Composite diaphragm, preparation method thereof and battery
By using a composite coating prepared by solid electrolyte and SiO2 aerogel particles on the lithium-ion battery separator, the problems of low conductivity and interface instability of the existing separator coating are solved, and the conductivity and high temperature resistance of the battery are improved. Achieve more stable battery performance and low-cost production.
Patent Information
- Application Number
- CN202411025763.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
The existing lithium-ion battery separator coatings have problems such as low ion conductivity and unstable interface, and the processing equipment is large and the cost is high.
A composite coating combining solid electrolyte particles and SiO2 aerogel particles is prepared by sol-gel method and in-situ loading method to form a solid electrolyte/SiO2 aerogel composite material, and is coated on the surface of the membrane to improve the coating. structural uniformity and stability.
It significantly improves the total ionic conductivity, breathability and high temperature resistance of the battery, reduces the internal resistance of the battery's charging and discharge, improves the long-term cycle stability and high temperature performance, and has a simple process and low cost, which is suitable for industrial production.
Smart Images

Figure CN118943656A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of new energy batteries, and in particular to a composite diaphragm, a preparation method thereof, and a battery. Background Art
[0002] With the development of 3C products such as mobile phones, digital cameras, and laptops, as well as the demand for high-power system products such as electric vehicles and hybrid vehicles, lithium-ion batteries (LIBs) have become the most commonly used energy storage devices due to their relatively high energy density, high rate capability, and safety. The diaphragm in LIBs plays an important role in preventing short circuits between the cathode and the anode, and provides porous channels for lithium ion transmission between the two electrodes. Polyester film, polyethylene diaphragm, and polypropylene diaphragm are commonly used diaphragms in LIBs, but they are limited by electrolyte absorption and poor thermal stability. The poor thermal stability of the diaphragm causes serious safety issues for the battery at high temperatures, especially safety issues such as breakdown during high-power discharge. To solve this problem, from the perspective of comprehensively improving the thermal stability and high-temperature resistance of the diaphragm, a high-temperature resistant coating such as Al2O3 and boehmite is coated on the surface of the diaphragm. However, the existing diaphragm coatings have problems such as low ion conductivity and unstable interface. At the same time, there are disadvantages such as large equipment loss and high cost during processing. Therefore, a production technology for diaphragm coatings that solves the above problems is urgently needed. Summary of the invention
[0003] In view of this, the present invention is committed to providing a composite diaphragm and its preparation method and battery to solve the problems of low ion conductivity and unstable interface of the diaphragm coating in the prior art, as well as the disadvantages of large equipment loss and high cost during processing.
[0004] In order to solve the above technical problems, this application is implemented as follows:
[0005] A first aspect of the present invention provides a composite diaphragm, the composite diaphragm comprising a base film and a coating disposed on the surface of the base film, the coating containing solid electrolyte particles and SiO2 aerogel particles;
[0006] Wherein, at least part of the solid electrolyte particles are distributed in the pores of the SiO2 aerogel particles to form solid electrolyte / SiO2 aerogel composite particles.
[0007] Optionally, the particle size D50 of the solid electrolyte / SiO2 aerogel composite particles is 500-800nm, preferably 600-700nm; optionally, the pore size of the solid electrolyte / SiO2 aerogel composite particles is 2-15nm, preferably 8-10nm; optionally, based on the total mass of the solid electrolyte particles and the SiO2 aerogel particles, the mass fraction of the SiO2 aerogel particles is 80-90wt%, preferably 84-86wt%.
[0008] Optionally, the particle size D50 of the solid electrolyte particles is 10 to 80 nm; preferably, the particle size D50 of the solid electrolyte particles is 40 to 50 nm; optionally, the solid electrolyte particles are selected from at least one of lithium aluminum titanium phosphate solid electrolyte particles, lithium lanthanum titanium oxide solid electrolyte particles and lithium lanthanum zirconium oxide solid electrolyte particles; preferably, the solid electrolyte particles are lithium aluminum titanium phosphate solid electrolyte particles.
[0009] Optionally, the coating also contains a binder; preferably, the mass ratio of the total mass of the solid electrolyte particles and the SiO2 aerogel particles to the binder is 1:(0.02-0.16), preferably 1:(0.05-0.1); preferably, the binder is selected from at least one of acrylate binders, polytetrafluoroethylene, polyvinylidene fluoride, polyacrylonitrile and polyvinyl alcohol; preferably, the acrylate binder is selected from at least one of acrylates, cyanoacrylates and diester acrylates.
[0010] Optionally, the porosity of the composite membrane is 40-60%, preferably 50-55%.
[0011] Optionally, the base film has a thickness of 7 to 9 μm and a porosity of 35 to 45%; optionally, the base film is made of one of polyester, polyethylene and polypropylene.
[0012] A second aspect of the present invention provides a method for preparing the above-mentioned composite membrane, the method comprising the following steps:
[0013] S1, dispersing solid electrolyte particles in a first solvent to obtain a solid electrolyte suspension; dispersing an inorganic silicon source in a second solvent to obtain a first material; adding a dilute acid solution to the first material for stirring to obtain a silica sol; mixing the silica sol with the solid electrolyte suspension to obtain a solid electrolyte / silica sol composite sol;
[0014] S2, subjecting the solid electrolyte / silica sol composite sol to gel treatment and drying treatment to obtain a composite material precursor; subjecting the composite material precursor to heat treatment to obtain a composite material containing a solid electrolyte and SiO2 aerogel; subjecting the composite material containing a solid electrolyte and SiO2 aerogel to grinding treatment to obtain first particles; wherein the first particles include solid electrolyte / SiO2 aerogel composite particles;
[0015] S3, dispersing the solid electrolyte / SiO2 aerogel composite particles in a third solvent to obtain a diaphragm slurry; coating the diaphragm slurry on the surface of the base film and performing a baking treatment.
[0016] Optionally, a binder is also dispersed in the third solvent; preferably, the binder is selected from at least one of acrylate binders, polytetrafluoroethylene, polyvinylidene fluoride, polyacrylonitrile and polyvinyl alcohol; preferably, the acrylate binder is selected from at least one of acrylates, cyanoacrylates and diester acrylates.
[0017] Optionally, based on the total mass of the solid electrolyte suspension, the mass fraction of the solid electrolyte particles is 4-10%, preferably 5-8%; and / or, based on the total volume of the first material, the volume fraction of the inorganic silicon source is 15-40%, preferably 20-30%; and / or, the molar concentration of the dilute acid solution is 1-2 mol / L; and / or, based on the total volume of the silica sol, the volume fraction of the dilute acid solution is 0.5-0.8%, preferably 0.6-0.7%; and / or, the mixing ratio of the silica sol and the solid electrolyte suspension is 4-5:1; and / or, the mass fraction of the first particles contained in the diaphragm slurry is 25-45%, preferably 30-40%.
