Catalyst, catalyst precursor, method for producing catalyst, catalyst-filled reaction tube, and method for decomposing nitrous oxide
By using a honeycomb structure catalyst supported by ruthenium-supported ruthenium in the catalyst-filled reaction tube, the problem of low nitrous oxide decomposition efficiency is solved, efficient nitrous oxide decomposition is achieved, its emissions are reduced, and the decomposition efficiency is significantly improved.
Patent Information
- Application Number
- CN202380027288.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-05-12
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The decomposition efficiency of nitrous oxide in the prior art is not high enough, and the shape and loading of the catalyst are insufficiently studied, resulting in the emission of nitrous oxide in the atmosphere still exists, affecting the slowdown of global warming.
A catalyst containing titanium oxide as a support is used to support ruthenium and its compounds to form a honeycomb structure catalyst fill layer of 35 to 50% by volume, and decompose by contacting the gas of nitrous oxide, and the reaction tube is filled with a catalyst to improve the decomposition efficiency.
The decomposition efficiency of nitrous oxide is significantly improved, and it can efficiently decompose nitrous oxide in the catalyst-filled reaction tube, reduce its emissions, and achieve a concentration reduction rate of more than 50% and a decomposition rate of more than 3.0/sec.
Smart Images

Figure BDA0005040563360000241 
Figure BDA0005040563360000242
Abstract
Description
Technical Field
[0001] The present invention relates to a catalyst, a catalyst precursor, a method for producing a catalyst, a catalyst-filled reaction tube, and a method for decomposing nitrous oxide. Background Art
[0002] From the perspective of protecting the global environment and preventing air pollution, nitrogen oxides (NO x ) has become a problem, and its emission has been strictly regulated. In particular, the nitrogen oxides that are the subject of emission regulations are nitrogen dioxide (NO2), which is harmful to the human body and causes photochemical smog and acid rain. With the goal of reducing emissions, various denitrification technologies have been studied and put into practical use. However, nitrous oxide (N2O), which is a type of nitrogen oxide, is not currently subject to emission regulations and is usually released directly into the atmosphere. In fact, although the gases emitted from chemical manufacturing facilities such as nitric acid manufacturing plants, ε-caprolactam manufacturing plants, and adipic acid manufacturing plants are decomposed and removed of nitrogen monoxide and nitrogen dioxide through denitrification treatment, there are many cases where nitrous oxide produced as a by-product is not decomposed and removed and is emitted (released) into the atmosphere.
[0003] However, when greenhouse gases such as nitrous oxide are released into the atmosphere, the greenhouse effect of the atmosphere will be enhanced due to the increase in the concentration of greenhouse gases, which is considered to be the cause of global warming. In addition, it is said that nitrous oxide exhibits a warming effect of about 300 times that of carbon dioxide. Therefore, in recent years, not only carbon dioxide, methane, etc., but also the reduction of nitrous oxide emissions into the atmosphere has been paid more attention. With the improvement of sustainable environmental awareness, it is expected that nitrous oxide will become the target of emission restriction gases in the near future, so it is required to decompose and remove nitrous oxide in exhaust gas to suppress the emission into the atmosphere. As a technology for decomposing and removing nitrous oxide in exhaust gas, for example, a method for decomposing nitrous oxide is described in Patent Document 1, using a catalyst characterized by supporting at least one or more precious metals selected from ruthenium (Ru), rhodium (Rh), palladium (Pd), rhenium (Re), osmium (Os), iridium (Ir), and platinum (Pt), and a gas containing nitrous oxide is contact-decomposed (catalytically decomposed) in the coexistence of a reducing gas.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 06-218232 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] The method for decomposing nitrous oxide described in Patent Document 1 is said to be able to decompose nitrous oxide in nitrous oxide-containing gas by allowing carbon monoxide, hydrocarbon gas, mineral oil-based hydrocarbon gas, alcohols, etc. to coexist as reducing gases during the contact decomposition of the gas containing nitrous oxide. However, in Patent Document 1, although the amount of noble metal supported on the catalyst is described, no research is conducted on the shape of the catalyst, etc., and the decomposition efficiency of nitrous oxide cannot be said to be necessarily sufficient, and further improvement is desired.
[0009] The present invention aims to provide a catalyst capable of efficiently decomposing nitrous oxide, a precursor of the catalyst, and a method for producing the same. In addition, the present invention aims to provide a method for decomposing nitrous oxide capable of efficiently decomposing nitrous oxide, and a catalyst-filled reaction tube used in the method.
[0010] Solutions for solving problems
[0011] That is, the subject of the present invention is achieved by the following means.
[0012] <1> A catalyst is a catalyst comprising a catalyst-filled layer of a reaction tube, wherein a catalyst is supported on a carrier comprising titanium oxide and containing at least one component selected from the group consisting of ruthenium and ruthenium compounds, wherein:
[0013] The catalyst packing layer has a honeycomb structure with a packing volume ratio of 35 to 50 volume %.
[0014] <2> according to <1> The catalyst, wherein
[0015] The catalyst is formed by supporting 2 mass % or more of the component containing at least one selected from the group consisting of ruthenium and ruthenium compounds on the carrier based on metallic ruthenium.
[0016] <3> A catalyst, wherein
[0017] The catalyst is formed by supporting a component containing ruthenic acid on a carrier containing titanium oxide.
[0018] <4> A catalyst precursor, wherein
[0019] The catalyst precursor is formed by supporting a component containing an alkali metal salt of ruthenate on a carrier containing titanium oxide.
[0020] <5> A method for producing a catalyst is a method for producing a catalyst in which a carrier containing titanium oxide supports a component containing at least one selected from the group consisting of ruthenium and ruthenium compounds, wherein:
[0021] The method comprises the following steps (1) and (2),
[0022] Step (1): a step of contacting a support containing titanium oxide with a solution containing an alkali metal salt of ruthenate and water;
[0023] Step (2): a step of contacting the support containing titanium oxide and ruthenate alkali metal salt obtained in step (1) with an acidic aqueous solution.
[0024] <6> A catalyst-filled reaction tube comprises a catalyst-filled layer, wherein the catalyst-filled layer is filled with a catalyst containing at least one component selected from the group consisting of ruthenium and ruthenium compounds supported on a carrier containing titanium oxide, wherein:
[0025] The filling volume ratio of the catalyst in the catalyst filling layer is 35 to 50 volume %.
[0026] <7> A method for decomposing nitrous oxide, wherein:
[0027] Contains the above <1> ~ <3> A step of contacting the catalyst described in any one of claims 1 to 5 with a nitrous oxide-containing gas containing nitrous oxide.
[0028] <8> according to <7> The method for decomposing nitrous oxide, wherein:
[0029] The nitrous oxide-containing gas includes at least one gas selected from the group consisting of nitrogen, carbon monoxide, carbon dioxide, water vapor, oxygen, hydrogen, ammonia, nitric oxide, nitrogen dioxide, and hydrocarbons.
[0030] <9> according to <7> or <8> The method for decomposing nitrous oxide, wherein:
[0031] The nitrous oxide-containing gas is a gas exhausted from a chemical manufacturing facility.
[0032] <10> A method for decomposing nitrous oxide, wherein:
[0033] comprising causing the nitrous oxide-containing gas to be contained in the above <6> The step of circulating the catalyst in the filled reaction tube.
[0034] <11> according to <10> The method for decomposing nitrous oxide, wherein:
[0035] The nitrous oxide-containing gas includes at least one gas selected from the group consisting of nitrogen, carbon monoxide, carbon dioxide, water vapor, oxygen, hydrogen, ammonia, nitric oxide, nitrogen dioxide, and hydrocarbons.
[0036] <12> according to <10> or <11> The method for decomposing nitrous oxide, wherein:
[0037] The nitrous oxide-containing gas is a gas exhausted from a chemical manufacturing facility.
[0038] Effects of the Invention
[0039] The catalyst and catalyst-filled reaction tube of the present invention can efficiently decompose nitrous oxide by being used in a method for decomposing nitrous oxide. In addition, the catalyst precursor and production method of the present invention can produce the catalyst of the present invention exhibiting the above-mentioned excellent characteristics. Furthermore, the method for decomposing nitrous oxide of the present invention can efficiently decompose nitrous oxide. DETAILED DESCRIPTION
[0040] In the present invention and this specification, the numerical range expressed using "to" means a range including the numerical values described before and after "to" as the lower limit and the upper limit.
