the present application.

[0101] The positive electrode sheet 1 and the negative electrode sheet 2 provided above serve as the positive electrode and the negative electrode of the energy storage cell respectively. The positive electrode is the electrode plate where oxidation reaction occurs in the energy storage cell, and the negative electrode is the electrode plate where reduction reaction occurs in the energy storage cell. The positive electrode and the negative electrode are isolated and connected together by an electrolyte, and the positive electrode and the negative electrode serve as the electrochemical reaction area of ​​the energy storage cell.

[0102] refer to Fig.11 The preparation method includes: forming a diaphragm 3.

[0103] The separator 3 can be located between the positive electrode sheet 1 and the negative electrode sheet 2 to prevent the short circuit problem caused by the physical contact between the positive electrode sheet 1 and the negative electrode sheet 2, while allowing ions to be conducted through the electrolyte and hindering the transmission of electrons, so that ions and electrons form a circuit during the charge and discharge process of the battery.

[0104] The diaphragm 3 can be any one of a microporous membrane, a modified microporous membrane, a non-woven membrane and a composite membrane. A microporous membrane is a membrane with a pore size in the micrometer range, mainly including polyolefin microporous membranes and other polymer microporous membranes. A modified microporous membrane is a membrane obtained by modifying a microporous membrane. Common modification methods include surface treatment, chemical grafting, surface coating, etc. Non-woven membranes have a small fiber diameter and generally show a higher porosity than other types of membranes. Composite membranes are prepared by coating or filling inorganic materials in microporous membranes or non-woven membranes, and have higher thermal stability and electrolyte wettability than other types of membranes.

[0105] In some embodiments, the diaphragm 3 may be coated with a polyvinylidene fluoride (PVDF) material so that the diaphragm 3 has excellent adhesion and flexibility. Since the diaphragm 3 has excellent adhesion, the diaphragm 3 and the positive electrode sheet 1 or the diaphragm 3 and the negative electrode sheet 2 can have good contact performance, thereby reducing the assembly time of the energy storage battery cell, thereby effectively reducing the overall production cost of the energy storage battery cell. Since the diaphragm 3 has excellent flexibility, the strength of the diaphragm 3 is improved, which is conducive to effectively improving the impact resistance of the diaphragm 3.

[0106] refer to Fig.11 , the positive electrode sheet 1, the negative electrode sheet 2 and the separator 3 are wound.

[0107] In some embodiments, the winding process is to wind the separator 3, the positive electrode sheet 1, and the negative electrode sheet 2 into a single winding core by a winding machine. The order is to use the negative electrode sheet 2 to wrap the positive electrode sheet 1, and then separate the positive electrode sheet 1 and the negative electrode sheet 2 by the separator 3.

[0108] In some embodiments, a small winding tension will affect the internal resistance and shell penetration rate; excessive tension can easily cause short circuit or fragmentation risks. Therefore, the winding tension is generally between 0.08 and 0.15 MPa for positive tension, 0.08 and 0.15 MPa for negative tension, 0.08 and 0.15 MPa for upper diaphragm tension, and 0.08 and 0.15 MPa for lower diaphragm tension. The width of the negative electrode sheet 2, the width of the positive electrode sheet 1, and the width of the diaphragm 3 are not the same. For example, the width of the negative electrode sheet is 59.5 mm, the width of the positive electrode sheet is 58 mm, and the width of the diaphragm is 61 mm. The three are aligned in the center to improve the alignment of the electrode sheets and avoid the risk of short circuit. The electrode sheet alignment refers to the relative positions of the positive electrode sheet 1, the negative electrode sheet 2, and the diaphragm 3.

[0109] It should be noted that in order to explain and distinguish the diaphragm, the positive electrode sheet and the negative electrode sheet, Fig.11 The dotted line indicates the separator, the thinner solid line indicates the negative electrode, and the thicker solid line indicates the positive electrode, but this does not represent the thickness relationship between the separator, the positive electrode, and the negative electrode. Fig.11 There are gaps between the middle diaphragm, the positive electrode sheet and the negative electrode sheet. This is to clearly indicate the winding correspondence between the diaphragm, the positive electrode sheet and the negative electrode sheet, but it does not mean that there must be a gap between the diaphragm and the positive electrode sheet or between the diaphragm and the negative electrode sheet. In other words, the diaphragm and the positive electrode sheet can contact each other, or the diaphragm and the negative electrode sheet can contact each other.