[0018] Optionally, the inorganic silicon source is selected from silicon tetrachloride and / or water glass; optionally, the dilute acid solution is selected from at least one of dilute hydrochloric acid, dilute nitric acid and dilute sulfuric acid; optionally, the first solvent, the second solvent and the third solvent are water.
[0019] Optionally, in step S1, the rate of dripping the dilute acid solution is 0.8-1.2 mL / min; and / or, in step S2, the conditions for the gel treatment include: a temperature of 30-50°C and a time of 3-6 h; and / or, the conditions for the drying treatment include: a pressure of 0.001-0.1013 MPa, a temperature of 60-80°C, a time of 24-48 h, and an air flow rate of 1-1.5 m / s; and / or, the heat treatment is carried out in an oxygen atmosphere; the conditions for the heat treatment include: a temperature of 600-800°C, a time of 1-2 h, and a heating rate of 5-10°C / min; and / or, in step S3, the conditions for the baking treatment include: a temperature of 40-50°C, a time of 20-30 min, and an air flow rate in the baking equipment of 2-2.5 m / s.
[0020] A third aspect of the present invention provides a battery, comprising the composite diaphragm described above, and / or the composite diaphragm prepared according to the method described above.
[0021] Through the above technical solution, the beneficial technical effects of the present invention are:
[0022] 1. In the present invention, an inorganic silicon source and a solid electrolyte are used, and a sol-gel method and an in-situ loading method are adopted to prepare a solid electrolyte / SiO2 gel, and a solid electrolyte / SiO2 aerogel composite material is obtained after normal pressure drying and heat treatment. The composite material is crushed and coated on both sides of the diaphragm, and a composite diaphragm is obtained after drying. Compared with similar diaphragm coating materials, the coating material prepared by the present invention has excellent performance, uniform structure, good stability, low cost, and is easy to realize industrial production.
[0023] 2. In the present invention, the small amount of secondary phase LiTiOPO4 generated by SiO2-induced lithium aluminum titanium phosphate solid electrolyte after high temperature heat treatment can adjust the microstructure morphology of the material, improve grain boundary ion transport, and thus improve the total ion conductivity of the battery. The porous structure of SiO2 aerogel can improve the permeability and high temperature resistance of the diaphragm.
[0024] 3. The solid electrolyte / SiO2 aerogel coating prepared by the present invention is more uniform and stable, and the peel strength between the coating and the base film is improved, which can effectively reduce the charging internal resistance and discharging internal resistance of the battery and improve the long-term cyclability and high-temperature performance of the battery.
[0025] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:
[0027] Figure 1 Shown is a SEM image of the composite membrane prepared in Example 1.
[0028] Figure 2 Shown is a schematic structural diagram of the composite diaphragm prepared in Example 1. DETAILED DESCRIPTION
[0029] The present invention discloses a composite diaphragm and a method for preparing the same and a battery. Those skilled in the art can refer to the contents of this article and appropriately improve the process parameters to achieve the same. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art and are deemed to be included in the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
[0030] In the description of the present invention, a list of items connected by the term "at least one of" or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.
[0031] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range or the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0032] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0033] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0034] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0035] In order to solve the problems of low ion conductivity and unstable interface of the diaphragm coating in the prior art, as well as the problems of large equipment loss and high cost during processing, the present invention adopts the following technical solution:
[0036] A first aspect of the present invention provides a composite diaphragm, the composite diaphragm comprising a base film and a coating disposed on the surface of the base film, the coating containing solid electrolyte particles and SiO2 aerogel particles;
[0037] Wherein, at least part of the solid electrolyte particles are distributed in the pores of the SiO2 aerogel particles to form solid electrolyte / SiO2 aerogel composite particles.
[0038] The composite diaphragm of the present invention comprises a base film and a coating disposed on the surface of the base film, wherein the coating contains solid electrolyte particles and SiO2 aerogel particles, wherein at least part of the solid electrolyte particles are distributed in the pores of the SiO2 aerogel particles to form solid electrolyte / SiO2 aerogel composite particles. For example, some of the solid electrolyte particles with smaller particle sizes are distributed in the pores of the SiO2 aerogel particles to form solid electrolyte / SiO2 aerogel composite particles; some of the solid electrolyte particles with larger particle sizes are distributed between the SiO2 aerogel particles to form mixed particles. The porous structure of the SiO2 aerogel in the present invention can improve the overall air permeability, liquid retention, and high temperature resistance of the diaphragm. At the same time, the composite diaphragm of the present invention has good high temperature dimensional stability, flame retardancy and mechanical properties, and can be free of perforation at high power. Compared with conventional diaphragms, the composite diaphragm structure of the present invention is more uniform and stable, which is beneficial to the high power performance of the battery such as long-term cycle stability and high temperature performance.
[0039] According to the present invention, in order to ensure the uniformity of distribution in the composite diaphragm, and to avoid the problems of easy falling off, poor thermal insulation and thermal conductivity due to excessive particle size, and preparation cost due to too small particle size, the particle size D50 of the solid electrolyte / SiO2 aerogel composite particles can be 500-800nm. Exemplarily, the particle size D50 of the solid electrolyte / SiO2 aerogel composite particles can be any value among 500nm, 550nm, 600nm, 650nm, 700nm, 750nm and 800nm, or any value within the range of any two of the above values. Preferably, the particle size D50 of the solid electrolyte / SiO2 aerogel composite particles can be 600-700nm.
[0040] According to the present invention, the solid electrolyte / SiO2 aerogel composite particles have a certain number of mesopores, and the mesoporous structure in the solid electrolyte / SiO2 aerogel composite particles can improve the air permeability, liquid retention, and high temperature resistance of the diaphragm. Optionally, the pore size of the solid electrolyte / SiO2 aerogel composite particles can be 2 to 15 nm. Exemplarily, the pore size of the solid electrolyte / SiO2 aerogel composite particles can be any value among 2nm, 4nm, 6nm, 8nm, 10nm, 12nm and 15nm or any value within the range of any two of the above values. Preferably, the pore size of the solid electrolyte / SiO2 aerogel composite particles can be 8 to 10nm.
[0041] According to the present invention, the appropriate ratio of SiO2 aerogel particles and solid electrolyte particles in the coating can further improve the stability of the composite diaphragm, which is beneficial to the long-term cycle stability of the battery. Optionally, based on the total mass of the solid electrolyte particles and the SiO2 aerogel particles, the mass fraction of the SiO2 aerogel particles can be 80-90wt%. Exemplarily, the mass fraction of the SiO2 aerogel particles can be any value among 80wt%, 82wt%, 84wt%, 86wt%, 88wt% and 90wt% or any value within the range of any two of the above values. Preferably, the mass fraction of the SiO2 aerogel particles can be 84-86wt%.
