Surface-treated steel sheet and method for manufacturing component
By using a coating film with a thickness of 0.5 μm to 5.0 μm on the surface-treated steel plate, containing a phenolic resin with moderate crosslinking, and heating and crosslinking after electrodeposition coating, the scar and coating of the steel plate after electrodeposition are solved. The problem of peeling achieves excellent welding properties, corrosion resistance and film adhesion.
Patent Information
- Application Number
- CN202380030423.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-12
AI Technical Summary
The existing surface-treated steel plates are prone to blisters and film peeling after electrodeposition coating, resulting in insufficient corrosion resistance and difficult to take into account both welding, corrosion resistance and film adhesion after electrodeposition coating.
The coating film having an average film thickness of 0.5 μm to 5.0 μm is used, and the coating film includes an adhesive resin, an anti-rust agent and a conductive agent, wherein the adhesive resin is a phenolic resin having a crosslinking degree of 40% to 80%, and is in the After electrodeposition coating, heating is performed to cross-link the phenolic resin to improve the adhesion between the coating film and the outermost layer.
It effectively inhibits the occurrence of bubble scars and coating film peeling, improves welding properties, corrosion resistance and coating film adhesion after electrodeposition coating, and ensures excellent corrosion resistance and spot welding properties.
Smart Images

Figure BDA0005059742480000181 
Figure BDA0005059742480000191
Abstract
Description
Technical Field
[0001] The present application discloses a method for producing a surface-treated steel plate and a component. Background Art
[0002] Surface-treated steel sheets are used as constituent materials for automobiles and the like. The surface-treated steel sheets include, for example: a plated steel sheet having a Zn-containing coating layer; and a surface-treated layer provided on at least one main surface of the plated steel sheet. In the prior art, a coating film is used as the surface-treated layer, and the type and content of the components constituting the coating film are adjusted, thereby improving the weldability and corrosion resistance of the surface-treated steel sheet.
[0003] For example, Patent Document 1 discloses a technology in which, in a surface-treated steel sheet having a coating film on at least one side of a plated steel sheet, the weldability and corrosion resistance of the surface-treated steel sheet are improved by causing the coating film to contain a binder resin, non-oxide ceramic particles containing V, and doped zinc oxide particles in specified amounts.
[0004] In addition, Patent Document 2 discloses a technology in which, in a coated steel plate comprising two or more coating layers formed on at least one surface of a Zn-plated steel plate, the outermost layer of the coating film is set to a specified thickness, the outermost layer of the coating film contains a specified non-chromium compound, and the composition of the coating film is improved in such a way that the conductivity of the immersion water when the coated steel plate is immersed in ion exchange water under specified conditions becomes 30 μS / cm or more, thereby improving the corrosion resistance of the end surface of the coated steel plate.
[0005] Patent document 3 discloses a technology for improving the weldability and corrosion resistance of a coated metal material having an organic film on the surface of the metal material by making the organic film contain a specified resin having a urethane bond and specified conductive particles.
[0006] Patent Document 4 discloses a technology for improving weldability and corrosion resistance of a coated metal plate having a coating layer on the surface of the metal plate by causing the coating layer to contain a predetermined amount of conductive particles having a predetermined particle size.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: International Publication No. 2018 / 092244
[0010] Patent Document 2: Japanese Patent Application Publication No. 2012-136025
[0011] Patent Document 3: Japanese Patent Application Publication No. 2004-042622
[0012] Patent Document 4: Japanese Patent Application Publication No. 2004-183080 Summary of the invention
[0013] Problems to be solved by the invention
[0014] Surface-treated steel sheets used as constituent materials for automobiles and the like are required to have, in addition to the weldability and corrosion resistance mentioned above, also the adhesion of the coating after electrodeposition coating. For example, as a test for evaluating the adhesion of the coating after electrodeposition coating, there is a warm salt water immersion test (SDT). According to the new understanding of the inventors of the present invention, when SDT is performed on conventional surface-treated steel sheets after electrodeposition coating, blisters and peeling of the coating may occur on the surface after SDT. If blisters and peeling of the coating occur in the surface-treated steel sheets, it becomes a cause of red rust, etc., and it is difficult to ensure sufficient corrosion resistance. In conventional surface-treated steel sheets, there has been no sufficient research on suppressing the occurrence of blisters and peeling of the coating during SDT and improving the corrosion resistance after SDT. As described above, a new technology is needed in surface-treated steel sheets that can take into account weldability, corrosion resistance, and adhesion of the coating after electrodeposition coating.
[0015] Means for solving problems
[0016] As one of means for solving the above-mentioned problems, the present application discloses the following multiple solutions.