[0041] [catalyst]
[0042] The catalyst of the present invention is formed by supporting a carrier containing titanium oxide with at least one component selected from the group consisting of ruthenium and ruthenium compounds. In addition, the catalyst is filled in the catalyst filling area of the reaction tube described later to form a catalyst filling layer, and has a honeycomb structure in which the filling volume ratio at this time is 35 to 50 volume%. Such a catalyst of the present invention can decompose nitrous oxide efficiently by being used in the decomposition reaction of nitrous oxide.
[0043] First, the composition of the catalyst of the present invention will be described.
[0044] In the present invention, "a catalyst comprising a carrier comprising titanium oxide and containing at least one component selected from the group consisting of ruthenium and ruthenium compounds supported on the carrier" means a catalyst comprising at least one component selected from the group consisting of ruthenium and ruthenium compounds attached to the surface and / or pores of the carrier comprising titanium oxide.
[0045] In the present invention, as the component supported on the carrier, at least one selected from the group consisting of ruthenium and ruthenium compounds is selected from the viewpoint of balance between catalyst activity and cost.
[0046] (Ruthenium compounds)
[0047] There are no particular restrictions on the ruthenium compound, and examples thereof include ruthenium oxide, ruthenium hydroxide, ruthenium nitrate, ruthenium chloride, ruthenic acid, chlororuthenate, chlororuthenate hydrate, salts of ruthenic acid, ruthenium oxychloride, salts of ruthenium oxychloride, ruthenium ammine complex, chloride of ruthenium ammine complex, ruthenium bromide, ruthenium carbonyl complex, ruthenium organic acid salt, ruthenium nitrosyl complex, and the like.
[0048] Examples of ruthenium oxide include RuO2 and the like.
[0049] Examples of ruthenium hydroxide include Ru(OH) 3 .
[0050] Examples of ruthenium nitrate include Ru(NO3)3.
[0051] Examples of ruthenium chloride include RuCl 3 , RuCl 3 hydrate, and the like.
[0052] As ruthenic acid, H2RuO4 can be mentioned.
[0053] As chlororuthenate, K3RuCl6 and the like can be cited as [RuCl6] 3- Salts with anions such as K2RuCl6 or (NH4)2RuCl6 are [RuCl6] 2- Anionic salts.
[0054] Examples of chlororuthenate hydrates include [RuCl5(H2O)4] 2- As anionic salt hydrate, [RuCl2(H2O)4] + Cationic salt hydrates, etc.
[0055] As a salt of ruthenic acid, containing Ru VI O4 2- (tetraoxoruthenate(VI) ion), and Ru VII O4 - (perruthenate ion, tetraoxyruthenate (VII) ion). Examples of cations forming the salt include cations of alkali metal elements, cations of alkaline earth metal elements, Ag + , ammonium cations, etc. Among them, alkali metal salts of ruthenic acid (each salt of Li, Na, K, Rb, Cs) are preferred, and Na salts or K salts of ruthenic acid are more preferred. Specifically, Na2RuO4, K2RuO4, etc. can be listed.
[0056] Examples of ruthenium oxychloride include Ru2OCl4, Ru2OCl5, and Ru2OCl6.
[0057] Examples of ruthenium oxychloride salts include K2Ru2OCl 10 , Cs2Ru2OCl4, etc.
[0058] Examples of ruthenium ammine complexes include [Ru(NH3)6] 2+ , [Ru(NH3)6] 3+ 、[Ru(NH3)5H2O] 2+ The complexes of complex ions, etc.
[0059] Examples of chlorides of ruthenium ammine complexes include [Ru(NH3)5Cl] 2+It is a complex of complex ions, [Ru(NH3)6]Cl2, [Ru(NH3)6]Cl3, [Ru(NH3)6]Br3, etc.
[0060] Examples of ruthenium bromide include RuBr 3 , RuBr 3 hydrate, and the like.
[0061] Examples of ruthenium carbonyl complexes include Ru(CO)5, Ru3(CO) 12 wait.
[0062] Examples of ruthenium organic acid salts include [Ru3O(OCOCH3)6(H2O)3]OCOCH3 hydrate and Ru2(RCOO)4Cl (R = alkyl group having 1 to 3 carbon atoms).
[0063] Examples of ruthenium nitrosyl complexes include K2[RuCl5NO)], [Ru(NH3)5(NO)]Cl3, [Ru(OH)(NH3)4(NO)](NO3)2, and Ru(NO)(NO3)3.
[0064] The ruthenium compound is preferably ruthenium oxide, ruthenium nitrate, ruthenium chloride, ruthenium bromide, ruthenic acid, a salt of ruthenic acid, or a ruthenium nitrosyl complex, and more preferably ruthenium oxide or ruthenic acid.
[0065] The component supported on the carrier containing titanium oxide only needs to contain at least one selected from the group consisting of ruthenium and ruthenium compounds mentioned above, and may further contain a metal other than ruthenium, a metal compound other than ruthenium compounds, and the like.
[0066] In the present invention, in order to prevent substances that cause catalyst poisoning from being adsorbed on the catalyst surface, prevent the performance of the catalyst from being reduced, or prevent the sintering of the catalyst active sites, the catalyst is preferably a catalyst further loaded with at least one selected from the group consisting of metals other than ruthenium and metal compounds other than ruthenium compounds on a carrier comprising titanium oxide.
[0067] As the metal other than ruthenium, there is no particular restriction, and silicon, zirconium, aluminum, niobium, tin, copper, iron, cobalt, nickel, vanadium, chromium, molybdenum, tungsten, manganese, antimony, tellurium etc. can be listed. As the metal compound other than the ruthenium compound, there is no particular restriction, and the compound with the metal other than the above-mentioned ruthenium can be listed, preferably the oxide of the metal other than the above-mentioned ruthenium. The metal oxide can also be a composite oxide of multiple metal species. In addition, the catalyst can also be an alloy of a metal other than ruthenium and ruthenium, a catalyst comprising a composite oxide of a metal other than ruthenium and ruthenium on a carrier.
[0068] The catalyst is more preferably a catalyst in which at least one oxide selected from the group consisting of silicon oxide, zirconium oxide, aluminum oxide, niobium oxide, manganese oxide, antimony oxide, tellurium oxide and tin oxide is further supported on a carrier containing rutile crystalline titanium oxide.
[0069] The metal salt used to obtain the metal oxide is not particularly limited.
[0070] The content of at least one selected from the group consisting of ruthenium and ruthenium compounds in the catalyst is not particularly limited and is appropriately set, for example, preferably 1 to 20 mass %, more preferably 2 to 10 mass %, and further preferably 2 to 5 mass %, based on metallic ruthenium.
[0071] The content of at least one selected from the group including ruthenium and ruthenium compounds is: when the total amount of the component including at least one selected from the group including ruthenium and ruthenium compounds and the carrier is set to 100 mass%, based on metallic ruthenium, it is preferably 1 to 20 mass%, more preferably 2 to 10 mass%, and further preferably 2 to 5 mass%.
[0072] The content of the metal other than ruthenium and the metal compound other than the ruthenium compound in the catalyst is not particularly limited and can be appropriately set in consideration of the above content (supported amount) depending on the above purpose.
[0073] (Carrier)
[0074] The carrier can be any carrier containing titanium oxide, and can also contain other compounds described later. The crystal form of the titanium oxide constituting the carrier is not particularly limited, and can be any one of rutile crystal form, anatase crystal form, and brookite crystal form. In the present invention, the carrier is preferably composed of titanium oxide containing rutile crystal form titanium oxide. From the viewpoint of catalyst activity, the content of rutile crystal form titanium oxide in the titanium oxide contained in the carrier is preferably 20 mass % or more, more preferably 30 mass % or more, further preferably 80 mass % or more, and further preferably 90 mass % or more when the total amount of titanium oxide contained in the carrier is 100 mass %.