[0110] The method for preparing the energy storage battery cell also includes: placing the whole body formed by winding the positive electrode sheet 1, the negative electrode sheet 2 and the separator 3 in a cavity formed by the shell, and the cavity is also filled with electrolyte.

[0111] The electrolyte is a carrier that conducts electrons between the positive and negative electrodes in the battery. In some embodiments, the electrolyte can be an electrolyte, which consists of three parts: a solvent, a lithium salt, and an additive. The solvent is used to dissolve the lithium salt, and the solvent may include cyclic carbonates (PC, EC); chain carbonates (DEC, DMC, EMC); carboxylates (MF, MA, EA, MA, MP, etc.). The lithium salt may be LiPF6, LiClO4, LiBF4, LiAsF6, etc. The additive may be a film-forming additive, a conductive additive, a flame retardant additive, an overcharge protection additive, an additive for controlling the content of H2O and HF in the electrolyte, an additive for improving low temperature performance, and a multifunctional additive. One or more.

[0112] The preparation method includes: welding the pole ear, welding the pole ear to the adapter, connecting the other end of the adapter to the pole, and engaging the top rod with the shell. The adapter is located in the chamber, and the pole passes through the top cover.

[0113] Among them, the adapter plate includes at least a first adapter plate and a second adapter plate, the pole includes a positive pole pole and a negative pole pole, the first adapter plate is electrically connected to the pole ear 110 of the positive pole plate 1 and the positive pole pole respectively, and the second adapter plate is electrically connected to the negative pole ear and the negative pole pole of the negative pole plate 2 respectively.

[0114] The beneficial effects of the embodiments of the present application will be further illustrated below in combination with embodiments and comparative examples.

[0115] Example 1: Boehmite powder and polytetrafluoroethylene material are evenly dispersed by high-speed air flow shearing to obtain a mixed powder, wherein the mass percentage of boehmite powder is 85wt%, and the mass percentage of polytetrafluoroethylene material is 15wt%; the mixed powder is roller-pressed to obtain a ceramic diaphragm.

[0116] Example 2: The difference from Example 1 is that the mass percentage of boehmite powder is 90wt%, and the mass percentage of polytetrafluoroethylene material is 10wt%.

[0117] Example 3: The difference from Example 1 is that the mass percentage of boehmite powder is 94wt%, and the mass percentage of polytetrafluoroethylene material is 6wt%.

[0118] Comparative Example 1: The difference from Example 1 is that: a ceramic diaphragm is prepared by a wet process, boehmite powder, PVDF particles and NMP solvent are stirred at 50°C until no PVDF particles and boehmite powder are visually removed to obtain a mixed slurry; the mixed slurry is coated on a current collector and dried.

[0119] Comparative Example 2: The difference from Comparative Example 1 is that after the drying treatment, the dried ceramic diaphragm is subjected to a roller pressing treatment.

[0120] Comparative Example 3: The difference from Example 1 is that the mass percentage of boehmite powder is 99wt%, and the mass percentage of polytetrafluoroethylene material is 1wt%.

[0121] Comparative Example 4: The difference from Example 1 is that the mass percentage of boehmite powder is 78wt%, and the mass percentage of polytetrafluoroethylene material is 22wt%.

[0122] The above embodiments and comparative examples were subjected to mechanical tensile strength tests in turn, and the test results were summarized and recorded in Table 1. The mechanical tensile strength test is used to characterize the strength of the ceramic diaphragm, which is then expressed as the ability of the tab to resist tearing, and the tear test is used to characterize whether the tab has a tearing problem. The ceramic diaphragm defect rate refers to the summary of the ceramic diaphragm being damaged, the ceramic diaphragm having poor insulation performance, and the ceramic particles of the ceramic diaphragm being detached, and the defect rate is determined by the magnitude of the defect.

[0123] Table 1

[0124]

[0125]

[0126] The experimental data of the above-mentioned Examples 1, 2 and 3 indicate that the ceramic material and the adhesive are evenly mixed by high-speed airflow shearing to form a ceramic diaphragm, which can improve the tensile strength of the ceramic diaphragm and thereby improve the performance of the prepared ceramic diaphragm.