[0042] According to the present invention, the particle size D50 of the solid electrolyte particles can be 10 to 80 nm. Among them, some solid electrolyte particles with smaller particle sizes can be distributed in the pores of the SiO2 aerogel particles to form solid electrolyte / SiO2 aerogel composite particles; some solid electrolyte particles with larger particle sizes can be distributed between the SiO2 aerogel particles to form mixed particles. Exemplarily, the particle size D50 of the solid electrolyte particles can be any value among 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm and 80nm or any value within the range of any two of the above values. Preferably, the particle size D50 of the solid electrolyte particles can be 40 to 50nm.
[0043] The solid electrolyte particles used in the present invention may be well known in the art. Preferably, the solid electrolyte particles may be selected from at least one of lithium titanium aluminum phosphate solid electrolyte particles, lithium lanthanum titanium oxide solid electrolyte particles and lithium lanthanum zirconium oxide solid electrolyte particles; further preferably, the solid electrolyte particles are lithium titanium aluminum phosphate solid electrolyte particles.
[0044] In one embodiment of the present invention, in order to make the coating layer more tightly bonded to the surface of the base film, the coating layer may also contain a binder. Preferably, the mass ratio of the total mass of the solid electrolyte particles and the SiO2 aerogel particles to the binder may be 1:(0.02-0.16). Exemplarily, the mass ratio of the total mass of the solid electrolyte particles and the SiO2 aerogel particles to the binder may be any of 1:0.02, 1:0.04, 1:0.06, 1:0.08, 1:0.10, 1:0.12, 1:0.14 and 1:0.16 or any value within the range of any two of the above values. Further preferably, the mass ratio of the total mass of the solid electrolyte particles and the SiO2 aerogel particles to the binder may be 1:(0.05-0.1).
[0045] The binder in the present invention can be selected from at least one of acrylate binders, polytetrafluoroethylene, polyvinylidene fluoride, polyacrylonitrile and polyvinyl alcohol; preferably, the acrylate binder can be selected from at least one of acrylate, cyanoacrylate and diester acrylate.
[0046] According to the present invention, the porosity of the composite membrane may be 40-60%. Exemplarily, the porosity of the composite membrane may be any value among 40%, 42%, 44%, 46%, 48%, 50%, 52%, 54%, 56%, 58% and 60%, or any value within the range of any two of the above values. Preferably, the porosity of the composite membrane may be 50-55%.
[0047] According to the present invention, the thickness of the base film may be 7 to 9 μm. Exemplarily, the thickness of the base film may be any value among 7 μm, 7.5 μm, 8 μm, 8.5 μm and 9 μm, or any value within the range of any two of the above values. The porosity of the base film in the present invention may be 35 to 45%; Exemplarily, the porosity of the base film may be any value among 35%, 37.5%, 40%, 42.5% and 45%, or any value within the range of any two of the above values.
[0048] Illustratively, the material of the base film may include one of polyester, polyethylene and polypropylene.
[0049] A second aspect of the present invention provides a method for preparing the above-mentioned composite membrane, the method comprising the following steps:
[0050] S1, dispersing solid electrolyte particles in a first solvent to obtain a solid electrolyte suspension; dispersing an inorganic silicon source in a second solvent to obtain a first material; adding a dilute acid solution to the first material for stirring to obtain a silica sol; mixing the silica sol with the solid electrolyte suspension to obtain a solid electrolyte / silica sol composite sol;
[0051] S2, subjecting the solid electrolyte / silica sol composite sol to gel treatment and drying treatment to obtain a composite material precursor; subjecting the composite material precursor to heat treatment to obtain a composite material containing a solid electrolyte and SiO2 aerogel; subjecting the composite material containing a solid electrolyte and SiO2 aerogel to grinding treatment to obtain first particles; wherein the first particles include solid electrolyte / SiO2 aerogel composite particles;
[0052] S3, dispersing the first particles in a third solvent to obtain a diaphragm slurry; coating the diaphragm slurry on the surface of the base film and performing a baking treatment.
[0053] The method of the present invention uses an inorganic silicon source and a solid electrolyte, adopts a sol-gel method and an in-situ loading method, prepares a solid electrolyte / SiO2 gel, and obtains a composite material containing a solid electrolyte and a SiO2 aerogel after normal pressure drying and heat treatment, wherein the solid electrolyte and the SiO2 aerogel in the composite material containing a solid electrolyte and a SiO2 aerogel are mutually doped. The composite material is crushed to obtain a first particle, and the first particle is coated on both sides of the diaphragm, and a composite diaphragm is obtained after drying. The first particle of the present invention may contain solid electrolyte particles and SiO2 aerogel particles, wherein solid electrolyte particles with a smaller particle size are distributed in the pores of the SiO2 aerogel particles to form solid electrolyte / SiO2 aerogel composite particles; and some solid electrolyte particles with a larger particle size are distributed between the SiO2 aerogel particles to form mixed particles with the solid electrolyte / SiO2 aerogel composite particles.
[0054] The method of the present invention disperses the solid electrolyte inside the three-dimensional skeleton of SiO2 aerogel. For example, the solid electrolyte can be lithium aluminum titanium phosphate. After high-temperature heat treatment, SiO2 induces the lithium aluminum titanium phosphate solid electrolyte to generate a small amount of secondary phase LiTiOPO4, which can adjust the microstructure morphology of the material, improve the grain boundary ion transport, and thus improve the total ion conductivity of the battery. The composite diaphragm prepared by the method of the present invention has excellent properties such as good high-temperature dimensional stability, flame retardancy and mechanical properties, and can be punctured without occurrence of perforation under high current. It has low preparation cost and simple process, and meets the technical requirements for realizing industrialization.
[0055] According to the present invention, a binder is also dispersed in the third solvent; preferably, the binder is selected from at least one of acrylate binders, polytetrafluoroethylene, polyvinylidene fluoride, polyacrylonitrile and polyvinyl alcohol; preferably, the acrylate binder is selected from at least one of acrylates, cyanoacrylates and diester acrylates.
[0056] According to the present invention, based on the total mass of the solid electrolyte suspension, the mass fraction of the solid electrolyte particles is 4-10%. Exemplarily, the mass fraction of the solid electrolyte particles can be any value among 4%, 6%, 8% and 10%, or any value within the range of any two of the above values. Preferably, the mass fraction of the solid electrolyte particles can be 5-8%.
[0057] In one embodiment of the present invention, based on the total volume of the first material, the volume fraction of the inorganic silicon source is 15-40%. Exemplarily, the volume fraction of the inorganic silicon source can be any value among 15%, 20%, 25%, 30%, 35% and 40%, or any value within the range of any two of the above values. Preferably, the volume fraction of the inorganic silicon source is 20-30%.
