Monocrystal ternary positive electrode material and regeneration method thereof

Through the adsorption treatment of dilute acid and reducing agent and the loaded porous oxide, combined with spray drying and sintering steps, the problem of difficult purification of target metal salts and complex process in waste lithium batteries is solved, and efficient and environmentally friendly The single crystal ternary cathode material recycling improves resource utilization and material performance.

CN118943549APending Publication Date: 2024-11-12ZHEJIANG ZEEKR INTELLIGENT TECH CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411014839.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, the purification of target metal salts in waste lithium batteries is difficult, the process is complex and the cost is high, and the dry recycling has problems such as impurity residue and low compatibility.

Method used

The active ions are leaching liquid of dilute acid and reducing agent, combined with the adsorption treatment of loaded porous oxides and inorganic alkalis, and the regenerated single-crystal ternary cathode material is prepared by spray drying and sintering steps, simplifying the process, reducing pollution and cost .

Benefits of technology

It realizes efficient recycling of lithium, nickel, cobalt and manganese elements, improves resource utilization, ensures the uniformity of the morphology, size and structural properties of the material, and is suitable for a wide range of applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943549A_ABST
    Figure CN118943549A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of waste lithium battery recycling, in particular to a single-crystal ternary positive electrode material and a regeneration method thereof.The method comprises the steps that S1, slurry containing to-be-treated battery powder and leaching liquid are mixed to be subjected to acid leaching treatment, and acid leaching liquid is obtained; s2, mixing the acid leaching solution with an adsorbent, and performing adsorption treatment to obtain a purified solution; s3, adjusting the ratio of the amount of substance of Li, Ni, Co and Mn in the purified liquid to be consistent with the proportion of each metal of the target ternary positive electrode material to obtain a compound liquid; s4, performing spray drying on the compound liquid to obtain a lithium-containing intermediate; carrying out sintering treatment on the intermediate; wherein the leaching solution comprises a reducing agent and acid; the adsorbent includes a supported porous oxide. The method is simple in technology, small in pollution and easy to control, solves the problem of waste lithium battery resource recovery, can utilize lithium, nickel, cobalt and manganese elements to the maximum extent, and improves the utilization rate of waste resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of waste lithium battery recycling, and in particular to a single crystal ternary cathode material and a regeneration method thereof. Background Art

[0002] Compared with traditional lithium iron phosphate, nickel cobalt manganese oxide ternary cathode material (LiNi x Co y Mn 1-x-y O2) has a higher specific capacity and can greatly improve the energy density of the battery. It is the mainstream positive electrode material in the field of electric passenger vehicles. Comparing the performance of single crystal and polycrystalline ternary materials, single crystal ternary materials do not have the secondary particle breakage problem of polycrystalline ternary materials during the cycle process. They perform better in terms of safety performance and cycle performance, and the compaction density is relatively high. Single crystalization is an important research and development direction for ternary materials and battery companies. However, with the widespread application of lithium batteries, the amount of waste is also increasing. Waste lithium batteries contain a large amount of valuable metals, such as nickel, cobalt, manganese and lithium. The recovery and reuse of these metals are of great significance to environmental protection and sustainable resource utilization. Therefore, there is an urgent need to develop an efficient and environmentally friendly recycling process in this field.

[0003] Currently, the recycling of used lithium batteries is primarily divided into two methods: wet recycling and dry recycling. The wet method involves dissolving the valuable metals from the used lithium batteries through methods such as acid leaching, followed by separation and purification through precipitation and solvent extraction. However, the dry method is difficult to repair and remove impurities, and residual impurities seriously affect the morphology, size, and structural uniformity of the recycled products, thereby affecting the electrochemical performance of the recycled materials and leading to low-end applications. Furthermore, the dry method has low process compatibility and cannot be mass-produced, which also limits its application in industrial production. Summary of the Invention

[0004] In view of this, the present invention is committed to providing a method for regenerating single-crystal ternary positive electrode materials using waste batteries, so as to solve the problems of difficulty, complex process and high cost in purifying each target metal salt in waste ternary lithium batteries in the prior art.

[0005] A first aspect of the present invention provides a method for regenerating a single crystal ternary cathode material, the method comprising the following steps:

[0006] S1. Mixing a slurry containing battery powder to be processed with a leaching solution and performing an acid leaching treatment to obtain an acid leaching solution;

[0007] S2, mixing the acid leaching solution with an adsorbent and performing adsorption treatment to obtain a purified solution and a used adsorbent;

[0008] S3. Adjusting the molar ratio of Li, Ni, Co, and Mn in the purified solution to be consistent with the ratio of each metal in the target ternary positive electrode material to obtain a composite solution;

[0009] S4, spray drying the composite liquid to obtain a lithium-containing ternary oxide intermediate; sintering the lithium-containing ternary oxide intermediate;

[0010] Wherein, the leaching solution includes a reducing agent and an acid; and the adsorbent includes a supported porous oxide.

[0011] The method of the present invention removes impurities and retains valuable metal ions, obtains a compounded mixed liquid through compounding, obtains a lithium-containing ternary oxide intermediate through spray drying, and then directly synthesizes the target single crystal ternary material through sintering treatment. The method of the present invention has lower recovery cost, less three wastes, high environmental protection, and can be matched with production lines for different raw materials (such as liquid-injected and non-liquid-injected scrapped battery cells or electrodes), and has high compatibility.