[0075] In the present invention, titanium oxide containing rutile crystalline titanium oxide refers to titanium oxide containing rutile crystals by measuring the ratio of rutile crystals and anatase crystals in titanium oxide by X-ray diffraction analysis. As an X-ray source, various radiation sources are used. For example, copper Kα rays and the like can be cited. When copper Kα rays are used, the ratio of rutile crystals and the ratio of anatase crystals are determined by the intensity of the diffraction peak of 2θ=27.5 degrees of the (110) plane and the intensity of the diffraction peak of 2θ=25.3 degrees of the (101) plane, respectively. The carrier used in the present invention is a carrier having the peak intensity of rutile crystals and the peak intensity of anatase crystals, or a carrier having the peak intensity of rutile crystals. That is, it can be a carrier having both the diffraction peak of rutile crystals and the diffraction peak of anatase crystals, or it can be a carrier having only the diffraction peak of rutile crystals.
[0076] Other compounds that may be included in the carrier include, for example, metal oxides other than titanium oxide, composite oxides of titanium oxide and other metal oxides, and mixtures of titanium oxide and other metal oxides. Examples of metal oxides other than titanium oxide include aluminum oxide, silicon oxide, and zirconium oxide.
[0077] Titanium oxide produced by a known method may be used, or a commercially available product may be used.
[0078] As a method for producing rutile crystalline titanium oxide, the following method can be mentioned.
[0079] Titanium tetrachloride is dropped into ice-cold water to dissolve, then neutralized with an aqueous ammonia solution at a temperature above 20°C to generate titanium hydroxide (orthotitanic acid), then the generated precipitate is washed with water to remove chloride ions, and then calcined at a temperature above 600°C (Catalyst Preparation Chemistry, 1989, p. 211, Kodansha);
[0080] A method of preparing a reaction gas by passing an oxygen-nitrogen mixed gas through a titanium tetrachloride evaporator, introducing the mixed gas into a reactor, and reacting the mixed gas at a temperature above 900°C (Catalyst Preparation Chemistry, 1989, p. 89, Kodansha);
[0081] A method in which titanium tetrachloride is hydrolyzed in the presence of ammonium sulfate and then calcined (e.g., Catalyst Engineering Lecture 10 Elements Catalyst Overview (Catalyst Engineering Lecture 10 Elements Catalyst Handbook), 1978, p. 254, Jiren Bookstore);
[0082] Method for calcining anatase-type titanium oxide (e.g., Metal Oxides and Composite Oxides (Metal Oxides and Composite Oxides), 1980, p. 107, Kodansha);
[0083] A method of heating and hydrolyzing an aqueous solution of titanium chloride; and
[0084] A method in which an aqueous solution of a titanium compound such as titanium sulfate or titanium chloride is mixed with a rutile crystalline titanium oxide powder, the mixture is subjected to heating hydrolysis or alkali hydrolysis, and then fired at a temperature of about 500°C.
[0085] The carrier can be obtained by shaping titanium oxide or the like into a desired shape. When the carrier contains a compound other than titanium oxide or the like, it can be obtained by shaping a mixture of titanium oxide and the compound other than titanium oxide or the like into a desired shape.
[0086] Next, the shape and the like of the catalyst of the present invention will be described.
[0087] The shape of the catalyst (carrier) is not particularly limited and can be appropriately set.
[0088] In a preferred embodiment of the present invention, when the catalyst is filled in a catalyst-filled region of a reaction tube described later to form a catalyst-filled layer, the catalyst has a honeycomb shape (honeycomb structure) that satisfies a filling volume ratio described later.
[0089] On the other hand, in another preferred embodiment of the present invention, for example, about the catalyst of the form formed by the component that supports ruthenic acid, various shapes can be adopted.As such shape, there is no particular restriction, for example, spherical granular, cylindrical pellet (pellet) shape, ring shape, honeycomb shape, monolith (monolith) shape, corrugated shape or the particle of the appropriate size of crushing classification after molding can be listed, microparticle etc. The shape of catalyst is preferably spherical granular, cylindrical pellet, ring shape, honeycomb shape, monolith shape, corrugated shape or granular etc., but from the viewpoint of the decomposition efficiency of nitrous oxide, more preferably ring shape, honeycomb shape.
[0090] In the present invention, the honeycomb structure refers to a "honeycomb structure" generally referred to as a honeycomb catalyst such as a honeycomb catalyst that is often used as an exhaust gas purification catalyst, and examples thereof include a structure in which a plurality of through holes densely arranged along a planar direction are perforated on a substrate such as a columnar body.
[0091] As a substrate, an appropriate shape is selected according to the shape of the catalyst filling area of the reaction tube, the filling scheme of the honeycomb structure, etc., and a columnar body, a block, a plate body, etc. can be listed. The opening shape of the through hole is not particularly limited, for example, polygons such as quadrilaterals and hexagons, circles, and ellipses can be listed. The arrangement of the through holes is not particularly limited, and is appropriately determined considering the opening shape. For example, in the plane direction of the substrate (usually a plane perpendicular to the axis), a series (parallel) configuration (Straight arrangement), a staggered arrangement (staggered arrangement), a honeycomb arrangement (honeycomb arrangement), etc. can be listed.
[0092] Examples of the honeycomb structure include circular holes arranged in parallel, staggered, and circular honeycomb, and polygonal square holes arranged in parallel, staggered, and square honeycomb.
[0093] The size of the catalyst (carrier) is not particularly limited and can be appropriately set.
[0094] When the catalyst is in the shape of spherical particles, cylindrical pellets, etc., from the viewpoint of catalyst activity, the catalyst diameter is preferably less than 10 mm. In addition, the catalyst diameter mentioned here refers to the diameter of the ball when it is spherical particles, the diameter of the cross section when it is cylindrical pellets, and the maximum diameter of the cross section when it is other shapes.
[0095] In a preferred embodiment of the present invention described above, the size of the catalyst is set to a size that satisfies the filling volume ratio described later when the catalyst is filled into the catalyst filling area of the reaction tube described later to form a catalyst filling layer. For example, the size is set to a size suitable for the catalyst filling area of the reaction tube, and is usually set to an outer dimension that is approximately the same as the inner dimension (inner diameter and length) of the catalyst filling area.
[0096] The opening diameter (also called cell size), the through-hole spacing (also called the thickness of the inner wall), the porosity, etc. of the through-holes in the honeycomb structure are appropriately determined, and in a preferred embodiment of the present invention, are determined by taking into account the filling volume rate, etc. For example, as the cell size, it can be set to 1 to 3 mm, preferably 1 to 2 mm. As the thickness of the inner wall, it can be set to 0.1 to 2 mm, preferably 0.2 to 1 mm. As the porosity ([(total area of through-holes opened on the surface of the honeycomb structure) / (apparent surface area of the honeycomb structure)]×100(%)), it can be set to 50 to 65%, preferably 50 to 62%. The cell size and the thickness of the inner wall can be determined by observing and measuring the surface of the honeycomb shape. The porosity can be calculated from the measured total area of the through-holes and the calculated apparent surface area.
[0097] In a preferred embodiment of the present invention described above, a honeycomb structure has a filling volume rate of 35 to 50% by volume when the catalyst filling area of the reaction tube described later is filled to form a catalyst filling layer. From the perspective of being able to further improve the decomposition efficiency of nitrous oxide, the filling volume rate is preferably 38 to 50% by volume. The filling volume rate of the honeycomb structure (catalyst) refers to the ratio (percentage) of the actual volume of the honeycomb structure to the apparent volume of the honeycomb structure. Here, the apparent volume of the honeycomb structure is generally synonymous with the volume of the catalyst filling area of the reaction tube. The apparent volume and the actual volume can be calculated from the various dimensions of the honeycomb structure by conventional methods.
[0098] In the present invention, the catalyst includes a solution having a honeycomb structure that satisfies the above-mentioned filling volume ratio by combining multiple catalysts (a solution in which multiple catalysts filled in the catalyst filling area form a honeycomb structure that satisfies the above-mentioned filling volume ratio as a whole), but preferably has a honeycomb structure that satisfies the above-mentioned filling volume ratio alone. In this case, the above-mentioned filling volume ratio represents the catalyst filling ratio of the catalyst alone, and becomes synonymous with the ratio (percentage) of the actual volume to the apparent volume. In addition, in the case of combining multiple catalysts, it is preferred that the honeycomb structure of each catalyst satisfies the above-mentioned filling volume ratio.