[0017] <Scheme 1>
[0018] A surface treated steel plate comprising:
[0019] A coated steel sheet having a Zn-containing coating; and
[0020] A surface treatment layer provided on at least one main surface of the plated steel sheet,
[0021] The surface treatment layer has at least a coating film as an outer layer.
[0022] The coating film has an average film thickness of 0.5 μm to 5.0 μm.
[0023] The coating film comprises a binder resin, a rust inhibitor and a conductive agent.
[0024] The binder resin includes a phenolic resin having a cross-linking degree of 40% to 80%.
[0025] <Solution 2>
[0026] The surface-treated steel sheet according to claim 1 is a surface-treated steel sheet for electrodeposition coating.
[0027] <Scheme 3>
[0028] The surface-treated steel sheet according to claim 1 or 2, wherein the conductive agent comprises doped oxide particles,
[0029] The coating film contains 5 volume % to 30 volume % of the doped oxide particles.
[0030] <Scheme 4>
[0031] In the surface-treated steel sheet according to claim 3, the doped oxide particles are doped zinc oxide particles.
[0032] <Scheme 5>
[0033] The surface-treated steel sheet according to any one of items 1 to 4, wherein the rust inhibitor comprises at least one magnesium compound selected from magnesium hydroxide and magnesium oxide,
[0034] The coating film contains 5 volume % to 15 volume % of the magnesium compound.
[0035] <Scheme 6>
[0036] The surface-treated steel sheet according to any one of items 1 to 5, wherein the surface-treated layer has an inorganic or organic-inorganic composite film as an inner layer between the coating film and the plated steel sheet,
[0037] The film has an average film thickness of 0.1 μm to 1.0 μm.
[0038] <Scheme 7>
[0039] A manufacturing method, which is a method for manufacturing a component, comprises:
[0040] Prepare a surface-treated steel plate according to any one of schemes 1 to 6; and
[0041] By laminating the outermost layer on the surface of the coating film of the surface-treated steel sheet and then heating it, the phenolic resin is cross-linked, and the coating film and the outermost layer are bonded together.
[0042] <Scheme 8>
[0043] According to the production method of claim 7, an electrodeposition coating film is laminated on the surface of the coating film as the outermost layer.
[0044] Effects of the Invention
[0045] The surface treated steel sheet disclosed in the present invention has excellent weldability, corrosion resistance and coating film adhesion after electrodeposition coating. For example, the occurrence of blisters and coating film peeling during SDT can be suppressed, and the steel sheet has excellent corrosion resistance even after SDT. DETAILED DESCRIPTION
[0046] Hereinafter, embodiments of the present invention will be described. It should be noted that these descriptions are intended to simply illustrate embodiments of the present invention, and the present invention is not limited to the following embodiments.
[0047] 1. Surface treated steel plate
[0048] The surface treated steel sheet of the embodiment comprises: a plated steel sheet having a Zn-containing plated layer; and a surface treated layer provided on at least one main surface of the steel sheet. The surface treated layer has at least a coating film as an outer layer. The coating film has an average film thickness of 0.5 μm to 5.0 μm. The coating film contains a binder resin, a rust preventive agent, and a conductive agent. The binder resin contains a phenolic resin having a crosslinking degree of 40% to 80%.
[0049] 1.1 Coated steel sheet
[0050] The plated steel sheet, for example, comprises: a base steel sheet; and a Zn-containing coating provided on at least one main surface of the base steel sheet. The so-called "main surface" in the present application refers to a surface corresponding to the front side or the back side of the steel sheet. The Zn-containing coating may be provided only on one main surface of the base steel sheet, or on both main surfaces. In addition, the Zn-containing coating may be provided on the entire main surface of the base steel sheet, or on a portion of the main surface.
[0051] As the base steel plate, base steel plates having various chemical compositions and metal structures can be used. The base steel plate can be a normal steel plate or a steel plate containing additive elements such as chromium. The base steel plate can be adjusted in terms of the chemical composition and metal structure of the base steel plate in consideration of the target mechanical properties and formability. In addition, the thickness of the base steel plate is not particularly limited, and can be, for example, 0.2 mm or more or 6.0 mm or less.
[0052] The Zn-containing coating may have a chemical composition known to those skilled in the art. For example, the Zn-containing coating may contain additional elements such as Al in addition to Zn, and may contain Fe and the like when alloying treatment is performed. As an example, the Zn-containing coating may be a Zn-Al-Mg alloy coating containing at least Al and Mg, or a Zn-Al-Mg-Si alloy coating further containing Si. The content (concentration) of these elements may also be Al: 0-60%, Mg: 0-10%, Si: 0-2%, Mn: 0-1%, Ni: 0-1%, Sb: 0-1%, Fe: 0-20% in mass %. The Zn-containing coating may also be an alloyed hot-dip galvanized layer, a hot-dip galvanized layer or an electroplated galvanized layer. The amount of the zinc-containing coating relative to the base steel plate is not particularly limited, and may be a general amount of coating. For example, the thickness of the Zn-based alloy coating may also be 1-30 μm.