[0012] Optionally, in step S1, the reducing agent includes at least one of hydrogen peroxide, sodium sulfite, glucose and ascorbic acid; the acid includes an organic acid; optionally, the reducing agent includes hydrogen peroxide and the acid includes acetic acid; and / or, based on the total mass of the leaching solution, the mass fraction of the reducing agent is 5 to 10 wt%; and / or, the solid-liquid ratio of the acid leaching treatment is 40 to 100 g / L; and / or, the conditions of the acid leaching treatment include: the acid leaching temperature is 50 to 95° C., the acid leaching time is 1 to 4 h, and the pH in the system is 1.5 to 4.

[0013] Optionally, in step S2, the supported porous oxide comprises ZrO2 and / or TiO2; and / or

[0014] Or, the amount of the adsorbent per liter of the acid leaching solution satisfies the formula Y=X / a (wherein, X represents the mass concentration of anions in the acid leaching solution; a represents the actual optimal adsorption capacity of the adsorbent for the anions; the anions include fluoride ions and / or phosphate ions); and / or, the conditions for the adsorption treatment include: an adsorption temperature of 40 to 80°C, an adsorption time of 0.3 to 2 hours, and a pH in the system of 3 to 6; optionally, the conditions for the adsorption treatment further include: adding a pH regulator during the adsorption treatment; optionally, the pH regulator includes an inorganic base and / or an organic acid.

[0015] Optionally, in step S3, in the composite liquid, the ratio of the amount of Li to the total amount of Ni, Co and Mn is 1.01-1.14:1; the ratio of the amount of Ni, Co and Mn is (0.53-0.93):(0.043-0.1):(0.016-0.28).

[0016] Optionally, in step S4, the spray drying conditions include: an inlet temperature of 160 to 250°C, an outlet temperature of 80 to 100°C, an atomization pressure of 0.2 to 0.4 MPa, and a feed rate of 5 to 20 mL / min; the sintering treatment includes: pre-sintering the lithium-containing ternary oxide intermediate to obtain a lithium-containing ternary oxide precursor; and sintering the lithium-containing ternary oxide precursor at a high temperature; wherein the pre-sintering conditions include: a heating rate of 2 to 6°C / min, a pre-sintering temperature of 400 to 550°C, and a pre-sintering time of 4 to 8 hours; the high-temperature sintering conditions include: a heating rate of 2 to 5°C / min, a sintering temperature of 800 to 950°C, and a sintering time of 4 to 8 hours.

[0017] Optionally, the battery powder to be processed includes ternary lithium battery powder.

[0018] Optionally, the method further includes: regenerating the used adsorbent to obtain a regenerated adsorbent; mixing the regenerated adsorbent with the acid leaching solution and then performing the adsorption treatment; wherein the regeneration treatment includes: performing a first leaching on the used adsorbent to obtain a leached adsorbent; mixing the leached adsorbent with an alkaline solution to obtain a regenerated mixed solution; and vacuum filtering and a second leaching on the regenerated mixed solution.

[0019] Optionally, the washing liquid of the first elution includes water; the alkaline solution includes aqueous ammonia; the pH of the regeneration mixed solution is 10-12; and the washing liquid of the second elution includes water.

[0020] Optionally, the method further comprises: collecting acid waste gas generated by the spray drying; and dissolving the acid waste gas in a solvent and mixing the solvent with the reducing agent, and adding the solvent as the leaching liquid to step S1.

[0021] A second aspect of the present invention provides a single crystal ternary cathode material, which is prepared by the above method.

[0022] Through the above technical scheme, the method of the present invention uses dilute acid and reducing agent as leaching liquid to directly leach active ions in waste ternary lithium battery powder; by using loaded porous oxide and inorganic base for efficient simultaneous impurity removal and filtration, a purified solution is obtained; the elements in the purified solution are compounded to obtain a compounded solution; a lithium-containing ternary oxide intermediate is synthesized by spray drying, and the lithium-containing ternary oxide intermediate is pre-sintered and high-temperature sintered to prepare a regenerated single crystal ternary positive electrode material. The technical process of the present invention is simple, has low pollution, and is easy to control. It solves the problem of recycling waste lithium battery resources, and can maximize the utilization of lithium, nickel, cobalt and manganese elements therein, thereby improving the utilization rate of waste resources. The regenerated single crystal ternary positive electrode material prepared by the method of the present invention ensures the uniformity of the morphology, size and structure of the material, has strong performance, and is suitable for a wide range of applications.

[0023] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following detailed description, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:

[0025] Figure 1 Shown is a process flow chart of Example 1;

[0026] Figure 2 Shown is a SEM image of the lithium-containing ternary oxide intermediate prepared in Example 1;

[0027] Figure 3 Shown is a SEM image of the recycled single crystal ternary cathode material prepared in Example 1;

[0028] Figure 4 Shown is an XRD comparison chart of the regenerated single crystal ternary cathode material prepared in Example 1 and the conventionally synthesized single crystal ternary cathode material;

[0029] Figure 5 Shown is a SEM image of the regenerated single crystal ternary cathode material prepared in Example 2;

[0030] Figure 6 Shown is a SEM image of the regenerated single crystal ternary cathode material prepared in Example 3;

[0031] Figure 7 Shown is the SEM image of the regenerated single crystal ternary positive electrode material prepared in Example 4. DETAILED DESCRIPTION

[0032] The present invention discloses a method for regenerating single-crystal ternary positive electrode materials using waste ternary lithium batteries. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the method. It is particularly important to point out that all similar replacements and modifications are obvious to those skilled in the art and are considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments. Relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0033] In the description of the present invention, a list of items connected by the term "at least one of" or other similar terms can mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A can include a single element or multiple elements. Item B can include a single element or multiple elements. Item C can include a single element or multiple elements.