[0099] [Method for producing catalyst]
[0100] The catalyst can be prepared, for example, by impregnating a carrier containing titanium oxide in a solution containing at least one component selected from the group including ruthenium and ruthenium compounds to allow the component containing at least one component selected from the group including ruthenium and ruthenium compounds to adhere to the carrier, and then drying.
[0101] The carrier may be formed into the various shapes described in the above-mentioned shape of the catalyst, or may be crushed, formed, etc. after supporting the above-mentioned components to form the above-mentioned catalyst shape.
[0102] The solvent in the solution containing at least one component selected from the group consisting of ruthenium and ruthenium compounds is not particularly limited, and water, ethanol, etc. can be used. The calcination may be performed after drying.
[0103] When the catalyst contains ruthenium oxide, for example, it can be obtained by a method comprising the following steps: a step of immersing a carrier containing titanium oxide in a solution containing ruthenium halide to load the ruthenium halide on the carrier; a step of drying the supported material in which the ruthenium halide is supported on the carrier; and a step of calcining the dried material.
[0104] The catalyst can be used after being diluted with an inert substance.
[0105] In the present invention, a preferred method for producing the catalyst includes a method comprising the following steps (1) and (2).
[0106] Step (1): a step of contacting a support containing titanium oxide with a solution containing an alkali metal salt of ruthenate and water;
[0107] Step (2): a step of contacting the support containing titanium oxide and ruthenate alkali metal salt obtained in step (1) with an acidic aqueous solution.
[0108] <Step (1)>
[0109] The support and the alkali metal salt of ruthenate used in step (1) are as described above.
[0110] The content of the alkali ruthenate in the solution comprising the alkali ruthenate and water is not particularly limited, but is preferably 1 to 10% by mass, more preferably 2 to 8% by mass, and further preferably 3 to 6% by mass based on metallic ruthenium. The solution may also contain components other than the alkali ruthenate, for example, metals other than ruthenium described in the components loaded on the carrier, and further organic solvents such as alcohols may be cited to allow the solution to be well fused with the carrier.
[0111] The contact method and conditions in step (1) are not particularly limited and can be appropriately set. As the contact method, various methods for making the components containing the above-mentioned ruthenium etc. supported on the carrier as a catalyst manufacturing method can be applied, for example, a method of immersing the carrier in the above-mentioned solution, a coating method of spraying or coating the above-mentioned solution on the carrier, etc. can be listed. The amount of solution used at this time is preferably 0.1 to 20 ml relative to 1 g of the carrier, and more preferably 0.3 to 10 ml. As contact conditions, for example, conditions of contacting at 5 to 40° C. (preferably 10 to 30° C.) for 1 to 60 minutes (preferably 5 to 20 minutes) can be listed.
[0112] In this manner, the alkali metal salt of ruthenate is supported or adsorbed on the support containing titanium oxide, thereby obtaining a support containing titanium oxide and the alkali metal salt of ruthenate.
[0113] The support containing titanium oxide and ruthenate alkali metal salt obtained in step (1) corresponds to the catalyst precursor of the present invention.
[0114] <Step (2)>
[0115] In step (2), an acidic aqueous solution is used. The acid used in the preparation of the acidic aqueous solution is not particularly limited, but is generally an inorganic acid from the aspect of reactivity with the alkali metal salt of ruthenate, and examples thereof include nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid, etc., preferably nitric acid.
[0116] The content (concentration) of the acid in the acidic aqueous solution is not particularly limited, but is, for example, preferably 0.1 to 10 N (equivalent), more preferably 0.2 to 5 N, and further preferably 0.5 to 2 N. The acidic aqueous solution may contain components other than the acid.
[0117] The contact method in step (2) is not particularly limited, and for example, the contact method of step (1) can be appropriately applied. The amount of the acidic aqueous solution used at this time is appropriately determined in consideration of the acid content, for example, the acid is preferably 1 to 200 moles, more preferably 5 to 50 moles, relative to 1 mole of ruthenic acid alkali metal salt. As the contact conditions, the conditions under which the ruthenic acid alkali metal salt reacts with the acid are set, for example, the conditions of contact at 10 to 100° C. (preferably 20 to 80° C.) for 1 to 60 minutes (preferably 5 to 20 minutes) can be listed. In order to contact at a temperature above room temperature, for example, a method of heating the carrier and / or the acidic aqueous solution used to a specified temperature in advance, a method of heating the two after contacting, etc. can be listed.
[0118] In this manner, the alkali metal hydrochloric acid of ruthenate supported on the carrier can be decomposed into ruthenic acid, thereby producing a catalyst supporting a component containing ruthenic acid.
[0119] <Other Processes>
[0120] The method for producing the catalyst of the present invention may also include steps other than the above-mentioned steps (1) and (2). For example, the steps include a step of forming a carrier, a step of drying the carrier containing titanium oxide and ruthenate alkali metal salt obtained in step (1), a step of drying the catalyst obtained in step (2), and further a step of calcining.
[0121] The step of molding the carrier is not particularly limited as long as it can be molded into the above-mentioned shape. In the present invention, it is preferred that the carrier is molded into the above-mentioned honeycomb structure.
[0122] The method and conditions in the drying step are not particularly limited, and common methods and conditions can be applied. For example, air drying at 5 to 120° C., air drying, and heat drying can be mentioned.
[0123] The method and conditions in the above-mentioned firing step are not particularly limited, and general methods and conditions can be applied, for example, heating treatment at 120° C. to 400° C. in an oxygen-containing gas or inert gas atmosphere.
[0124] [Catalyst filled reaction tube]
[0125] The catalyst-packed reaction tube of the present invention is the catalyst-packed reaction tube having a catalyst-packed layer filled with the catalyst of the present invention, wherein the filling volume ratio of the catalyst in the catalyst-packed layer is set to 35 to 50% by volume. The catalyst-packed reaction tube can process the reaction gas supplied to the reaction tube by the catalyst (catalyst-packed layer) filled therein, and can efficiently decompose nitrous oxide when treating nitrous oxide-containing gas.
[0126] The shape and size of the catalyst-filled reaction tube are appropriately set. As the shape of the catalyst-filled reaction tube, for example, as long as it is a reaction tube used in a continuous contact method, tubular or tower-shaped reaction tubes such as metal tubes and column towers can be listed. The cross-sectional shape of the reaction tube is usually set to a circular ring shape, but it can also be set to a prismatic ring shape, for example. Although the size of the catalyst-filled reaction tube and the catalyst-filled area cannot be uniquely determined by the reaction scale, reaction conditions, etc., for example, as an inner diameter, it can be set to 5 to 10000 mm, preferably 20 to 5000 mm. The length of the catalyst-filled area cannot be uniquely determined either, but for example, it can be set to 5 to 45000 mm, preferably 20 to 11250 mm. The material forming the reaction tube can be any material that is resistant to the reaction gas, such as the nitrous oxide-containing gas described later, and materials such as stainless steel with iron and glass as the main components can be listed.
[0127] The catalyst filled into the catalyst-filled reaction tube is filled to a state satisfying the above-mentioned filling volume rate according to the shape, size, etc. of the catalyst as described above. For example, in a preferred embodiment of the present invention, the catalyst is filled (arranged) in the catalyst-filled area in such a way that the axis of the through hole of the honeycomb structure is along the axial direction of the reaction tube. Here, making the axis of the through hole along the axial direction of the reaction tube is not limited to a parallel scheme, and includes a scheme in which the axis of the through hole is inclined at an angle of, for example, 45° or less relative to the axial direction of the reaction tube. On the other hand, in another preferred embodiment of the present invention (the case in which the catalyst is not a honeycomb structure but the above-mentioned cylindrical granular shape, etc.), its shape, size, etc. are appropriately adjusted so that when the catalyst is filled into the catalyst-filled area and the catalyst-filled layer is made, the catalyst is filled in such a way that the above-mentioned filling volume rate is achieved.