[0127] The experimental data of the above-mentioned Example 1, Comparative Example 1 and Comparative Example 2 show that, compared with the ceramic diaphragm prepared by the conventional wet process, the ceramic diaphragm prepared by high-speed airflow shearing has higher mechanical strength and stronger tensile strength, thereby making the prepared ceramic diaphragm have better performance.

[0128] The experimental data of the above-mentioned Example 1 and Comparative Examples 3 and 4 show that when the content of the adhesive is high, the mechanical strength of the ceramic diaphragm increases, that is, the tensile strength increases, but the defective rate of the positive electrode increases significantly; on the contrary, although the proportion of the ceramic material can be increased to increase the insulation effect of the positive electrode, the content of the adhesive is low, which reduces the mechanical strength of the ceramic diaphragm, that is, the tensile strength decreases. The energy storage cell prepared by the ceramic diaphragm provided by the above-mentioned embodiment includes the following embodiments:

[0129] Example 4: The ceramic diaphragm prepared in the above Example 2; 86wt% of lithium cobalt oxide, 9wt% of the conductive agent and 5wt% of the first binder are dissolved in N-methylpyrrolidone solvent according to the mass ratio, and stirred for 15h under the conditions of vacuum degree of -0.07Mpa and stirring speed of 1000rpm to obtain positive electrode slurry, and the positive electrode slurry is coated on the current collector and dried to form an active material layer. The current collector including the ceramic diaphragm and the active material layer is subjected to thermal curing treatment to prepare a positive electrode sheet; the negative electrode sheet, the positive electrode sheet and the separator are prepared into an energy storage battery cell. Among them, the distance between the active material layer and the ceramic diaphragm is 0.8mm.

[0130] Example 5: The difference from Example 4 is that the active material layer is formed by a dry process. The conductive agent, active material and binder are uniformly dispersed by high-speed air flow shearing to obtain a conductive powder, wherein the mass percentage of the conductive agent is 2wt%, the mass percentage of the active material is 95wt%, and the mass percentage of the binder is 3wt%; the conductive powder is roll-pressed to obtain an active material layer.

[0131] Example 6: The difference from Example 4 is that the distance between the active material layer and the ceramic diaphragm is 1.2 mm.

[0132] Comparative Example 5: The difference from Example 4 is that the distance between the active material layer and the ceramic diaphragm is 0 mm.

[0133] Comparative Example 6: The difference from Comparative Example 4 is that the distance between the active material layer and the ceramic diaphragm is 2 mm.

[0134] Comparative Example 7: The difference from Example 5 is that the distance between the active material layer and the ceramic diaphragm is 0 mm.

[0135] The above-mentioned embodiments and comparative examples were subjected to cross-linking test and tearing test in turn, and the test results were summarized and recorded in Table 1. The cross-linking test is used to characterize whether there is a cross-linking problem between the ceramic diaphragm and the active material layer, and the tearing test is used to characterize whether the tab has a tearing problem. The positive electrode sheet yield refers to the summary of the electrochemical properties, compaction density, and separation of active material particles of the positive electrode sheet, and the yield is judged by the magnitude of the performance.

[0136] The cross-linking test includes: using a scanning electron microscope (SEM) to magnify the structure of the connection between the ceramic diaphragm and the active material layer, and observe whether the two are in contact and whether the particles of the two are mixed. If the two are in contact with each other or the particles of the two are mixed, it is considered that there is cross-linking. If not, it is considered that there is no cross-linking.

[0137] The tear test includes: bending the positive electrode sheet including the tab along the arrangement direction of the tab and the active material part, with a bending angle of 60° to 120°. After bending 10 times, the surface condition of the end of the tab is observed under a microscope. If there are torn gaps or even damage on the surface of the tab, it is considered to have a tear probability, and the tear probability is judged based on the surface condition; if there is no trace, it is considered to have no tear probability.

[0138] The electrochemical test includes: the weight of the energy storage cell of each embodiment is a fixed value, i.e. 25g. The cell is fully charged at room temperature (25°C), and then discharged at a rate of 1C to a cut-off voltage (2.5V) after being fully left in the test environment, and the released capacity (energy) is recorded. In actual experiments, the test can be repeated three times in a row to take the average value to improve accuracy.