[0058] In one embodiment of the present invention, the molar concentration of the dilute acid solution is 1-2 mol / L; illustratively, the molar concentration of the dilute acid solution can be any value among 1 mol / L, 1.2 mol / L, 1.4 mol / L, 1.6 mol / L, 1.8 mol / L and 2 mol / L or any value within the range consisting of any two of the above values.
[0059] In one embodiment of the present invention, based on the total volume of the silica sol, the volume fraction of the dilute acid solution can be 0.5-0.8%. For example, the volume fraction of the dilute acid solution can be any value among 0.5%, 0.6%, 0.7% and 0.8%, or any value within the range of any two of the above values. Preferably, the volume fraction of the dilute acid solution can be 0.6-0.7%.
[0060] In one embodiment of the present invention, the mixing ratio of the silica sol and the solid electrolyte suspension may be 4 to 5: 1. Exemplarily, the mixing ratio of the silica sol and the solid electrolyte suspension may be any value among 4: 1, 4.2: 1, 4.4: 1, 4.6: 1, 4.8: 1 and 5: 1 or any value within the range of any two of the above values.
[0061] According to the present invention, the mass fraction of the first particles contained in the diaphragm slurry may be 25-45%. Exemplarily, the mass fraction of the solid electrolyte / SiO2 aerogel composite particles contained in the diaphragm slurry may be any value among 25%, 30%, 35%, 40% and 45%, or any value within the range of any two of the above values. Preferably, the mass fraction of the first particles contained in the diaphragm slurry is 30-40%.
[0062] According to the present invention, the inorganic silicon source can be selected from silicon tetrachloride and / or water glass; optionally, the dilute acid solution is selected from at least one of dilute hydrochloric acid, dilute nitric acid and dilute sulfuric acid; optionally, the first solvent, the second solvent and the third solvent are water.
[0063] Illustratively, in step S1, the rate of dripping the dilute acid solution may be 0.8 to 1.2 mL / min.
[0064] Exemplarily, in step S2, the conditions for the gel treatment may include: a temperature of 30 to 50°C and a time of 3 to 6 hours; and / or, the conditions for the drying treatment may include: a pressure of 0.001 to 0.1013 MPa, a temperature of 60 to 80°C, a time of 24 to 48 hours, and an air flow rate of 1 to 1.5 m / s; and / or, the heat treatment is carried out in an oxygen atmosphere; the conditions for the heat treatment may include: a temperature of 600 to 800°C, a time of 1 to 2 hours, and a heating rate of 5 to 10°C / min.
[0065] Exemplarily, in step S3, the coating method can be one or more of gravure roller coating, dip coating, narrow coating or spray coating; the baking treatment conditions can include: temperature of 40 to 50°C, time of 20 to 30 minutes, and air flow rate in the baking equipment of 2 to 2.5 m / s.
[0066] A third aspect of the present invention provides a battery, comprising the composite diaphragm described above, and / or the composite diaphragm prepared according to the method described above.
[0067] In the embodiment of the present invention, the battery structure includes but is not limited to button batteries, soft-pack batteries, cylindrical batteries, etc.
[0068] The present application has no special restrictions on the negative electrode sheet, positive electrode sheet, electrolyte, etc. in the battery, and those skilled in the art can choose according to actual needs as long as the purpose of the present application can be achieved.
[0069] The present invention is further described in detail by way of examples. The raw materials used in the examples can be obtained through commercial sources.
[0070] Example 1
[0071] (1) Preparation of solid electrolyte / SiO2 aerogel composite material: Weigh 6 g of lithium aluminum titanium phosphate solid electrolyte Li 1.3 Al 0.3 Ti 1.7 P3O 12 (D50 is 50nm), dispersed in 100mL aqueous solution to obtain a solid electrolyte suspension. Disperse 50mL of silicon tetrachloride in 200mL aqueous solution, slowly add 1.5mL of 1.5mol / L dilute hydrochloric acid solution, and stir evenly to obtain silica sol. Subsequently, take 50mL of solid electrolyte suspension and add it to the prepared silica sol to obtain a solid electrolyte / silica sol composite sol.
[0072] The composite sol was poured into the mold, sealed with plastic wrap, and placed in a 40°C oven for gelation for 5 hours. After gelation, the plastic wrap was opened and placed in a blast drying oven at 70°C for 30 hours to obtain a composite material precursor, wherein the air flow rate of the blast drying oven was 1.2 m / s. The composite material precursor was heat treated at a heating rate of 5°C / min and a holding temperature of 700°C for 1 hour in an air atmosphere to obtain a solid electrolyte / SiO2 aerogel composite material.
[0073] (2) Preparation of composite diaphragm: Grind the prepared solid electrolyte / SiO2 aerogel composite material to a D50 of 600nm to obtain the first particles, add 150g of the ground first particles and 10g of binder (polytetrafluoroethylene) into 340mL of water and stir and disperse for 2h to obtain diaphragm slurry (the mass fraction of solid electrolyte / SiO2 aerogel composite particles in the diaphragm slurry is 50%). Spray the diaphragm slurry on both sides of the 7μm polyethylene diaphragm, and the coating thickness is 2±0.5μm. After baking at 45°C for 30min in an oven with an air flow rate of 2m / s, a composite diaphragm coated with solid electrolyte / SiO2 aerogel is obtained.
[0074] (3) Preparation of lithium-ion batteries: The negative electrode sheet (the negative electrode active material is graphite), the prepared composite separator, and the positive electrode sheet (the positive electrode active material is lithium nickel cobalt manganese oxide) are stacked in sequence and wound to obtain a bare battery cell. After the tabs are welded, the bare battery cell is placed in a battery aluminum shell / soft-pack aluminum-plastic film. After liquid injection, side top sealing, drying, formation, constant volume, and exhaust sealing, a lithium-ion battery is obtained.
[0075] Example 2
[0076] (1) Preparation of solid electrolyte / SiO2 aerogel composite material: Weigh 6 g of lithium aluminum titanium phosphate solid electrolyte Li 1.3 Al 0.3 Ti 1.7 P3O 12(D50 is 50nm), dispersed in 100mL aqueous solution to obtain a solid electrolyte suspension. Disperse 50mL of silicon tetrachloride in 200mL aqueous solution, slowly add 1.5mL of 1.5mol / L dilute nitric acid solution, and stir evenly to obtain silica sol. Subsequently, take 50mL of solid electrolyte suspension and add it to the prepared silica sol to obtain a solid electrolyte / silica sol composite sol.
[0077] The composite sol was poured into the mold, sealed with plastic wrap, and placed in a 40°C oven for gelation for 5 hours. After gelation, the plastic wrap was opened and placed in a blast drying oven at 70°C for 30 hours to obtain a composite material precursor, wherein the air flow rate of the blast drying oven was 1.2 m / s. The composite material precursor was heat treated at a heating rate of 5°C / min and a holding temperature of 800°C for 1 hour in an air atmosphere to obtain a solid electrolyte / SiO2 aerogel composite material.