[0128] The catalyst-packed reaction tube is preferably used together with a heater for heating the catalyst-packed reaction tube, a line (supply pipe) for introducing a reaction gas into the catalyst-packed reaction tube, a line (discharge pipe) for discharging a post-reaction gas from the catalyst-packed reaction tube, and the like.
[0129] [Method for decomposing nitrous oxide]
[0130] The method for decomposing nitrous oxide of the present invention (hereinafter, sometimes referred to as "the decomposition method of the present invention") comprises a step of contacting the catalyst of the present invention with a nitrous oxide-containing gas containing nitrous oxide (gas) (hereinafter, sometimes referred to as a contact step), or a step of circulating the nitrous oxide-containing gas containing nitrous oxide (gas) in a catalyst-filled reaction tube. By the contact or circulation step, as described later, nitrous oxide in the nitrous oxide-containing gas can be efficiently decomposed into nitrogen molecules (usually nitrogen gas) and oxygen molecules (usually oxygen gas).
[0131] <Catalyst>
[0132] The catalyst used in the decomposition method of the present invention is as described above, and the use mode is not particularly limited. For example, it is preferable to use a catalyst having a honeycomb structure, and it is more preferable to use a catalyst-filled reaction tube filled with the catalyst having a honeycomb structure.
[0133] <Gas containing nitrous oxide>
[0134] As the nitrous oxide-containing gas used in the contacting step, as long as it contains nitrous oxide, it may also contain an inert gas as a diluent gas. The nitrous oxide-containing gas preferably contains at least one gas selected from nitrous oxide, nitrogen, carbon monoxide, carbon dioxide, water vapor, oxygen, hydrogen, ammonia, nitric oxide, nitrogen dioxide, and hydrocarbons (including saturated hydrocarbons and unsaturated hydrocarbons). Regarding these gases, the content (concentration) in the nitrous oxide-containing gas is not particularly limited and can be appropriately set. For example, it can be set to the same content as the appropriate nitrous oxide-containing gas described later.
[0135] The nitrous oxide-containing gas may contain a liquid. In the decomposition method of the present invention, the nitrous oxide-containing gas may be a gas at least during the period of contact with the catalyst (under the reaction conditions), and may be a liquid before contact, or may be a mixture of gas and liquid.
[0136] The nitrous oxide-containing gas (sometimes referred to as a suitable nitrous oxide-containing gas) used in the preferred contact step described later may contain nitrous oxide, water vapor and ammonia, and may contain one or more gases other than these gases. Such a gas may include, for example, various gases such as oxygen, helium, argon, nitrogen and carbon dioxide, and further may include the reducing gas described later.
[0137] The content (concentration) of each component in a suitable nitrous oxide-containing gas is not particularly limited and can be appropriately set, but except for components that bring special effects, it is usually efficient to use almost directly the value specific to the factory that discharges the nitrous oxide-containing gas. Therefore, for example, the molar concentration of nitrous oxide in a suitable nitrous oxide-containing gas is generally preferably 0.002 to 10 mol%. The molar concentration of water vapor is generally preferably 0.1 to 10 mol%. From the perspective of the decomposition efficiency of nitrous oxide, the molar concentration of ammonia in a suitable nitrous oxide-containing gas is preferably 0.0002 mol% or more, preferably 1 mol% or less. The molar concentration of ammonia is more preferably 0.0002 to 0.5 mol%, and further preferably 0.0002 to 0.2 mol%.
[0138] The content ratio of ammonia to water vapor [ammonia / water vapor] contained in a suitable nitrous oxide-containing gas is not particularly limited and can be appropriately set, but is preferably 0.0010 or more in terms of the decomposition efficiency of nitrous oxide. It is more preferably 0.0010 to 0.050 in terms of the molar ratio, and is more preferably 0.0010 to 0.030, and is further preferably 0.0010 to 0.010 in terms of being able to suppress or avoid the problem of residual ammonia (emission to the atmosphere, implementation of removal operations). In addition, the content ratio of ammonia to nitrous oxide [ammonia / nitrous oxide] contained in a suitable nitrous oxide-containing gas is not particularly limited and can be appropriately set, but is preferably 0.005 to 10 in terms of the molar ratio.
[0139] When the suitable nitrous oxide-containing gas contains oxygen, the content of oxygen in the suitable nitrous oxide-containing gas is not particularly limited and can be appropriately set, but is preferably 0.01 to 10000 times by mole relative to the content of ammonia in the suitable nitrous oxide-containing gas. When the suitable nitrous oxide-containing gas does not contain oxygen, it can be obtained by, for example, mixing a suitable nitrous oxide-containing gas and an oxygen-containing gas. As the oxygen-containing gas, air can be cited.
[0140] Suitable nitrous oxide-containing gas can also contain reducing gas in order to further improve the decomposition efficiency of nitrous oxide. In addition, similarly, in order to further improve the decomposition efficiency of nitrous oxide, it can also contain saturated hydrocarbon gas, which becomes a raw material for reacting with oxygen contained in nitrous oxide-containing gas or oxygen generated in the reactor to produce reducing gas such as carbon monoxide gas. In terms of the decomposition efficiency of nitrous oxide, it is preferred to make the suitable nitrous oxide-containing gas contain reducing gas. As a reducing gas, as long as it is a reducing gas other than ammonia, the reducing gas used in the general contact reduction method can be used without special restrictions. For example, unsaturated hydrocarbon gases such as ethylene, propylene, α-butene, β-butene, carbon monoxide gas, hydrogen, and gases of alcohol compounds such as methanol, ethanol, propanol, butanol, etc. can be listed. Among them, at least one of carbon monoxide gas, unsaturated hydrocarbon gas and hydrogen is preferred. In addition, as a saturated hydrocarbon gas that becomes a raw material for producing reducing gases such as carbon monoxide gas, methane, ethane, propane, n-butane, etc. can be listed. Preferred saturated hydrocarbon gases include ethane, propane, and n-butane. In order to contain the saturated hydrocarbon gas, for example, a mixture such as natural gas, liquefied natural gas, and liquefied petroleum gas can be used.
[0141] The content of the reducing gas or saturated hydrocarbon gas in the suitable nitrous oxide-containing gas is not particularly limited and can be appropriately set. For example, the molar concentration of the reducing gas or saturated hydrocarbon gas in the suitable nitrous oxide-containing gas is 0.001 to 1 mol%. The molar ratio of the reducing gas or saturated hydrocarbon gas to water vapor in the suitable nitrous oxide-containing gas [reducing gas or saturated hydrocarbon gas / water vapor] is preferably 0.0003 to 0.03. In addition, the molar ratio of the reducing gas or saturated hydrocarbon gas contained in the suitable nitrous oxide-containing gas to the content ratio of nitrous oxide [reducing gas or saturated hydrocarbon gas / nitrous oxide] is preferably 0.01 to 100.
[0142] The nitrous oxide-containing gas can be prepared by appropriately mixing nitrous oxide, water vapor, ammonia, and the above-mentioned gases other than these. In addition, various waste gases discharged from chemical manufacturing facilities (plants) can also be used. For example, the gas discharged from chemical manufacturing facilities such as nitric acid manufacturing plants, ε-caprolactam manufacturing plants, and adipic acid manufacturing plants, in addition to nitrous oxide, mostly also contains water vapor and ammonia, and even oxygen, which can be effectively used in the preferred contact process described later. In particular, when the waste gas meets the above-mentioned range of content, content ratio, etc., it is preferred that it can be directly applied to the preferred contact process without adjusting the content, etc.
[0143] <Contact process>
[0144] The contact process can be any process as long as it is a process of contacting the catalyst with the nitrous oxide-containing gas containing nitrous oxide, and the contact process in the known method for decomposing nitrous oxide can be applied. As a contact process in the known method for decomposing nitrous oxide, for example, the method (process) of contacting the catalyst with nitrous oxide in the coexistence of a reducing gas described in Patent Document 1 can be cited. In addition, the contact process can also be carried out by circulating the nitrous oxide-containing gas containing nitrous oxide in the catalyst-filled reaction tube of the present invention. The contact process in the present invention is preferably a process (sometimes referred to as a "preferred contact process") of contacting the catalyst (including the catalyst filled in the catalyst-filled reaction tube used in the above-mentioned circulation process) with the nitrous oxide-containing gas containing nitrous oxide, water vapor and ammonia.