[0053] 1.2 Surface treatment layer
[0054] The surface treatment layer is provided on at least one main surface of the plated steel sheet. The surface treatment layer may be provided on only one main surface of the plated steel sheet, or on both main surfaces. In addition, the surface treatment layer may be provided on the entire main surface of the plated steel sheet, or on a portion of the main surface. The surface treatment layer may be laminated on the surface of the Zn-containing coating on the surface of the plated steel sheet.
[0055] The surface treatment layer has at least a coating film as an outer layer. The surface treatment layer may be made of only a coating film, or may have a two-layer structure of a coating film as an outer layer and a chemical conversion treatment film as an inner layer. When the surface treatment layer has the two-layer structure, more excellent corrosion resistance can be exerted. On the other hand, when the surface treatment layer does not have a chemical conversion treatment film as an inner layer, more excellent spot weldability can be exerted.
[0056] 1.2.1 Coating
[0057] In the surface-treated steel sheet of the present embodiment, the coating film contains a binder resin, a rust inhibitor, and a conductive agent.
[0058] (Binder resin)
[0059] The binder resin includes a phenolic resin having a crosslinking degree of 40% to 80%. Since the coating film includes a phenolic resin in a semi-crosslinked state, the crosslinking of the phenolic resin in a semi-crosslinked state can be performed, for example, by heating during electroplating, and the adhesion between the coating film and the electroplating coating film is improved. Alternatively, according to the surface-treated steel sheet of this embodiment, the adhesion between the outermost layer other than the electroplating coating film and the coating film can also be improved. As long as the phenolic resin is a thermosetting phenolic resin (for example, a resol type phenolic resin), it can be used. There is no particular restriction on the types of phenols, aldehydes, and catalysts that constitute the semi-crosslinked phenolic resin. In any case, in this embodiment, the crosslinking degree of the phenolic resin only needs to be 40% to 80%. It should be noted that the crosslinking degree of the phenolic resin is measured as follows. That is, the surface-treated steel sheet is cut into two pieces of a specified size by shearing, one is used as sample A, and the remaining is cooled after standing in an oven set to 200°C for 1 hour as sample B. Using two samples, FT-IR was used to determine the wavelengths of 3200 to 3400 cm in the coating film. -1 Transmittance (%) of hydroxyl group A ,I B After that, the coating films of samples A and B were removed by resin shot blasting or solvent, and the 3200 to 3400 cm -1 Transmittance (%) of hydroxyl group A0 ,I B0 . It is possible to find ((IA0 -I A ) / (I B0 -I B )×100) is taken as “degree of crosslinking of phenolic resin (%)”.
[0060] According to the knowledge of the inventors of the present invention, even in the semi-crosslinked state as described above, the phenolic resin can form a film having excellent hardness and adhesion and excellent weldability. When a resin other than the phenolic resin is used as the semi-crosslinked resin, it is difficult to obtain such an effect. For example, if a polyester resin is used as the semi-crosslinked resin, the surface-treated steel plate is subjected to pressing processing, etc., there is a tendency for the coating film to peel off. In addition, when a polyester resin is used as the semi-crosslinked resin, there is a tendency for the coating film to become an adhesive, and for example, pressing and welding may become difficult.
[0061] In addition to the above-mentioned phenolic resin, the binder resin may also include other resins. As other resins, various thermosetting resins and thermoplastic resins may be listed. For example, at least one resin selected from epoxy resin, polyester resin, polyurethane resin, acrylic resin, nylon resin and olefin resin may be listed. The epoxy resin may be an aromatic epoxy resin, an aliphatic epoxy resin, or an epoxy resin such as an amine. As specific examples of epoxy resins, for example, bisphenol A type epoxy resin, bisphenol F type epoxy resin, hydrogenated bisphenol A type epoxy resin, brominated bisphenol A type epoxy resin, bisphenol S type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, biphenyl type epoxy resin, naphthalene type epoxy resin, dicyclopentadiene type epoxy resin, triphenylmethane type epoxy resin, etc. may be listed. The epoxy resin may be combined with a curing agent. As a curing agent, various epoxy curing agents such as phenolic resin may be used. When a polyester resin is used as the binder resin, the polyester resin may be a polyester resin having a glass transition temperature Tg of -20 to 70°C, or a polyester resin having a number average molecular weight of 3000 to 30000. When a polyurethane resin is used as the binder resin, the polyurethane resin may be a polyurethane resin having a Tg of 0 to 50°C, or a polyurethane resin having a number average molecular weight of 5000 to 25000. When an acrylic resin is used as the binder resin, the acrylic resin may be an acrylic resin having a Tg of 0 to 50°C, or an acrylic resin having a number average molecular weight of 3000 to 25000. The binder resin may also contain a curing agent other than the epoxy curing agent. For example, melamine resin, isocyanate resin, etc. may be used.