[0139] Table 2

[0140] project Tab tearing probability Is there any cross-linking problem? Positive electrode yield Example 4 0.1% 0.2% 99.6% Example 5 0.1% 0.01% 99.99% Example 6 0.1% 0.1% 99.9% Comparative Example 5 0.4% 0.5% 99.1% Comparative Example 6 0.01% 1% 99.99% Comparative Example 7 0.2% 0.1% 99.7%

[0141] The experimental data of the above-mentioned Example 4, Example 5, Comparative Example 7 and Comparative Example 6 show that forming the active material layer by a dry process can avoid the problem of particles of the ceramic diaphragm and the active material layer mixing with each other, and the yield of the positive electrode sheet is higher.

[0142] The experimental data of the above-mentioned Example 6, Comparative Example 5 and Comparative Example 6 show that separating the ceramic diaphragm from the active material layer and controlling the spacing distance can avoid the problem of cross-linking, improve the yield of the positive electrode sheet, and improve the energy density of the energy storage cell. The preparation method of the energy storage cell provided in the embodiment of the present application uses high-speed airflow shearing to evenly mix the ceramic material and the adhesive, rather than using the process of dissolving the adhesive and dispersing the ceramic material with an NMP solution, which can avoid the safety problem of NMP solvent volatilization. Compared with the preparation of the ceramic diaphragm 110 using an NMP solution, the use of the high-speed airflow shearing method can be regarded as preparing the ceramic diaphragm 110 through a dry process. In this process, the adhesive forms friction between the adhesive molecules through the high-speed shear force, thereby generating fibers. The fibers can coat the ceramic material and form a network structure, thereby having good mechanical properties, thereby improving the mechanical properties of the tabs and avoiding the tabs from tearing. Secondly, the positive electrode sheet is formed by thermal curing treatment, that is, the current collector 10 including the ceramic diaphragm 110 and the active material layer 120 is roll-pressed at a preset temperature, which can effectively increase the compaction density of the ceramic and active material layers in the positive electrode sheet, and can also further increase the degree of entanglement of various substances in the tab and the active material layer, thereby improving the mechanical properties.

[0143] Accordingly, according to some embodiments of the present application, the embodiments of the present application further provide an energy storage cell, which can be prepared using the preparation method provided in the above embodiments, and the technical features that are the same as or corresponding to the above embodiments will not be described in detail here.

[0144] refer to Fig.10 and Fig.11 , the energy storage cell comprises: a diaphragm 3, and a positive electrode sheet 1 and a negative electrode sheet 2 located on both sides of the diaphragm 3, the positive electrode sheet 1 is prepared by the preparation method of the energy storage cell of any one of the above embodiments; the positive electrode sheet 1 comprises a current collector 10, a ceramic diaphragm 110 and an active material layer 120, the current collector 10 has a pole ear 13 and an active material part 11, the ceramic diaphragm 110 is at least located on the pole ear 3 and at the junction between the pole ear and the active material part 11; the active material layer 120 is located on the active material part 11, and there is a second preset range L2 between the active material layer 120 and the ceramic diaphragm 110. In other words, the active material layer 120 and the ceramic diaphragm 110 are arranged at intervals from each other and do not abut each other, so that the problem of mutual material between the slurry of the active material layer 120 and the slurry of the ceramic diaphragm 110 can be effectively avoided, and the adsorption problem caused by the combination of the slurry of the active material layer 120 and the slurry of the ceramic diaphragm 110 can be effectively avoided, thereby improving the electron transmission capacity of the lithium-ion battery.

[0145] In some embodiments, the ceramic diaphragm 110 is also located on a portion of the active material portion 11 , and the distance of the ceramic diaphragm 110 located in the active material portion 11 along the first direction is a third preset distance, and a ratio of the third preset distance to the second preset distance is 5-20.

[0146] Those skilled in the art will appreciate that the above-mentioned embodiments are specific examples for implementing the present application, and in practical applications, various changes may be made to the embodiments in form and detail without departing from the spirit and scope of the present application. Any person skilled in the art may make various changes and modifications without departing from the spirit and scope of the present application, and therefore the scope of protection of the present application shall be subject to the scope defined in the claims.