[0034] The endpoints of the ranges and any values ​​disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoints of each range, the endpoints of each range or the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered to be specifically disclosed herein.

[0035] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0036] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0037] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.

[0038] In order to solve the problems of difficulty, complex process and high cost in purifying target metal salts in waste ternary lithium batteries in the prior art, the present invention adopts the following technical solution:

[0039] The first aspect of the present invention provides a method for regenerating a single crystal ternary cathode material, such as Figure 1 As shown, the method includes the following steps:

[0040] S1. Mixing a slurry containing battery powder to be processed with a leaching solution and performing an acid leaching treatment to obtain an acid leaching solution;

[0041] S2, mixing the acid leaching solution with an adsorbent and performing adsorption treatment to obtain a purified solution and a used adsorbent;

[0042] S3. Adjusting the molar ratio of Li, Ni, Co, and Mn in the purified solution to be consistent with the ratio of each metal in the target ternary positive electrode material to obtain a composite solution;

[0043] S4, spray drying the composite liquid to obtain a lithium-containing ternary oxide intermediate; sintering the lithium-containing ternary oxide intermediate;

[0044] Wherein, the leaching solution includes a reducing agent and an acid; and the adsorbent includes a supported porous oxide.

[0045] The method provided by the present invention for regenerating single-crystal ternary cathode materials from waste batteries involves directly leaching active ions from waste battery powder using a dilute acid and a reducing agent as leaching solutions; efficiently and simultaneously removing impurities using a supported porous oxide and an inorganic base to obtain a purified solution; compounding the various elements in the purified solution to obtain a compounded solution; and synthesizing a lithium-containing ternary oxide intermediate using spray drying. This lithium-containing ternary oxide intermediate is then sintered to produce a regenerated single-crystal ternary cathode material. The present invention has a simple process, minimal pollution, and is easy to control. It solves the problem of recycling waste lithium batteries and maximizes the utilization of the lithium, nickel, cobalt, and manganese elements present, improving the utilization rate of waste resources.

[0046] According to the present invention, in step S1, by adding a reducing agent to the leachate, the leaching efficiency of the metal elements can be improved, thereby achieving efficient recovery and utilization. The reducing agent in the present invention can include at least one of hydrogen peroxide, sodium sulfite, glucose, and ascorbic acid. To avoid secondary contamination, the reducing agent can be hydrogen peroxide.

[0047] The acid used in step S1 of the present invention can be any known acid in the art, and can include, for example, an organic acid or an inorganic acid. Preferably, to reduce corrosion to equipment and the release of toxic gases, while also reducing energy consumption in the subsequent spray drying step, the acid can include an organic acid, such as acetic acid and / or citric acid. More preferably, the acid is acetic acid.

[0048] According to the present invention, the mass fraction of the reducing agent may be 5 to 10 wt % based on the total mass of the leachate. For example, the mass fraction of the reducing agent may be any one of 5 wt %, 6 wt %, 7 wt %, 8 wt %, 9 wt %, and 10 wt %, or any value within a range consisting of any two of the foregoing values.

[0049] According to the present invention, in step S1, the solid-to-liquid ratio of the acid leaching treatment can be 40 to 100 g / L. The "solid-to-liquid ratio of the acid leaching treatment" referred to in the present invention refers to the ratio of the mass of solids to the volume of liquid in the acid leaching treatment system. For example, the solid-to-liquid ratio of the acid leaching treatment can be any value among 40 g / L, 50 g / L, 60 g / L, 70 g / L, 80 g / L, 90 g / L, and 100 g / L, or any value within a range consisting of any two of these values. In the present invention, the conditions for the acid leaching treatment may include: an acid leaching temperature of 50 to 95°C, an acid leaching time of 1 to 4 hours, and a pH within the system of 1.5 to 4.

[0050] The adsorbent used in the present invention includes a supported porous oxide, which has a high adsorption capacity and can achieve deep and efficient impurity removal. In the present invention, the supported porous oxide can be selected from ZrO2 and / or TiO2. In an exemplary embodiment of the present invention, the adsorbent used in the present invention is a zirconium-titanium adsorbent, wherein the total content of ZrO2 and / or TiO2 is not less than 33wt%, and the adsorbent may contain trace amounts of other metal elements, for example, it may contain no more than 0.003wt% Ni, no more than 0.02wt% Ca, no more than 0.002wt% Pb, no more than 0.002wt% Zn, no more than 0.01wt% Fe, and no more than 0.002wt% Mg.

[0051] According to the present invention, the amount of the adsorbent per liter of the acid leaching solution can satisfy the formula Y=X / a (wherein, X represents the mass concentration of anions in the acid leaching solution (in mg / L), optionally, 5 mg / L≤X≤1500 mg / L; a represents the actual optimal adsorption capacity of the adsorbent for the anions (in mg / g); the anions include fluoride ions and / or phosphate ions; optionally, 5 mg / g≤a≤200 mg / g).

[0052] The acid leaching process involved in the present invention may include an acid leaching step and a subsequent filtration step to remove solid precipitates insoluble in the leaching solution. The filtered solid precipitates are washed to produce graphite slag and a used washing solution, which can be recycled for slurrying of ternary lithium battery powder. Unless otherwise specified, the acid leaching solution prepared in step S1 may contain impurity ions such as F, P, Al, and Cu, as well as target ions such as Li, Ni, Co, and Mn.