[0145] The method of contacting the nitrous oxide-containing gas with the catalyst is not particularly limited, and may be, for example, a batch method or a continuous method, but the continuous method is preferred from the perspective of reaction efficiency. Examples of the continuous method include a fixed bed method and a fluidized bed method.
[0146] In the contact step, nitrous oxide in the nitrous oxide-containing gas contacts the catalyst, and a decomposition reaction of nitrous oxide represented by the following formula occurs even in the presence of water vapor, whereby nitrous oxide is efficiently decomposed into nitrogen molecules and oxygen molecules.
[0147] Decomposition reaction of nitrous oxide: N2O→N2+1 / 2O2
[0148] In the above-mentioned preferred contact process, ammonia in the nitrous oxide-containing gas further promotes the decomposition reaction of nitrous oxide. Although the details of its mechanism of action are not clear, it is considered to be as follows. For example, it is speculated that in the presence of a catalyst that exhibits a reducing effect such as a catalyst loaded with ruthenium, ammonia reacts with nitrous oxide on the catalyst surface, and nitrous oxide can be decomposed into nitrogen molecules and water molecules and further promote the decomposition reaction of nitrous oxide. On the other hand, it is speculated that in the presence of a catalyst that does not exhibit a reducing effect such as a catalyst loaded with ruthenium oxide, oxygen atoms can be removed from the catalyst surface by reacting with oxygen atoms remaining on the catalyst surface, so that the catalyst activity is continued (inhibiting the deactivation of the catalyst), and the above-mentioned decomposition reaction can be promoted.
[0149] When a known process is applied as the contact process, the contact method and contact conditions can be appropriately adopted as appropriate methods and conditions that can be adopted in each process.
[0150] There are no particular restrictions on the contact conditions in the preferred contact step, and for example, the following conditions can be cited. The contact temperature (reaction temperature) is appropriately determined, but is preferably 500°C or less from the viewpoint of catalyst activity degradation, and is preferably 100°C or more from the viewpoint of reaction rate. The contact temperature is preferably 200-450°C, and more preferably 250-400°C. The supply rate of the nitrous oxide-containing gas relative to the weight of the catalyst in the continuous contact method is not particularly limited and is appropriately determined, for example, as a flow rate at 0°C and 0.1013 MPa (absolute) relative to 1 g of the catalyst, preferably 10-10000 cm 3 / min, more preferably 50 to 5000cm 3 / minute. The contact time is appropriately determined according to the nitrous oxide concentration in the nitrous oxide-containing gas or the supply rate, the contact temperature, etc. The reaction pressure varies according to the contact temperature, the supply rate of the nitrous oxide-containing gas, or the pressure of the external gas around the reactor, but is preferably a pressure higher than that of the external gas, preferably 0.08 to 1 MPa (absolute) in absolute pressure, and more preferably 0.09 to 0.7 MPa (absolute) in absolute pressure.
[0151] <Other Processes>
[0152] The decomposition method of the present invention may include steps other than the contact step, for example, a step of adjusting the content of the components of the nitrous oxide-containing gas, a step of introducing oxygen or a reducing gas into the nitrous oxide-containing gas, etc.
[0153] The decomposition method of the present invention can decompose nitrous oxide efficiently. In particular, in a continuous process, by allowing the nitrous oxide-containing gas to circulate (pass) through the catalyst, nitrous oxide can be decomposed efficiently, and the emission of nitrous oxide can be suppressed. For example, in the embodiments described below, as the concentration reduction rate of nitrous oxide in the reaction gas, a high concentration reduction rate of 50% or more, preferably 70% or more can be achieved, and as the decomposition rate of nitrous oxide, a high decomposition rate of 3.0 / second or more, preferably 5.0 / second or more can be achieved. In addition, in the preferred contact process, ammonia in the nitrous oxide-containing gas can also be decomposed efficiently, and the emission of ammonia can be suppressed.
[0154] The decomposition method of the present invention can be used in various fields and applications for decomposing and removing nitrous oxide, for example, in chemical manufacturing facilities. In particular, it can be suitably used in chemical manufacturing facilities such as nitric acid manufacturing plants, ε-caprolactam manufacturing plants, and adipic acid manufacturing plants that emit gas containing nitrous oxide, ammonia, and water vapor.
[0155] When the decomposition method of the present invention is applied to an existing manufacturing facility, the installation position of the device for performing the decomposition method of the present invention is not particularly limited, and is usually installed at the last stage in the flow direction of the exhaust gas, such as the first stage of the discharge tower. Specifically, in the case of a nitric acid manufacturing facility, it is installed at the last stage of the denitration reactor.
[0156] Example
[0157] Hereinafter, although the Example of this invention is shown, this invention is not limited to these.
[0158] [Example 1] Preparation of catalyst
[0159] <Example 1-1: Preparation of H2RuO4 / TiO2 Catalyst 1>
[0160] As shown below, H2RuO4 / TiO2 catalyst 1 was prepared.
[0161] A titanium oxide forming precursor 1 (cubic shape with a length of 20 mm, a width of 20 mm, and a height of 20 mm, with through holes arranged in parallel in the vertical and horizontal directions, a quadrilateral opening shape of the through holes, a cell size of 1.3 mm, an inner wall thickness of 0.5 mm, and an opening rate of 50%) formed by extruding titanium oxide powder (manufactured by Showa Denko K.K.) into a honeycomb shape was sintered at 600° C. for 2 hours to obtain a support 1 (specific surface area: 15 m 2 / g, 100% rutile crystal form). The specific surface area of the support 1 was measured by the BET 1-point method performed by nitrogen adsorption at 77K.
[0162] The support 1 maintains the shape and size of the titanium oxide molded precursor 1. The size of the titanium oxide molded precursor 1 is measured or calculated as described above (the same shall apply hereinafter).
[0163] Next, the carrier 1 was immersed in about 50 ml of a sodium ruthenate aqueous solution (manufactured by Furuya Metals Co., Ltd., a Na2RuO4 aqueous solution, about 15°C) prepared so that the Ru content was 5.7% by mass. After 10 minutes, the carrier 1 was pulled out of the sodium ruthenate aqueous solution and excess water was blown off with a blower. The obtained carrier 1 was placed on a laboratory bench at room temperature (about 15°C) and air-dried until the weight no longer decreased, thereby obtaining a catalyst precursor 1.
[0164] The obtained catalyst precursor 1 was heated to about 60°C in an oil bath and immersed in a 2N nitric acid aqueous solution stirred by a stirrer. After bubbles were no longer generated, the catalyst precursor 1 was pulled out and air-dried at room temperature (about 15°C) until the weight no longer decreased, thereby producing a H2RuO4 / TiO2 catalyst 1 having a honeycomb structure. The catalyst 1 maintained the shape and size of the titanium oxide shaped precursor 1.
[0165] <Example 1-2: Preparation of H2RuO4 / TiO2 Catalyst 2>
[0166] A H2RuO4 / TiO2 catalyst 2 having a honeycomb structure was obtained by the same method as in Example 1, except that a titanium oxide forming precursor 2 (cubic shape with a length of 19 mm, a width of 19 mm, and a height of 20 mm, through holes arranged in parallel along the length and width directions, the opening shape of the through holes being a quadrilateral, the unit cell size being 1.0 mm, the thickness of the inner wall being 0.25 mm, and the opening rate being 62%) was used. The catalyst 2 maintained the shape and size of the titanium oxide forming precursor 2.
[0167] <Example 1-3: Preparation of RuO2 / TiO2 Catalyst 3>
[0168] RuO2 / TiO2 catalyst 3 was prepared as follows.