[0078] (2) Preparation of composite diaphragm: The prepared solid electrolyte / SiO2 aerogel composite material was ground to a D50 of 600 nm to obtain the first particles. 150 g of the ground first particles and 10 g of binder (polyvinyl alcohol) were added to 340 mL of water and stirred and dispersed for 2 h to obtain a diaphragm slurry. The diaphragm slurry was sprayed on both sides of a 7 μm polyethylene diaphragm, and the coating thickness was 2 ± 0.5 μm. After baking at 45 ° C for 30 min in an oven with an air flow rate of 2 m / s, a solid electrolyte / SiO2 aerogel-coated composite diaphragm was obtained.
[0079] (3) Preparation of lithium-ion battery: The preparation method of the lithium-ion battery of this embodiment is the same as that of embodiment 1.
[0080] Example 3
[0081] (1) Preparation of solid electrolyte / SiO2 aerogel composite material: Weigh 5 g of lithium aluminum titanium phosphate solid electrolyte Li 1.3 Al 0.3 Ti 1.7 P3O 12 (D50 is 50nm), dispersed in 100mL aqueous solution to obtain a solid electrolyte suspension. Disperse 50mL of water glass in 200mL of aqueous solution, slowly add 2mL of 1.5mol / L dilute hydrochloric acid solution, and stir evenly to obtain silica sol. Subsequently, take 50mL of solid electrolyte suspension and add it to the prepared silica sol to obtain a solid electrolyte / silica sol composite sol.
[0082] The composite sol was poured into the mold, sealed with plastic wrap, and placed in a 40°C oven for gelation for 5 hours. After gelation, the plastic wrap was opened and placed in a blast drying oven at 60°C for 48 hours to obtain a composite material precursor, wherein the air flow rate of the blast drying oven was 1.2 m / s. The composite material precursor was heat treated at a heating rate of 5°C / min and a holding temperature of 700°C for 1 hour in an air atmosphere to obtain a solid electrolyte / SiO2 aerogel composite material.
[0083] (2) Preparation of composite diaphragm: The prepared solid electrolyte / SiO2 aerogel composite material was ground to a D50 of 600 nm to obtain the first particles. 150 g of the ground first particles and 10 g of a binder (polyacrylonitrile) were added to 340 mL of water and stirred and dispersed for 2 h to obtain a diaphragm slurry. The diaphragm slurry was sprayed on both sides of a 7 μm polyethylene diaphragm, and the coating thickness was 2 ± 0.5 μm. After baking at 45 ° C for 30 min in an oven with an air flow rate of 2 m / s, a solid electrolyte / SiO2 aerogel-coated composite diaphragm was obtained.
[0084] (3) Preparation of lithium-ion battery: The preparation method of the lithium-ion battery of this embodiment is the same as that of embodiment 1.
[0085] Example 4
[0086] (1) Preparation of solid electrolyte / SiO2 aerogel composite material: Weigh 8 g of lithium aluminum titanium phosphate solid electrolyte Li 1.3 Al 0.3 Ti 1.7 P3O 12 (D50 is 50nm), dispersed in 100mL aqueous solution to obtain a solid electrolyte suspension. Disperse 50mL of water glass in 200mL aqueous solution, slowly add 1.5mL of 1.5mol / L dilute hydrochloric acid solution, and stir evenly to obtain silica sol. Subsequently, take 50mL of solid electrolyte suspension and add it to the prepared silica sol to obtain a solid electrolyte / silica sol composite sol.
[0087] The composite sol was poured into the mold, sealed with plastic wrap, and placed in a 50°C oven for gelation for 3 hours. After gelation, the plastic wrap was opened and placed in a blast drying oven at 70°C for 30 hours to obtain a composite material precursor, wherein the air flow rate of the blast drying oven was 1.2 m / s. The composite material precursor was heat treated at a heating rate of 5°C / min and a holding temperature of 700°C for 1 hour in an air atmosphere to obtain a solid electrolyte / SiO2 aerogel composite material.
[0088] (2) Preparation of composite diaphragm: The prepared solid electrolyte / SiO2 aerogel composite material was ground to a D50 of 600 nm to obtain the first particles. 200 g of the ground first particles and 12 g of binder (polytetrafluoroethylene) were added to 340 mL of water and stirred and dispersed for 2 h to obtain a diaphragm slurry. The diaphragm slurry was sprayed on both sides of a 7 μm polyethylene diaphragm, and the coating thickness was 2 ± 0.5 μm. After baking at 45 ° C for 30 min in an oven with an air flow rate of 2 m / s, a solid electrolyte / SiO2 aerogel-coated composite diaphragm was obtained.
[0089] (3) Preparation of lithium-ion battery: The preparation method of the lithium-ion battery of this embodiment is the same as that of embodiment 1.
[0090] Example 5
[0091] (1) Preparation of solid electrolyte / SiO2 aerogel composite material: Weigh 6 g of lithium aluminum titanium phosphate solid electrolyte Li 1.3 Al 0.3 Ti 1.7 P3O 12 (D50 is 50nm), dispersed in 100mL aqueous solution to obtain a solid electrolyte suspension. Disperse 50mL of silicon tetrachloride in 200mL aqueous solution, slowly add 1.5mL of 1.5mol / L dilute hydrochloric acid solution, and stir evenly to obtain silica sol. Subsequently, take 50mL of solid electrolyte suspension and add it to the prepared silica sol to obtain a solid electrolyte / silica sol composite sol.
[0092] The composite sol was poured into the mold, sealed with plastic wrap, and placed in a 40°C oven for gelation for 5 hours. After gelation, the plastic wrap was opened and placed in a blast drying oven at 60°C for 30 hours to obtain a composite material precursor, wherein the air flow rate of the blast drying oven was 1.5 m / s. The composite material precursor was heat treated at a heating rate of 5°C / min and a holding temperature of 700°C for 1 hour in an air atmosphere to obtain a solid electrolyte / SiO2 aerogel composite material.
[0093] (2) Preparation of composite diaphragm: The prepared solid electrolyte / SiO2 aerogel composite material was ground to a D50 of 600 nm to obtain the first particles. 150 g of the ground first particles and 10 g of binder (polytetrafluoroethylene) were added to 340 mL of water and stirred and dispersed for 2 h to obtain a diaphragm slurry. The diaphragm slurry was dip-coated on both sides of a 9 μm polypropylene diaphragm, and the coating thickness was 2 ± 0.5 μm. After baking at 45 ° C for 30 min in an oven with an air flow rate of 2 m / s, a solid electrolyte / SiO2 aerogel-coated composite diaphragm was obtained.