[0053] According to the present invention, in step S2, the adsorption treatment conditions may include: an adsorption temperature of 40-80°C, an adsorption time of 0.5-2 hours, and a system pH of 3-6. Optionally, the adsorption treatment conditions also include: adding a pH adjuster during the adsorption treatment; the pH adjuster may include an inorganic base and / or an organic acid. Exemplarily, to avoid introducing new impurities or increasing the cost of subsequent alkali and / or acid washing, the inorganic base is preferably ammonia water, and the organic acid is preferably acetic acid.

[0054] During the adsorption treatment process of the present invention, the pH in the system needs to be controlled between 3 and 6. On the one hand, this can avoid the dissolution of the adsorbent caused by too low a pH, the dissolution of components in the adsorbent, and the failure to achieve the purpose of impurity removal; on the other hand, it can avoid the loss (precipitation) of transition metal elements, thereby increasing the cost of compounding.

[0055] The adsorption treatment in the present invention can remove fluorine and phosphorus elements on the one hand, and impurities such as Al and Cu on the other hand. For example, the reaction formula involved in the adsorption treatment is as follows:

[0056] R-OH+F / P→RF / P+OH -

[0057] [Al(NH3)4](CH3COO)3+3OH - →Al(OH)3↓+3CH3COONH4+NH3↑

[0058] [Cu(NH3)4](CH3COO)2+2OH - →Cu(OH)2↓+2CH3COONH4+2NH3↑

[0059] Unless otherwise specified, the adsorption process involved in the present invention may include an adsorption step and a subsequent filtration step. The present invention obtains a purified liquid and a used adsorbent through the adsorption and filtration steps. The purified liquid undergoes a subsequent purified liquid reconstitution process, and the used adsorbent can undergo an adsorbent regeneration process.

[0060] According to the present invention, the content of Li, Ni, Co, and Mn elements in the reconstituted solution in step S3 can be adjusted according to the target ternary cathode material to be regenerated. For example, the chemical formula of the target ternary cathode material is Li a Ni x Co y Mn 1-x-y O2 (0.9≤a≤1.2, x>0, y≥0, z≥0, and x+y+z=1). The adjustment process involved in the present invention can be: first, the concentrations of Li, Ni, Co, and Mn in the purified solution are tested, and according to the composition ratio of the target ternary positive electrode material, at least one of a lithium source, a nickel source, a cobalt source, and a manganese source is added to finally obtain a compound solution that matches the composition of the target ternary positive electrode material.

[0061] The lithium source, nickel source, cobalt source, and manganese source used in the present invention are well known to those skilled in the art. Preferably, to avoid the introduction of unnecessary impurities, the lithium source may be a salt of lithium corresponding to the acid; the nickel source may be a salt of nickel corresponding to the acid; the cobalt source may be a salt of cobalt corresponding to the acid; and the manganese source may be a salt of manganese corresponding to the acid, wherein the acid refers to the acid used in the acid leaching process.

[0062] In a preferred embodiment of the present invention, in step S3, the lithium source, the nickel source, the cobalt source and the manganese source are organic acid salts of lithium, nickel, cobalt and manganese, respectively. The use of organic acid salts in the present invention is conducive to recycling during spray drying, thereby reducing harm to the environment.

[0063] For example, the lithium source may be lithium acetate; the nickel source may be nickel acetate; the cobalt source may be cobalt acetate; and the manganese source may be manganese acetate.

[0064] In one embodiment of the present invention, the ratio of the amount of Li to the total amount of Ni, Co and Mn in the composite liquid can be 1.01-1.14:1; illustratively, the ratio of the amount of Ni, Co and Mn can be (0.53-0.93): (0.043-0.1): (0.016-0.28).

[0065] Optionally, in step S4, the spray drying conditions may include: an inlet temperature of 160 to 250°C, an outlet temperature of 80 to 100°C, an atomization pressure of 0.2 to 0.4 MPa, and a feed rate of 5 to 20 mL / min; in this step, the compound liquid is atomized into small droplets (including centrifugal atomization and two-fluid atomization), and water is rapidly evaporated at high temperature to form a lithium-containing ternary oxide intermediate.

[0066] The lithium-containing ternary oxide intermediate involved in the present invention can be a mixture of Li oxide, Ni oxide, Co oxide and Mn oxide, and the target single crystal ternary positive electrode material is obtained by sintering the mixture.

[0067] In one embodiment of the present invention, the sintering process includes: pre-sintering the intermediate to obtain a lithium-containing ternary oxide precursor; and sintering the precursor at high temperature. Pre-sintering facilitates the removal of residual moisture from the particles, which is conducive to the slow growth and formation of the particle crystal form. The pre-sintering conditions may include: a heating rate of 2-6°C / min, a pre-sintering temperature of 400-550°C, and a pre-sintering time of 4-8 hours. Through pre-sintering, the mixed salts are further dried and decomposed to form a lithium-containing ternary oxide precursor. The high-temperature sintering conditions may include: a heating rate of 2-5°C / min, a sintering temperature of 800-950°C, and a sintering time of 4-8 hours. The protective gas for high-temperature sintering is any one of air, oxygen, nitrogen, argon, or helium, or a combination of at least two. For example, if the target product is a 5-6 series cathode, the protective gas for high-temperature sintering can be air; if the target product is a 7 series or higher cathode, the protective gas for high-temperature sintering can be air or oxygen, preferably oxygen.

[0068] Optionally, the battery powder to be processed includes ternary lithium battery powder.