[0169] A titanium oxide forming precursor 1 (cubic shape with a length of 20 mm, a width of 20 mm, and a height of 20 mm, with through holes arranged in parallel in the vertical and horizontal directions, a quadrilateral opening shape of the through holes, a cell size of 1.3 mm, an inner wall thickness of 0.5 mm, and an opening rate of 50%) formed by extruding titanium oxide powder (manufactured by Showa Denko K.K.) into a honeycomb shape was sintered at 600° C. for 2 hours to obtain a support 1 (specific surface area: 15 m 2 / g, 100% rutile crystal form). The specific surface area of the support 1 formed of titanium oxide was measured by the BET 1 point method performed by nitrogen adsorption at 77 K. The support 1 maintained the shape and size of the titanium oxide shaped precursor 1 .
[0170] Using RuCl3·nH2O (manufactured by Furuya Metal Co., Ltd., with a Ru content of 40% by mass), the carrier 1 was immersed in about 50 ml of a ruthenium chloride aqueous solution prepared in such a way that the Ru content was 5.7% by mass. After 10 minutes, the carrier 1 was pulled out of the ruthenium chloride aqueous solution and the excess water was blown off with a blower. Thereafter, the obtained carrier 1 was placed on a laboratory bench at room temperature (about 15°C) and air-dried until the weight no longer decreased, thereby obtaining a catalyst precursor 3.
[0171] The obtained catalyst precursor 3 was filled into a quartz glass tube equipped with a jacket for measuring the internal temperature, and then heated at 500 cm in an electric tubular furnace. 3The temperature of the quartz glass tube was raised to 275°C under air circulation (0°C, 0.1013 MPa (absolute)) / min, and then the temperature was maintained for 2 hours to perform sintering. The sintered catalyst precursor 3 was immersed in 130 g of a 19 mass % potassium iodide aqueous solution at room temperature for 1 hour, and then immersed in 150 g of ion exchange water at room temperature for 6 times to perform washing. The obtained solid was placed on a laboratory bench at room temperature (about 15°C) and air-dried until the weight no longer decreased, thereby obtaining a RuO2 / TiO2 catalyst 3 having a honeycomb structure.
[0172] <Example 1-4: Preparation of RuO2 / TiO2 Catalyst 4>
[0173] A RuO 2 / TiO 2 catalyst 4 having a honeycomb structure was obtained in the same manner as in Example 3 except that an aqueous ruthenium chloride solution adjusted so that the Ru content was 2.9 mass % was used.
[0174] <Comparative Example 1-1: Preparation of RuO2 / TiO2 Catalyst C1>
[0175] RuO2 / TiO2 catalyst C1 was prepared as follows.
[0176] Titanium oxide molded bodies (cylindrical pellets with a diameter of 3 mm and a length of 3 to 6 mm) obtained by extruding titanium oxide powder (produced by Showa Denko K.K.) were sintered at 600°C for 3 hours in a muffle furnace to obtain a support (specific surface area: 15 m 2 / g, 100% rutile crystal form). The specific surface area of the support composed of titanium oxide was measured by the BET 1-point method performed by nitrogen adsorption at 77K.
[0177] 0.76 g of ruthenium chloride hydrate (manufactured by Guwu Metal Co., Ltd., RuCl3·nH2O, Ru content of 40% by mass) was dissolved in 2.0 g of ion exchange water. The obtained solution was impregnated in 9.7 g of a support formed by titanium oxide by incipient wetness, and then air-dried overnight at room temperature (about 15° C.) in an air atmosphere to obtain a titanium oxide solid loaded with ruthenium chloride hydrate.
[0178] The obtained titanium oxide solid was filled into a quartz glass tube equipped with a sheath for measuring the internal temperature, and then heated at 200 cm using an electric tubular furnace. 3The temperature inside the quartz glass tube was raised to 275°C under air circulation (0°C, 0.1013 MPa (absolute)) / min, and then the temperature was maintained for 2 hours to perform sintering, thereby obtaining 10 g of RuO2 / TiO2 catalyst C1 containing ruthenium oxide in the form of cylindrical pellets.
[0179] <Comparative Example 1-2: Preparation of RuO2 / TiO2 Catalyst C2>
[0180] RuO2 / TiO2 catalyst C2 was prepared as shown below.
[0181] The RuO 2 / TiO 2 catalyst C1 was crushed with a magnetic mortar, and sieved so that the size of the crushed product was 0.5 mm or more and less than 1 mm, thereby obtaining a RuO 2 / TiO 2 catalyst C2.
[0182] [Example 2] Decomposition of nitrous oxide
[0183] <Examples 2-1 to 2-4>
[0184] (Preparation of Catalyst-Filled Reaction Tube)
[0185] For each of the H2RuO4 / TiO2 catalysts 1 and 2, and RuO2 / TiO2 catalysts 3 and 4 prepared in the above-mentioned Examples 1-1 to 1-4, the ends of the honeycomb shape in the horizontal direction were cut to form a cylindrical shape with a diameter of about 20 mm and a height of about 20 mm, while maintaining the flow path (through hole) connecting the gas inlet and outlet of the honeycomb shape in the vertical direction. It was filled into a quartz glass reaction tube (inner diameter 21 mm) with a sleeve for measuring the internal temperature in such a way that the flow path connecting the inlet and outlet of the honeycomb shape was in the same direction as the gas flow of the reaction tube. After that, quartz wool was filled between the inner wall of the reaction tube and the outer periphery of the catalyst, and it was sealed in such a way that it was difficult for the gas to flow between the inner wall of the reaction tube and the outer periphery of the catalyst. In this way, a catalyst-filled reaction tube having a catalyst-filled layer (inner diameter 21 mm, length about 20 mm) filled with catalyst was prepared. Table 1 shows the filling amount (g) and filling volume ratio (%) of the catalyst filled in the catalyst-filled layer.
[0186] Here, the filling volume of the catalyst-filled layer is the same as the filling volume ratio of the catalyst, and the value of 100% - opening ratio (%) is used.
[0187] (Decomposition reaction of nitrous oxide)
[0188] The jacket was arranged so that its front end was in contact with the upper part of the filled catalyst, and the gas temperature at the entrance of the catalyst layer could be measured. The catalyst-filled reaction tube was placed in an electric furnace and heated at normal pressure (0.1 MPa (absolute)) and 1500 cm 3 The temperature of the quartz glass tube was raised to 280°C under a nitrogen flow of (0°C, 0.1013 MPa (absolute)) / min. Then, at the same pressure and temperature, the gas in contact with the catalyst was switched from nitrogen to a gas containing 0.1% by volume of nitrous oxide and 2.7% by volume of oxygen (flow rate: 1500 cm 3 (0°C, 0.1013 MPa (absolute) / min), the decomposition reaction of nitrous oxide was carried out. The remainder of the nitrous oxide-containing gas was nitrogen. The reaction outlet gas (reaction-post-gas) from the reaction tube was analyzed 1 hour after the start of the decomposition reaction of nitrous oxide.
[0189] (Calculation of Nitrous Oxide Concentration Reduction Rate)
[0190] The nitrous oxide content C in the nitrous oxide-containing gas was measured using a gas chromatograph (Varian, Micro GC (detector: Micro TCD, column: CP-PoraPLOT Q10m)). B and the nitrous oxide content C in the reaction outlet gas A The reduction rate of nitrous oxide concentration was calculated from the analyzed nitrous oxide concentration by the following formula. The results are shown in Table 2.
[0191] Nitrous oxide concentration reduction rate (%) = [(C B -C A ) / C B ]×100
[0192] (Calculation of Decomposition Rate of Nitrous Oxide)
[0193] Based on the reduction rate of the nitrous oxide concentration, the decomposition rate of nitrous oxide was calculated from the following formula, assuming that the decomposition reaction of nitrous oxide was a single reaction. The results are shown in Table 2.
[0194] Decomposition rate of nitrous oxide ( / second) = -ln[1-(reduction rate of nitrous oxide concentration) / 100]÷(contact time between catalyst and nitrous oxide-containing gas)
[0195] Here, ln represents conversion to natural logarithm. In addition, the contact time between the catalyst and the nitrous oxide-containing gas is calculated by obtaining the reciprocal of the value obtained by dividing the gas flow rate per 1 second by the volume of the catalyst filling layer [cross-sectional area of the quartz glass reaction tube (inner diameter 21 mm) × catalyst height]. The contact time between the catalyst and the nitrous oxide-containing gas is shown in the "Contact Time" column of Table 1.