[0094] (3) Preparation of lithium-ion battery: The preparation method of the lithium-ion battery of this embodiment is the same as that of embodiment 1.
[0095] Comparative Example 1
[0096] (1) Preparation of composite material precursor: Weigh 6 g of lithium aluminum titanium phosphate solid electrolyte Li 1.3 Al 0.3 Ti 1.7 P3O 12 (D50 is 50nm), dispersed in 100mL aqueous solution to obtain a solid electrolyte suspension. Disperse 50mL of silicon tetrachloride in 200mL aqueous solution, slowly add 1.5mL of 1.5mol / L dilute hydrochloric acid solution, and stir evenly to obtain silica sol. Subsequently, take 50mL of solid electrolyte suspension and add it to the prepared silica sol to obtain a solid electrolyte / silica sol composite sol.
[0097] The composite sol was poured into the mold, sealed with plastic wrap, and placed in a 40°C oven for gelation for 5 hours. After gelation, the plastic wrap was opened and placed in a blast drying oven for drying at 70°C for 30 hours to obtain a composite material precursor, wherein the air flow rate of the blast drying oven was 1.2 m / s.
[0098] (2) Preparation of composite membrane: The preparation method of the composite membrane in this comparative example is the same as that in Example 1, except that the composite material precursor prepared in this comparative example is used to replace the solid electrolyte / SiO2 aerogel composite material in Example 1.
[0099] (3) Preparation of lithium-ion battery: The preparation method of the lithium-ion battery of this comparative example is the same as that of Example 1.
[0100] Comparative Example 2
[0101] (1) Preparation of composite diaphragm: 6 g of lithium aluminum titanium phosphate solid electrolyte Li 1.3 Al 0.3 Ti 1.7 P3O 12 (D50 is 50nm), 28.59g SiO2 and 10g binder (polytetrafluoroethylene) were added to 340mL water and stirred for 2h to obtain a diaphragm slurry. The diaphragm slurry was sprayed on both sides of a 7μm polyethylene diaphragm, and the coating thickness was 2±0.5μm. After baking at 45°C for 30min in an oven with an air flow rate of 2m / s, the composite diaphragm of this comparative example was obtained.
[0102] (2) Preparation of lithium-ion battery: The preparation method of the lithium-ion battery of this comparative example is the same as that of Example 1.
[0103] Comparative Example 3
[0104] (1) Preparation of composite diaphragm: SiO2 aerogel particles were ground to a D50 of 600 nm, 150 g of the ground SiO2 aerogel particles and 10 g of a binder (polytetrafluoroethylene) were added to 340 mL of water and stirred for 2 h to obtain a diaphragm slurry. The diaphragm slurry was sprayed on both sides of a 7 μm polyethylene diaphragm, and the coating thickness was 2 ± 0.5 μm. The composite diaphragm of this comparative example was obtained after baking at 45°C for 30 min in an oven with an air flow rate of 2 m / s.
[0105] (2) Preparation of lithium-ion battery: The preparation method of the lithium-ion battery of this comparative example is the same as that of Example 1.
[0106] Comparative Example 4
[0107] (1) Preparation of composite membrane: Lithium aluminum titanium phosphate solid electrolyte Li 1.3 Al 0.3 Ti 1.7 P3O 12 (D50 is 50nm) and 10g of binder (polytetrafluoroethylene) were added to 340mL of water and stirred for 2h to obtain a diaphragm slurry. The diaphragm slurry was sprayed on both sides of a 7μm polyethylene diaphragm, and the coating thickness was 2±0.5μm. After baking at 45°C for 30min in an oven with an air flow rate of 2m / s, the composite diaphragm of this comparative example was obtained.
[0108] (2) Preparation of lithium-ion battery: The preparation method of the lithium-ion battery of this comparative example is the same as that of Example 1.
[0109] Comparative Example 5
[0110] (1) Preparation of solid electrolyte / SiO2 aerogel composite material: The preparation method of the solid electrolyte / SiO2 aerogel composite material in this comparative example is the same as that in Example 1.
[0111] (2) Preparation of composite diaphragm: The prepared solid electrolyte / SiO2 aerogel composite material was ground to a D50 of 600 nm to obtain the first particles. 300 g of the ground first particles and 12 g of a binder (polytetrafluoroethylene) were added to 288 mL of water and stirred and dispersed for 2 h to obtain a diaphragm slurry (the mass fraction of the solid electrolyte / SiO2 aerogel composite particles in the diaphragm slurry was 60%). The diaphragm slurry was sprayed on both sides of a 7 μm polyethylene diaphragm, and the coating thickness was 2 ± 0.5 μm. After baking at 45 ° C for 30 min in an oven with an air flow rate of 2 m / s, a solid electrolyte / SiO2 aerogel-coated composite diaphragm was obtained.
[0112] (2) Preparation of lithium-ion battery: The preparation method of the lithium-ion battery of this comparative example is the same as that of Example 1.
[0113] Comparative Example 6
[0114] (1) Preparation of composite diaphragm: Al2O3 was ground to a D50 of 600 nm, 150 g of the ground Al2O3 and 10 g of a binder (polyvinyl alcohol) were added to 340 mL of water and stirred for 2 h to obtain a diaphragm slurry. The diaphragm slurry was sprayed on both sides of a 7 μm polyethylene diaphragm, and the coating thickness was 2 ± 0.5 μm. The composite diaphragm of this comparative example was obtained after baking at 45°C for 30 min in an oven with an air flow rate of 2 m / s.
[0115] (2) Preparation of lithium-ion battery: The preparation method of the lithium-ion battery of this comparative example is the same as that of Example 1.
[0116] Performance Testing
[0117] The performance tests of the composite diaphragms prepared in the above embodiments and comparative examples and the constructed lithium batteries were carried out as follows:
[0118] 1. Performance test of composite diaphragm:
[0119] (1) Thickness test: Use a high-precision thickness gauge to test the thickness of the diaphragm at different locations and take the average value of 10 thicknesses.
[0120] (2) Air permeability test: The diaphragm to be tested is placed between two air chambers. Gas is passed from one air chamber through the diaphragm to the other air chamber through a constant pressure difference. The air permeability of the diaphragm is calculated by measuring the amount of gas passing through the diaphragm per unit time.
[0121] (3) Needle puncture strength test: Referring to GB / T 36363-2018 standard, the diaphragm was placed under the sample table fixing fixture, and a universal tensile testing machine was used to record the maximum force value of the 1 mm diameter round needle puncturing the diaphragm at a speed of 100±100 mm / min.
[0122] (4) Heat shrinkage test: Cut the diaphragm into 100 mm*100 mm samples, place the samples flatly between two layers of A4 paper, and then bake the samples in an oven at 130°C for 1 hour. After heating, take out the samples and measure the sample size again.