[0069] For example, the battery powder to be processed in the present invention is a mixed powder or positive electrode powder obtained by crushing and pre-processing waste ternary lithium batteries or waste ternary lithium battery positive electrode sheets. The slurry containing the battery powder to be processed in the present invention can be a slurry obtained by mixing the battery powder to be processed with water.

[0070] As a preferred embodiment of the present invention, the method may further include: regenerating the used adsorbent to obtain a regenerated adsorbent; mixing the regenerated adsorbent with the acid leaching solution and then performing the adsorption treatment; wherein the regeneration treatment may include: performing a first rinsing on the used adsorbent to obtain a rinsing adsorbent; mixing the rinsing adsorbent with an alkaline solution to obtain a regenerated mixed solution; and vacuum filtering and performing a second rinsing on the regenerated mixed solution. wherein, the adsorption treatment after the regenerated adsorbent is mixed with the acid leaching solution requires attention to controlling the pH value in the system to be 3 to 6.

[0071] Illustratively, the washing liquid of the first rinse may include water; the alkaline solution may include aqueous ammonia; the pH of the regeneration mixed solution may be 10-12; and the washing liquid of the second rinse may include water.

[0072] The method of the present invention generates regeneration filtrate wastewater (containing F and Al) during the adsorbent regeneration process, and the wastewater can be further used for the synthesis of cryolite (Na3AlF6).

[0073] As a preferred embodiment of the present invention, the method may further include: collecting the acid waste gas generated by the spray drying; and dissolving the acid waste gas in a solvent and mixing it with the reducing agent, and adding the solvent as the leaching liquid to step S1.

[0074] A second aspect of the present invention provides a single crystal ternary cathode material, which is prepared by the above method.

[0075] The present invention is further described in detail below by way of examples. The raw materials used in the examples can all be obtained through commercial sources.

[0076] Example 1

[0077] The mass content (%) of each element in the waste ternary powder (obtained by crushing and sieving the positive electrode sheet) used in this embodiment is shown in Table 1, wherein the waste ternary powder is Ni of the scrapped 5 series battery cell. 0.55 Co 0.15 Mn 0.3 Ternary positive electrode.

[0078] Table 1

[0079] Li Ni Co Mn Al Cu F P 6.59 29.97 8.26 15.26 1.2 0.04 1.7 0.16

[0080] The method of synthesizing a single crystal ternary cathode material from ternary waste lithium battery materials in this embodiment specifically includes:

[0081] (1) Leaching: The scrapped ternary battery cells are subjected to appropriate pretreatment to obtain a lithium nickel cobalt manganese black powder material (as shown in Table 1), which is added to water and stirred to prepare a slurry, and then pumped into a reaction tank. 3 mol / L acetic acid and 8 wt% of the effective ingredient hydrogen peroxide are added, and the solid-liquid ratio is 50 g / L. The reaction is stirred at 80°C for 3 h, and the pH in the system is controlled to be 1.5-4. After the reaction is completed, the filtrate is filtered and separated to obtain a primary filtrate. The filtrate contains elements such as lithium, nickel, cobalt, manganese, aluminum, copper, fluorine and phosphorus, and the leaching rate of each main metal is above 98%.

[0082] (2) Adsorption: 10 wt% ammonia water is added to the primary filtrate of step (1), and the pH of the solution is adjusted to 4. Then, a zirconium-titanium adsorbent is added to the mixed solution at a solid-liquid ratio of 10 g / L, and the mixture is stirred at 45°C for 1 hour. The pH of the process is controlled between 4 and 6. After the reaction, the solid-liquid separation is performed by filtration to obtain a secondary purified filtrate and a primary filter residue. The impurity elements such as aluminum, copper, fluorine and phosphorus in the purified liquid are all less than 2 ppm, achieving the goal of deep synchronous impurity removal. The primary filter residue can be regenerated and recycled.

[0083] (3) Regeneration: The filter residue in step (2) is first rinsed with an appropriate amount of pure water. After washing, the adsorbent ZrO2 is poured into a reactor and an appropriate amount of dilute alkaline water is added. At room temperature and a stirring speed of 300 rpm, the pH is adjusted with a 3% ammonia solution to control the end point pH to 10-12, and the reaction is carried out for 0.5 h. After vacuum filtration, the filter residue is rinsed with an appropriate amount of water to obtain the regenerated adsorbent ZrO2, which is then returned to step (2) to continue adsorption and impurity removal.

[0084] (4) Compounding: Take the purified solution in step (2) and compound the main metals according to the target product single crystal 5 series. Add nickel acetate, cobalt acetate and manganese acetate according to the molar ratio of Li: (Ni + Co + Mn) in the purified mixed solution of 1.05:1 (0.55:0.15:0.3) to obtain a compounded liquid, mix well and spray dry.

[0085] (5) Drying: The compounded liquid of step (4) is pumped into a stirred kettle at 50-80°C while being stirred and spray-dried, centrifugally atomized into small droplets, and atomized at an atomization pressure of 0.2 MPa, an air inlet temperature of 220°C, and an air outlet temperature of 110°C to obtain a lithium-containing ternary oxide intermediate. The SEM image of the lithium-containing ternary oxide intermediate is as follows: Figure 2 The equipment is provided with a drying process evaporation material recovery pipeline to collect the waste gas, which is then used in step (1).