[0196] <Comparative Example 2-1>
[0197] The decomposition reaction and analysis of nitrous oxide were carried out in the same manner as in Examples 2-1 to 2-4, except that 5.0 g of the RuO2 / TiO2 catalyst C1 produced in Comparative Example 1-1 was directly filled in the catalyst filling area without changing its form. The reaction conditions and results are shown in Tables 1 and 2. The filling volume ratio (%) of the catalyst was calculated by the following formula.
[0198] Catalyst filling volume ratio (%) = Catalyst volume (cm 3 / g) / filling layer volume (cm 3 / g)×100
[0199] Here, the catalyst volume is calculated by using the loose bulk density of the RuO2 / TiO2 catalyst C1 of 1.26 g / cm when a 50 ml volume measuring cylinder with an inner diameter of 20 mm is used. 3 The volume of the packed layer is obtained by taking 42 shaped bodies of RuO2 / TiO2 catalyst C1 and dividing them by their shapes. The calculated volume was divided by the weight of 42 pieces, 2.49 g.
[0200] <Comparative Example 2-2>
[0201] 0.1 g of RuO2 / TiO2 catalyst C2 was filled in a quartz glass reaction tube (inner diameter 8 mm) equipped with a jacket for measuring the internal temperature. The filling volume ratio (%) of RuO2 / TiO2 catalyst C2 was calculated by the following formula.
[0202] Catalyst filling volume ratio (%) = Catalyst volume (cm 3 / g) / filling layer volume (cm 3 / g)×100
[0203] Here, the catalyst volume is calculated by using the loose bulk density of the RuO2 / TiO2 catalyst C2 (0.86 g / cm) using a 5 ml volume measuring cylinder with an inner diameter of 10 mm. 3The packed layer volume was obtained by taking 181 particles of RuO2 / TiO2 catalyst C2 and dividing the volume when the particle shape was assumed to be a sphere with a diameter of 0.75 mm by the weight of 181 particles, 0.10 g.
[0204] The jacket was arranged so that its front end was in contact with the upper part of the filled catalyst, and the gas temperature at the entrance of the catalyst layer could be measured. The catalyst-filled reaction tube was placed in an electric furnace and heated at normal pressure (0.1 MPa (absolute)) and 100 cm 3 The temperature of the quartz glass tube was raised to 280°C under a helium flow of (0°C, 0.1013 MPa (absolute)) / min. Then, at the same pressure and temperature, the gas in contact with the catalyst was switched from nitrogen to a gas containing 0.1% by volume of nitrous oxide and 2.7% by volume of oxygen (flow rate: 100 cm 3 (0°C, 0.1013 MPa (absolute) / min), the decomposition reaction of nitrous oxide was carried out. The rest of the nitrous oxide-containing gas was helium. The reaction outlet gas (reaction-post-gas) from the reaction tube 30 minutes after the start of the decomposition reaction of nitrous oxide was analyzed.
[0205] The concentration reduction rate (%) of nitrous oxide and the decomposition rate ( / sec) of nitrous oxide were calculated by the same method as in Example 1-1. Tables 1 and 2 show the reaction conditions and the results.
[0206] <Determination of Ru Content in Catalyst>
[0207] The catalysts after the reaction of Examples 2-1 to 2-4 and Comparative Example 2-1 were all recovered and crushed into powder using a magnetic mortar. The powdered samples were placed in the sample filling section. The trace powder holder was covered with a polyester film of 0.6 μm thickness, and SQX calculation was performed with a wavelength dispersive fluorescence X-ray analyzer (ZSXprimusII manufactured by Rigaku Corporation) to obtain a semi-quantitative value of Ru concentration. The results are shown in Table 1. Here, the Ru content of RuO2 / TiO2 catalyst C2 was set to the same value as that of RuO2 / TiO2 catalyst C1.
[0208] [Table 1]
[0209]
[0210] [Table 2]
[0211]
[0212] It is clear from the results shown in Tables 1 and 2 that the catalysts of Comparative Examples 1-1 and 1-2, which have a filling volume ratio exceeding 50 volume % when constituting the catalyst filling layer and do not have a honeycomb structure, and the catalyst-filled reaction tube using the catalysts of these comparative examples, have a small reduction in nitrous oxide concentration and a slow decomposition rate in the nitrous oxide decomposition method, and cannot efficiently decompose nitrous oxide.
[0213] In contrast, it is known that the catalysts of Examples 1-1 to 1-4 having a honeycomb structure with a filling volume ratio of 35 to 50% by volume when constituting a catalyst filling layer, and the catalyst-filled reaction tube using the catalysts of these Examples, in the method for decomposing nitrous oxide, have a large reduction in the concentration of nitrous oxide and a high decomposition rate, and can decompose nitrous oxide efficiently. In particular, the higher the filling volume ratio within the range specified in the present invention, the more efficiently nitrous oxide can be decomposed, but if it exceeds the range specified in the present invention, the decomposition efficiency of nitrous oxide will be significantly reduced. It is known that in order to improve the decomposition efficiency of nitrous oxide, it is not only necessary to increase the filling volume ratio, but it is important to comprehensively set the shape of the catalyst and the filling volume ratio.
Claims
1. A catalyst comprising a catalyst-filled layer of a reaction tube, wherein a catalyst is supported on a carrier comprising titanium oxide and containing at least one component selected from the group consisting of ruthenium and ruthenium compounds, wherein: The catalyst packing layer has a honeycomb structure with a packing volume ratio of 35 to 50% by volume.
2. The catalyst according to claim 1, wherein The catalyst is formed by supporting 2 mass % or more of the component containing at least one selected from the group consisting of ruthenium and ruthenium compounds on the carrier based on metallic ruthenium.
3. A catalyst, characterized in that The catalyst is formed by supporting a component containing ruthenium acid on a carrier containing titanium oxide.
4. A catalyst precursor, characterized in that The catalyst precursor is formed by supporting a component containing an alkali metal salt of ruthenate on a carrier containing titanium oxide.
5. A method for producing a catalyst, comprising supporting a carrier comprising titanium oxide with at least one component selected from the group consisting of ruthenium and ruthenium compounds, characterized in that: The method comprises the following steps (1) and (2), Step (1): a step of contacting a support containing titanium oxide with a solution containing an alkali metal salt of ruthenate and water; Step (2): a step of contacting the support containing titanium oxide and ruthenate alkali metal salt obtained in step (1) with an acidic aqueous solution.
6. A catalyst-filled reaction tube, comprising a catalyst-filled layer, wherein the catalyst-filled layer is filled with a catalyst comprising a carrier containing titanium oxide and supporting at least one component selected from the group consisting of ruthenium and ruthenium compounds, wherein the catalyst-filled reaction tube is characterized in that: The filling volume ratio of the catalyst in the catalyst filling layer is 35 to 50 volume %.
7. A method for decomposing nitrous oxide, characterized in that: A method comprising contacting the catalyst according to any one of claims 1 to 3 with a nitrous oxide-containing gas containing nitrous oxide.
8. The method for decomposing nitrous oxide according to claim 7, wherein: The nitrous oxide-containing gas includes at least one gas selected from the group consisting of nitrogen, carbon monoxide, carbon dioxide, water vapor, oxygen, hydrogen, ammonia, nitric oxide, nitrogen dioxide, and hydrocarbons.
9. The method for decomposing nitrous oxide according to claim 7, wherein: The nitrous oxide-containing gas is a gas exhausted from a chemical manufacturing facility.
10. A method for decomposing nitrous oxide, characterized in that: The method comprises the step of causing a nitrous oxide-containing gas containing nitrous oxide to flow through the catalyst-packed reaction tube according to claim 6.
11. The method for decomposing nitrous oxide according to claim 10, wherein: The nitrous oxide-containing gas includes at least one gas selected from the group consisting of nitrogen, carbon monoxide, carbon dioxide, water vapor, oxygen, hydrogen, ammonia, nitric oxide, nitrogen dioxide, and hydrocarbons.
12. The method for decomposing nitrous oxide according to claim 10, wherein: The nitrous oxide-containing gas is a gas exhausted from a chemical manufacturing facility.