[0123] Shrinkage rate: (size before shrinkage - size after shrinkage) / size before shrinkage * 100%
[0124] (5) Film rupture temperature test: The diaphragm is cut into appropriate sizes and placed in a hot press. A heating compression test is performed at different temperatures and pressures to test the compressive strength and density of the diaphragm at different temperatures and obtain the film rupture temperature.
[0125] (6) Peel force test: Fix the sample in the fixture of the universal tensile machine so that the peeling direction is perpendicular or opposite to the sample surface. Then, load the sample at a certain speed until peeling occurs. Based on the force and displacement data recorded by the universal tensile machine during the loading process, calculate the peel force and peel strength between the coating and the base film.
[0126] Table 1
[0127]
[0128] 2. Electrical performance test:
[0129] (1) At room temperature of 25°C, use a charge and discharge test cabinet to test the charge and discharge resistance of each lithium battery at 20% SOC to determine the internal resistance of the lithium battery at low SOC.
[0130] The RT 1C / 1C actual capacity C0 test method includes: placing each lithium battery at room temperature (25±2°C) for 5 minutes, discharging to 2.8V using a 1C constant current, standing for 15 minutes, charging to 4.25V using a 1C constant current, and then charging to I≤0.05C using a constant voltage, standing for 15 minutes, and discharging to 2.8 at a 1C constant current, which is recorded as the measured capacity C0.
[0131] The charging and discharging resistance test method of the lithium battery includes: after each lithium battery is allowed to stand at room temperature (25±2℃) for 5 minutes, 1C0 constant current charging to 4.25V, then 4.25V constant voltage charging to I≤0.05C0, standing for 5 minutes, 1C0 constant current discharge for 48 minutes (the power is adjusted to 20% SOC), standing for 60 minutes, 1C0 constant current discharge for 30 seconds, and obtaining the discharge resistance; standing for 40 seconds, 2C0 constant current charging for 30 seconds (the power is adjusted back to the original SOC), and obtaining the charging resistance.
[0132] (2) Each lithium battery was charged and discharged at an ambient temperature of 25°C and 45°C, with a starting and a cutting-off voltage of 2.8 V and 4.25 V, respectively. It was first charged at 1C to 4.25 V, then charged at a constant voltage of 4.25 V until the current decreased to 0.05C, and then discharged at 0.1C to 2.8 V. The discharge capacity of the first cycle was recorded. The charge and discharge cycle was repeated for 500 cycles, and the discharge capacity of the battery at the 200th and 500th cycles was recorded. Capacity retention rate = discharge capacity at the 200th or 500th cycle / discharge capacity of the first cycle*100%.
[0133] Table 2
[0134] Category / Project Discharge resistance / mΩ Charging resistance / mΩ Example 1 37.1 45.3 Example 2 37.3 45.4 Example 3 37.5 45.2 Example 4 37.0 45.5 Example 5 37.4 45.0 Comparative Example 1 39.2 48.1 Comparative Example 2 37.4 44.8 Comparative Example 3 41.2 49.7 Comparative Example 4 37.9 46.0 Comparative Example 5 39.4 46.5 Comparative Example 6 40.3 48.6
[0135] Table 3
[0136]
[0137]
[0138] It can be seen from the test results that the coating composite materials prepared in Examples 1-5 when applied to the diaphragm can effectively improve the air permeability and temperature resistance of the diaphragm, enhance the peel strength between the coating and the base film, and improve the long-term cycle and high temperature performance of the battery.
[0139] Figure 1 This is a SEM image of one side of the composite membrane prepared in Example 1. It can be seen that the coating has a uniform microstructure and a rich pore structure. The porosity of the composite membrane is 42.6% and the specific surface area is 67.8 m 2 / g, providing a basis for the air permeability of the diaphragm. Figure 2 is a schematic diagram of the structure of the composite diaphragm prepared in Example 1. Figure 2 It can be seen that the coating is evenly applied on both sides of the diaphragm.
[0140] In Table 1 and Table 2, the physical properties and peel strength of the diaphragms prepared by Examples 1 to 5 are compared with those prepared by Comparative Examples 1 to 6. The thickness of each group of diaphragms is uniform, and within the target thickness range, the needle puncture strength of the mixed solid electrolyte group is slightly improved. Comparative Example 1 is compared with Example 1. It can be seen that the charging resistance and discharge resistance of the battery are increased by 2-3mΩ without heat treatment of the composite precursor, indicating that the designed heat treatment process can induce the solid in situ to produce LiTiOPO4 secondary phase uniformly distributed at the grain boundary, which can prevent the excessive growth of LATP grains and the accompanying occluded pores and microcracks, thereby effectively regulating the uniform morphology of LATP grains. In Comparative Example 2, SiO2 is used to replace SiO2 aerogel. The results show that the constructed SiO2 aerogel porous structure can significantly improve the air permeability and high temperature resistance of the diaphragm. In Comparative Example 3, no solid electrolyte was added, and SiO2 aerogel and binder were directly coated on both sides of the diaphragm, and the charging resistance and discharge resistance were increased, indicating that the addition of solid electrolyte and the induced LiTiOPO4 secondary phase can significantly improve the internal resistance of the battery. In addition, in Comparative Example 4, solid electrolyte and binder were directly coated on both sides of the diaphragm, and the air permeability and temperature resistance of the diaphragm were significantly reduced, and the peeling force and peeling strength of the coating were also significantly reduced, and the high-temperature cycle performance of the battery was also significantly reduced, indicating that the SiO2 aerogel of the present invention has a significant effect on improving the high-temperature resistance of the diaphragm.
[0141] In addition, the difference of Comparative Example 5 is that the mass fraction of the solid electrolyte / SiO2 aerogel composite material in the diaphragm slurry is 60%, the solid content of the diaphragm slurry is increased, and the viscosity is increased. Although the temperature resistance of the diaphragm is slightly improved, the thickness of the diaphragm is uneven and the air permeability is poor, resulting in reduced long-term cycle stability. Compared with Example 1, Comparative Example 6 replaces the solid electrolyte / SiO2 aerogel composite material with conventional Al2O3 of the same particle size range and is coated on both sides of the diaphragm. The air permeability and temperature resistance of the diaphragm are reduced, and the peeling force and peeling strength of the coating are also reduced, resulting in reduced long-term performance of the battery, indicating that the prepared solid electrolyte / SiO2 aerogel composite material has obvious advantages over conventional Al2O3 coatings.