[0086] (6) Sintering treatment: The intermediate is transferred to an atmosphere furnace and pre-sintered at a heating rate of 4°C / min to 500°C in an air atmosphere. The temperature is maintained for 3 hours. The mixed salts are further dried and decomposed to form a lithium oxide precursor. In an air atmosphere, the pre-sintered lithium oxide precursor is uniformly heated to 900°C at a heating rate of 5°C / min and sintered at high temperature for 12 hours to obtain a regenerated single crystal ternary cathode material. The SEM image of the regenerated single crystal ternary cathode material is shown in FIG. Figure 3 As shown, through Figure 3 It can be seen that the regenerated single crystal ternary cathode material prepared in this embodiment is in the form of single crystal particles, and the particle surface is smooth and the layered structure is obvious. The composition of the regenerated single crystal ternary cathode material prepared in this embodiment is compared with the commercially available single crystal ternary cathode material. Figure 4 ,pass Figure 4 It can be seen that the composition of the regenerated single crystal ternary cathode material prepared in this embodiment is consistent with that of the commercially available single crystal ternary cathode material.

[0087] Example 2

[0088] The mass content (%) of each element in the waste ternary powder used in this embodiment (obtained by dismantling the scrapped battery cells of 1000 cycles of Xunhua) is shown in Table 2, where the waste ternary powder is the scrapped retired battery cells.

[0089] Table 2

[0090] Li Ni Co Mn Al Cu F P C 6.04 34.71 4.10 11.47 0.83 0.08 1.03 0.11 13.04

[0091] The method of synthesizing a single crystal ternary cathode material from ternary waste lithium battery materials in this embodiment specifically includes:

[0092] (1) Leaching: The scrapped ternary battery cells were properly pretreated to obtain a mixed black powder material containing lithium, nickel, cobalt and manganese (as shown in Table 2), which was added to water and stirred to prepare a slurry, and then pumped into a reaction tank. 4 mol / L acetic acid and 10 wt% of the effective ingredient hydrogen peroxide were added, and the solid-liquid ratio was 60 g / L. The mixture was stirred at 85 ° C for 3 h, and the pH in the system was controlled to be 1.5-3. After the reaction was completed, the mixture was filtered and separated to obtain a primary filtrate. The filtrate contained elements such as lithium, nickel, cobalt, manganese, aluminum, copper, fluorine and phosphorus, and the leaching rate of each main metal was above 98%.

[0093] (2) Impurity removal: 10 wt% ammonia water is added to the primary filtrate of step (1), and the pH of the solution is adjusted to 5. Then, a zirconium-titanium adsorbent is added to the mixed solution at a solid-liquid ratio of 15 g / L, and the mixture is stirred at 45°C for 1 hour. The pH of the process is controlled between 4 and 6. After the reaction, the secondary purified filtrate and the primary filter residue are obtained by filtration and solid-liquid separation. The impurity elements aluminum are less than 3 ppm, copper is less than 3 ppm, and fluorine and phosphorus are less than 1 ppm, thereby achieving the goal of deep synchronous impurity removal. The primary filter residue can be regenerated and recycled.

[0094] (3) Regeneration: The filter residue in step (2) is first rinsed with an appropriate amount of pure water. The washed adsorbent is poured into a reactor and an appropriate amount of dilute alkaline water is added. Under normal temperature and stirring speed of 300 rpm, the pH is adjusted with % ammonia solution to control the end point pH to 1, and the reaction is carried out for 0.5 h. After vacuum filtration, the filter residue is rinsed with an appropriate amount of water to obtain the regenerated adsorbent, which is then returned to step (2) to continue adsorption and impurity removal.

[0095] (4) Compounding: Take the purified solution in step (2) and compound the main metals according to the target product single crystal 7 series. The amount of each main metal in the purified mixed solution is based on the molar ratio of Li: (Ni + Co + Mn) of 1.01:1 (0.68:0.08:0.24). Nickel acetate, cobalt acetate and manganese acetate are added to obtain a compound liquid, which is mixed evenly and spray-dried.

[0096] (5) Drying: The compounded solution from step (4) is pumped into a stirred kettle at 50-80°C while being stirred and passed through a spray drying apparatus for centrifugal atomization into small droplets. The atomization pressure is 0.2 MPa, the air inlet temperature is 220°C, and the air outlet temperature is 110°C to obtain a lithium-containing intermediate. The equipment is provided with a pipeline for recovering the evaporated material during the drying process to collect the waste gas for reuse in step (1).

[0097] (6) Sintering treatment: The intermediate is transferred to an atmosphere furnace and pre-sintered at a heating rate of 4°C / min to 500°C in an oxygen atmosphere. The temperature is maintained for 3 hours. The mixed salts are further dried and decomposed to form a lithium oxide precursor. In an oxygen atmosphere, the pre-sintered lithium oxide precursor is uniformly heated to 950°C at a heating rate of 5°C / min and sintered at high temperature for 12 hours to obtain a regenerated single crystal ternary cathode material. The SEM image of the regenerated single crystal ternary cathode material is shown in FIG. Figure 5 As shown, through Figure 5 It can be seen that the regenerated single-crystal ternary cathode material prepared in this embodiment is in the form of single-crystal particles, and the particle surface is smooth and the layered structure is obvious.

[0098] Example 3

[0099] The waste ternary powder used in this embodiment is the same as that in Example 1.