Claims

1. A method for preparing an energy storage battery cell, characterized in that: include: forming a separator and a positive electrode sheet and a negative electrode sheet located on both sides of the separator; The process steps for forming the positive electrode sheet include: Providing a current collector, the current collector having two electrode lugs and an active material portion located between the two electrode lugs; A ceramic diaphragm is formed, the ceramic diaphragm being located at least at the electrode ear portion and at the interface between the electrode ear portion and the active material portion. The process steps for forming the ceramic diaphragm include: uniformly dispersing a ceramic material and a binder by high-speed airflow shearing to obtain a mixed powder, wherein the mass percentage of the ceramic material is 80wt% to 98wt% and the mass percentage of the binder is 2wt% to 20wt%; and roller-pressing the mixed powder to obtain the ceramic diaphragm; forming an active material layer, the active material layer being located on the active material portion; wherein a first preset range is defined between the active material layer and the ceramic diaphragm; Performing a heat curing treatment, wherein a second preset range is defined between the active material layer and the ceramic diaphragm after the heat curing treatment; the heat curing treatment comprising: performing a roller pressing treatment on the current collector including the ceramic diaphragm and the active material layer at a preset temperature to fix the ceramic diaphragm to the current collector and the active material layer to the current collector; Die-cutting the current collector corresponding to the tab portion according to preset parameters so that the tab portion of the current collector forms a tab; Cutting the current collector to form two identical positive electrode sheets; The separator, the positive electrode sheet, and the negative electrode sheet are wound together.

2. The method for preparing the energy storage battery cell according to claim 1, wherein: The second preset range is 0.5 mm to 1.5 mm.

3. The method for preparing the energy storage battery cell according to claim 1, wherein: The adhesive is one or more of polytetrafluoroethylene, polyhexafluoropropylene or polyvinylidene fluoride.

4. The method for preparing the energy storage battery cell according to claim 3, characterized in that: The adhesive is a polytetrafluoroethylene material, the mass percentage of the ceramic material is 85wt% to 95wt%, and the mass percentage of the polytetrafluoroethylene material is 5wt% to 15wt%.

5. The method for preparing the energy storage battery cell according to claim 1, wherein: The process parameters for uniformly dispersing the ceramic material and the adhesive by high-speed airflow shearing to obtain a mixed powder include: a feed flow rate of 100L / h to 2000L / h, an airflow velocity of 10m / s to 500m / s, and a temperature of 20°C to 60°C.

6. The method for preparing the energy storage battery cell according to claim 1, characterized in that: The preset temperature is 60-130°C.

7. The method for preparing an energy storage battery cell according to claim 1, wherein: The process steps for forming the active material layer include: uniformly dispersing the conductive agent, the active material and the adhesive by high-speed airflow shearing to obtain a conductive powder, wherein the mass percentage of the conductive agent is 1wt% to 2wt%, the mass percentage of the active material is 95wt% to 97wt%, and the mass percentage of the adhesive is 1wt% to 4wt%; and roller-pressing the conductive powder to obtain the active material layer.

8. The method for preparing an energy storage battery cell according to claim 1, wherein: The process steps of performing the thermal curing treatment and the die-cutting include: die-cutting the current collector corresponding to the pole ear portion according to preset parameters so that the end of the current collector forms a pole ear; the ceramic diaphragm is located at the pole ear and at the junction between the pole ear and the active material portion; and performing the thermal curing treatment on the current collector.

9. An energy storage battery cell, characterized in that: include: A diaphragm, and a positive electrode sheet and a negative electrode sheet located on both sides of the diaphragm, the positive electrode sheet is prepared by the preparation method of the energy storage cell according to any one of claims 1 to 8; the positive electrode sheet includes a current collector, a ceramic diaphragm and an active material layer, the current collector has a pole ear and an active material portion, the ceramic diaphragm is located at least on the pole ear and at the junction between the pole ear and the active material portion; the active material layer is located on the active material portion, and a second preset range is between the active material layer and the ceramic diaphragm.

10. The energy storage cell according to claim 9, characterized in that: The ceramic diaphragm is also located on a portion of the active material portion. The distance of the ceramic diaphragm located on the active material portion along the first direction is a third preset distance. The ratio of the third preset distance to the second preset distance is 5-20.

Citation Information

Patent Citations

  • All-solid-state lithium battery and preparation method thereof

    CN113140731A

  • All-solid-state battery cell and preparation method and application thereof

    CN114497752A

  • Dry-method electrode film, preparation method and application thereof

    CN116885182A

  • Nonaqueous secondary battery and method for producing the same