[0142] In summary, the present invention utilizes an inorganic silicon source and a solid electrolyte, adopts a sol-gel method and an in-situ loading method, to prepare a solid electrolyte / SiO2 gel, and obtains a doped solid electrolyte / SiO2 aerogel composite material after normal pressure drying and heat treatment. The composite material is crushed and coated on both sides of the diaphragm, and a composite diaphragm is obtained after drying. A small amount of secondary phase LiTiOPO4 generated after heat treatment of SiO2 and the solid electrolyte can adjust the microstructure morphology of the material, improve the grain boundary ion transport, and thus improve the total ion conductivity of the battery. The porous structure of SiO2 aerogel can improve the air permeability and high temperature resistance of the diaphragm. The prepared solid electrolyte / SiO2 aerogel coating is more uniform and stable, and the peel strength between the coating and the base film is improved, which can effectively reduce the charging internal resistance and the discharging internal resistance of the battery, and improve the long-term cycle and high temperature performance of the battery.
[0143] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A composite diaphragm, characterized in that: The composite diaphragm comprises a base film and a coating disposed on the surface of the base film, wherein the coating contains solid electrolyte particles and SiO2 aerogel particles; Wherein, at least part of the solid electrolyte particles are distributed in the pores of the SiO2 aerogel particles to form solid electrolyte / SiO2 aerogel composite particles.
2. The composite diaphragm according to claim 1, characterized in that: The particle size D50 of the solid electrolyte / SiO2 aerogel composite particles is 500 to 800 nm, preferably 600 to 700 nm; Optionally, the pore size of the solid electrolyte / SiO2 aerogel composite particles is 2 to 15 nm, preferably 8 to 10 nm; Optionally, based on the total mass of the solid electrolyte particles and the SiO2 aerogel particles, the mass fraction of the SiO2 aerogel particles is 80 to 90 wt%, preferably 84 to 86 wt%.
3. The composite diaphragm according to claim 1, characterized in that: The particle size D50 of the solid electrolyte particles is 10 to 80 nm; preferably, the particle size D50 of the solid electrolyte particles is 40 to 50 nm; Optionally, the solid electrolyte particles are selected from at least one of lithium titanium aluminum phosphate solid electrolyte particles, lithium lanthanum titanium oxide solid electrolyte particles and lithium lanthanum zirconium oxide solid electrolyte particles; preferably, the solid electrolyte particles are lithium titanium aluminum phosphate solid electrolyte particles.
4. The composite diaphragm according to claim 1, characterized in that: The coating also contains a binder; Preferably, the mass ratio of the total mass of the solid electrolyte particles and the SiO2 aerogel particles to the binder is 1:(0.02-0.16), preferably 1:(0.05-0.1); Preferably, the adhesive is selected from at least one of acrylate adhesives, polytetrafluoroethylene, polyvinylidene fluoride, polyacrylonitrile and polyvinyl alcohol; preferably, the acrylate adhesive is selected from at least one of acrylate, cyanoacrylate and diester acrylate.
5. The composite diaphragm according to claim 1, characterized in that: The porosity of the composite diaphragm is 40-60%, preferably 50-55%; The base film has a thickness of 7 to 9 μm and a porosity of 35 to 45%; Optionally, the material of the base film includes one of polyester, polyethylene and polypropylene.
6. A method for preparing the composite diaphragm according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: S1, dispersing solid electrolyte particles in a first solvent to obtain a solid electrolyte suspension; dispersing an inorganic silicon source in a second solvent to obtain a first material; adding a dilute acid solution to the first material for stirring to obtain a silica sol; mixing the silica sol with the solid electrolyte suspension to obtain a solid electrolyte / silica sol composite sol; S2, subjecting the solid electrolyte / silica sol composite sol to gel treatment and drying treatment to obtain a composite material precursor; subjecting the composite material precursor to heat treatment to obtain a composite material containing a solid electrolyte and SiO2 aerogel; subjecting the composite material containing a solid electrolyte and SiO2 aerogel to grinding treatment to obtain first particles; wherein the first particles include solid electrolyte / SiO2 aerogel composite particles; S3, dispersing the first particles in a third solvent to obtain a diaphragm slurry; coating the diaphragm slurry on the surface of the base film and performing a baking treatment.
7. The method according to claim 6, characterized in that A binder is also dispersed in the third solvent; Preferably, the adhesive is selected from at least one of acrylate adhesives, polytetrafluoroethylene, polyvinylidene fluoride, polyacrylonitrile and polyvinyl alcohol; preferably, the acrylate adhesive is selected from at least one of acrylate, cyanoacrylate and diester acrylate.
8. The method according to claim 6, characterized in that Based on the total mass of the solid electrolyte suspension, the mass fraction of the solid electrolyte particles is 4 to 10%, preferably 5 to 8%; And / or, based on the total volume of the first material, the volume fraction of the inorganic silicon source is 15 to 40%, preferably 20 to 30%; and / or, the molar concentration of the dilute acid solution is 1 to 2 mol / L; And / or, based on the total volume of the silica sol, the volume fraction of the dilute acid solution is 0.5-0.8%, preferably 0.6-0.7%; and / or, the mixing ratio of the silica sol and the solid electrolyte suspension is 4 to 5:1; And / or, the mass fraction of the first particles contained in the diaphragm slurry is 25-45%, preferably 30-40%; Optionally, the inorganic silicon source is selected from silicon tetrachloride and / or water glass; Optionally, the dilute acid solution is selected from at least one of dilute hydrochloric acid, dilute nitric acid and dilute sulfuric acid; Optionally, the first solvent, the second solvent and the third solvent are water.
9. The method according to claim 6, characterized in that In step S1, the dilute acid solution is added at a rate of 0.8 to 1.2 mL / min; And / or, in step S2, the conditions of the gel treatment include: temperature of 30-50°C, time of 3-6h; and / or, the conditions of the drying treatment include: pressure of 0.001-0.1013MPa, temperature of 60-80°C, time of 24-48h, air flow rate of 1-1.5m / s; and / or, the heat treatment is carried out in an oxygen atmosphere; the conditions of the heat treatment include: temperature of 600-800°C, time of 1-2h, heating rate of 5-10°C / min; And / or, in step S3, the baking treatment conditions include: a temperature of 40-50° C., a time of 20-30 min, and an air flow rate in the baking equipment of 2-2.5 m / s.
10. A battery, characterized in that: The battery comprises the composite diaphragm according to any one of claims 1 to 5, and / or the composite diaphragm prepared by the method according to any one of claims 6 to 9.
Citation Information
Patent Citations
Ceramic diaphragm taking aerogel as powder body, and applications of ceramic diaphragm in lithium ion battery
CN106784558A
Preparation method of porous gel electrolyte material
CN110504485A
Solid-state lithium battery silicon dioxide aerogel framework electrolyte and preparation method thereof
CN111916818A
Composite solid electrolyte, preparation method thereof and solid-state battery
CN112002940A
Super-hydrophilic long-acting antibacterial glass coating composition and preparation method thereof
CN112500722A
Cited By
Composite diaphragm, preparation method thereof and battery
CN119833889A
Composite separator, method for manufacturing the same, and battery
CN119833889B