[0100] The method of synthesizing a single crystal ternary cathode material from ternary waste lithium battery materials in this embodiment specifically includes:

[0101] (1) Leaching: The scrapped ternary battery cells are appropriately pretreated to obtain a material containing lithium nickel cobalt manganese black powder (as shown in Table 1), which is added to water and stirred to prepare a slurry, and then pumped into a reaction tank. 3 mol / L acetic acid and 8 wt% of the effective ingredient hydrogen peroxide are added, and the solid-liquid ratio is 80 g / L. The reaction is stirred at 80°C for 3 h, and the pH in the system is controlled to be 1.5-4. After the reaction is completed, the material is filtered and separated to obtain a primary filtrate. The filtrate contains elements such as lithium, nickel, cobalt, manganese, aluminum, copper, fluorine and phosphorus, and the leaching rate of each main metal is above 99%.

[0102] (2) Adsorption: 8 wt% ammonia water is added to the primary filtrate of step (1), and the pH of the solution is adjusted to 4.5. Then, a zirconium-titanium adsorbent is added to the mixed solution at a solid-liquid ratio of 15 g / L, and the reaction is stirred at 45°C for 1.5. The pH of the process is controlled between 4 and 6. After the end, the secondary purified filtrate and the primary filter residue are obtained by filtration and solid-liquid separation. The impurity elements such as aluminum, copper, fluorine and phosphorus in the purified liquid are all less than 2 ppm, achieving the goal of deep synchronous impurity removal. The primary filter residue can be regenerated and recycled.

[0103] (3) Regeneration: The filter residue in step (2) is first rinsed with an appropriate amount of pure water. After washing, the adsorbent ZrO2 is poured into the reactor and an appropriate amount of dilute alkaline water is added. At room temperature and a stirring speed of 300 rpm, the pH is adjusted with a 4% ammonia solution to control the end point pH to 10-11, and the reaction is carried out for 0.5 h. After vacuum filtration, the filter residue is rinsed with an appropriate amount of water to obtain the regenerated adsorbent ZrO2, which is then returned to step (2) to continue adsorption and impurity removal.

[0104] (4) Compounding: Take the purified solution in step (2) and compound the main metals according to the target product single crystal 5 series. Add nickel acetate, cobalt acetate and manganese acetate according to the molar ratio of Li: (Ni + Co + Mn) in the purified mixed solution of 1.05:1 (0.55:0.15:0.3) to obtain a compounded liquid, mix well and spray dry.

[0105] (5) Drying: The compounded solution from step (4) is pumped into a stirred tank at 45°C while being stirred and spray-dried, where it is centrifugally atomized into small droplets. The atomization pressure is 0.2 MPa, the air inlet temperature is 200°C, and the air outlet temperature is 105°C to obtain a lithium-containing intermediate. A pipeline for recovering evaporated substances during the drying process is provided within the equipment to collect the waste gas for reuse in step (1).

[0106] (6) Sintering treatment: The intermediate is transferred to an atmosphere furnace and pre-sintered at a heating rate of 5°C / min to 550°C in an air atmosphere. The temperature is maintained for 4 hours. The mixed salts are further dried and decomposed to form a lithium oxide precursor. In an air atmosphere, the pre-sintered lithium oxide precursor is uniformly heated to 950°C at a heating rate of 4°C / min and sintered at high temperature for 15 hours to obtain a regenerated single crystal ternary cathode material. The SEM image of the regenerated single crystal ternary cathode material is shown in FIG. Figure 6 As shown, through Figure 6 It can be seen that the regenerated single-crystal ternary cathode material prepared in this embodiment is in the form of single-crystal particles, and the particle surface is smooth and the layered structure is obvious.

[0107] Example 4

[0108] The regeneration method of the waste ternary lithium battery in this embodiment is the same as that in Example 1, except that: in this embodiment, the lithium-containing intermediate is not pre-sintered, and the temperature is directly raised to 900°C at a heating rate of 5°C / min and kept at this temperature for 12 hours. The regenerated single crystal ternary positive electrode material prepared in this embodiment has a SEM image as shown in FIG. Figure 7 As shown, through Figure 7 It can be seen that the regenerated single-crystal ternary cathode material prepared in this embodiment is in the form of single-crystal particles, but nano primary particles are attached to the surface of the particles and there are cracks on the surface.

[0109] Comparative Example 1

[0110] The lithium nickel cobalt manganese black powder material used in Example 1 was added to water, stirred and slurried, and then pumped into a reaction tank. 3 mol / L acetic acid was added, and the solid-liquid ratio was 50 g / L. The reaction was stirred at 80°C for 3 hours, and the pH in the system was controlled to be 1.5-4. After the reaction was completed, the mixture was filtered and separated to obtain a primary filtrate.

[0111] Comparative Example 2

[0112] (1) Leaching: The lithium nickel cobalt manganese black powder material used in Example 1 was added to water, stirred and slurried, and then pumped into a reaction tank. 3 mol / L acetic acid and 8 wt% of the effective ingredient hydrogen peroxide were added, and the solid-liquid ratio was 50 g / L. The mixture was stirred and reacted at 80°C for 3 h. The pH in the system was controlled to be 1.5-4. After the reaction was completed, the mixture was filtered and separated to obtain a primary filtrate. The filtrate contained elements such as lithium, nickel, cobalt, manganese, aluminum, copper, fluorine and phosphorus, and the leaching rate of each main metal was above 98%.

[0113] (2) Adsorption: 10 wt% ammonia water was added to the primary filtrate of step (1), and the pH of the solution was adjusted to 4. Then, activated alumina as an adsorbent was added to the mixture at a solid-liquid ratio of 10 g / L. The mixture was stirred at 45°C for 1 hour, and the pH of the process was controlled between 4 and 6. After the reaction was completed, the solid-liquid separation was performed by filtration to obtain a secondary purified filtrate and a primary filter residue.

[0114] Test Example 1

[0115] The elements in the regenerated ternary cathode materials prepared in Examples 1 to 4 were analyzed, and the analysis results are shown in Table 3. The leaching rate of the primary filtrate and the impurity element content in the secondary purified filtrate in Example 1 were tested, and the test results are shown in Table 4. The leaching rate of the primary filtrate in Comparative Example 1 and the impurity element content in the secondary purified filtrate in Comparative Example 2 were tested, and the test results are shown in Table 4.

[0116] Table 3

[0117]

[0118] Table 4

[0119]

[0120] It can be seen from Table 3 that the molar ratio of Li, Ni, Co and Mn in the regenerated single crystal ternary positive electrode material prepared by the method of the present invention meets the standard of ternary positive electrode material, and the impurities Al, Cu and F contained are relatively low.

[0121] It can be seen from Table 4 that in Comparative Example 1, no reducing agent is added to the acid leaching solution, and the leaching efficiency of the main metal elements is greatly reduced; in Comparative Document 2, activated alumina is used as an adsorbent, which introduces new impurities (S\Al) into the system, thereby increasing the recovery cost.

[0122] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A method for regenerating a single crystal ternary cathode material, characterized in that: The method comprises the following steps: S1, mixing the slurry containing the battery powder to be processed with the leaching solution and performing acid leaching treatment to obtain an acid leaching solution; S2, mixing the acid leaching solution with an adsorbent and performing adsorption treatment to obtain a purified solution and a used adsorbent; S3, adjusting the molar ratio of Li, Ni, Co and Mn in the purified solution to be consistent with the ratio of each metal in the target ternary positive electrode material to obtain a composite solution; S4, spray drying the composite liquid to obtain a lithium-containing ternary oxide intermediate; sintering the lithium-containing ternary oxide intermediate; Wherein, the leaching solution comprises a reducing agent and an acid; and the adsorbent comprises a supported porous oxide.

2. The regeneration method according to claim 1, characterized in that: In step S1, the reducing agent includes at least one of hydrogen peroxide, sodium sulfite, glucose and ascorbic acid; the acid includes an organic acid; Optionally, the reducing agent includes hydrogen peroxide; the acid includes acetic acid; and / or, based on the total mass of the leaching solution, the mass fraction of the reducing agent is 5 to 10 wt %; And / or, the solid-to-liquid ratio of the acid leaching treatment is 40 to 100 g / L; And / or, the conditions of the acid leaching treatment include: the acid leaching temperature is 50-95° C., the acid leaching time is 1-4 hours, and the pH in the system is 1.5-4.

3. The regeneration method according to claim 1, characterized in that: In step S2, the supported porous oxide includes ZrO2 and / or TiO2; and / or, the amount of the adsorbent per liter of the acid leaching solution satisfies the formula Y=X / a (wherein X represents the mass concentration of anions in the acid leaching solution; a represents the actual optimal adsorption capacity of the adsorbent for the anions; the anions include fluoride ions and / or phosphate ions); And / or, the conditions of the adsorption treatment include: the adsorption temperature is 40-80°C, the adsorption time is 0.3-2h, and the pH in the system is 3-6; Optionally, the conditions of the adsorption treatment further include: adding a pH adjuster during the adsorption treatment; optionally, the pH adjuster includes an inorganic base and / or an organic acid.

4. The regeneration method according to claim 1, characterized in that: In step S3, in the composite solution, the ratio of the amount of Li to the total amount of Ni, Co and Mn is 1.01-1.14:1; The molar ratio of Ni, Co and Mn is (0.53~0.93):(0.043~0.1):(0.016~0.28).

5. The regeneration method according to claim 1, characterized in that: In step S4, the spray drying conditions include: inlet temperature of 160-250°C, outlet temperature of 80-100°C, atomization pressure of 0.2-0.4MPa, and feed rate of 5-20mL / min; The sintering process includes: pre-sintering the lithium-containing ternary oxide intermediate to obtain a lithium-containing ternary oxide precursor; sintering the lithium-containing ternary oxide precursor at a high temperature; Among them, the pre-sintering conditions include: a heating rate of 2 to 6°C / min, a pre-sintering temperature of 400 to 550°C, and a pre-sintering time of 4 to 8h; the high-temperature sintering conditions include: a heating rate of 2 to 5°C / min, a sintering temperature of 800 to 950°C, and a sintering time of 4 to 8h.

6. The regeneration method according to claim 1, characterized in that: The battery powder to be processed includes ternary lithium battery powder.

7. The regeneration method according to claim 1, characterized in that: The method further comprises: regenerating the used adsorbent to obtain a regenerated adsorbent; mixing the regenerated adsorbent with the acid leaching solution and then performing the adsorption treatment; The regeneration process comprises: subjecting the used adsorbent to a first elution to obtain a eluted adsorbent; mixing the eluted adsorbent with an alkali solution to obtain a regenerated mixed solution; and vacuum filtering and second elution the regenerated mixed solution.

8. The regeneration method according to claim 7, characterized in that: The washing liquid of the first rinse comprises water; The alkaline solution includes ammonia water; the pH of the regeneration mixed solution is 10 to 12; The washing liquid of the second rinse liquid includes water.

9. The regeneration method according to claim 1, characterized in that: The method further comprises: collecting the acid waste gas generated by the spray drying; and dissolving the acid waste gas in a solvent and mixing it with the reducing agent, and adding the solvent as the leaching solution into step S1.