[0062] The content of the binder resin in the coating film is not particularly limited, and may be, for example, 50% by volume or more, or 60% by volume or more, or 90% by volume or less, 80% by volume or less, or 70% by volume or less. In addition, the proportion of the phenolic resin in the binder resin is not particularly limited, and the proportion of the phenolic resin may be 50% by volume or more, 60% by volume or more, 70% by volume or more, 80% by volume or more, or 90% by volume or more, when the binder resin as a whole is set to 100% by volume.
[0063] (Rust Inhibitor)
[0064] The rust inhibitor may be an inorganic rust inhibitor or an organic rust inhibitor. The rust inhibitor may also include at least one magnesium compound selected from magnesium hydroxide and magnesium oxide, for example. In the present embodiment, the coating film includes a magnesium compound as a rust inhibitor, and the corrosion resistance becomes easy to further improve. In this case, the content of the magnesium compound in the coating film is not particularly limited, but when the coating film includes 5% to 15% by volume of the magnesium compound, it is easy to show better corrosion resistance. The content of the magnesium compound in the coating film may also be 6% by volume or more, 7% by volume or more, or 8% by volume or more, or may be 14% by volume or less, 13% by volume or less, or 12% by volume or less.
[0065] The rust inhibitor may contain at least one of P and V, an element that exerts a rust-inhibiting function, together with the above-mentioned magnesium compound, or may contain at least one of P and V, an element that exerts a rust-inhibiting function, instead of the above-mentioned magnesium compound. Examples of the rust inhibitor containing P include phosphoric acids such as orthophosphoric acid, metaphosphoric acid, pyrophosphoric acid, triphosphoric acid, and tetraphosphoric acid, ammonium salts such as triammonium phosphate and diammonium hydrogen phosphate, metal phosphates with Na, Mg, Al, K, Ca, Mn, Ni, Zn, and Fe, phosphonic acids such as aminotri(methylenephosphonic acid), 1-hydroxyethylidene-1,1-diphosphonic acid, ethylenediaminetetra(methylenephosphonic acid), and diethylenetriaminepenta(methylenephosphonic acid), and their salts, organic phosphoric acids such as phytic acid, and their salts, and the like. In addition, examples of the rust inhibitor containing V include vanadium pentoxide, metavanadic acid HVO, and the like. 3 , ammonium metavanadate, vanadium oxychloride VOCl 3 、Vanadium trioxide V 2 O 3 , vanadium dioxide, vanadyl sulfate VOSO 4 、vanadium oxyacetylacetonate VO(OC(=CH 2 )CH 2 COCH 3 ) 3 、Vanadium acetylacetonate V(OC(=CH 2 )CH 2 COCH 3 ) 3 、Vanadium trichloride VCl3 In addition, the rust inhibitor may also include a guanidine group-containing compound, a biguanidine group-containing compound, a thiocarbonyl group-containing compound, etc. The rust inhibitor may be water-soluble or water-insoluble. When the rust inhibitor is water-soluble, for example, when the coating film is exposed to a wet environment, the rust inhibitor dissolves in water and dissolves, and can exert a rust-proof function of inhibiting corrosion of the coating.
[0066] The form of the rust inhibitor can be, for example, in the form of particles. In the case where the rust inhibitor is in the form of particles, its average particle size is not particularly limited, as long as the appropriate size is selected in consideration of the thickness of the coating film. If the particle size of the rust inhibitor is too large relative to the thickness of the coating film, the rust inhibitor becomes easy to fall off from the coating film. The average particle size of the rust inhibitor can be more than 1 / 10 or more than 1 / 5 of the thickness of the coating film, and can be less than 2 times or equal times. The average particle size of the rust inhibitor can also be, for example, more than 0.1 μm, more than 0.3 μm, more than 0.5 μm, or more than 1.0 μm, and can also be less than 20 μm, less than 10 μm, less than 8.0 μm, less than 6.0 μm, less than 5.0 μm, less than 4.0 μm, or less than 2.5 μm. It should be noted that the so-called "average particle size" of the rust inhibitor refers to the average primary particle size when the particles present in the coating film exist as primary particles, and refers to the average secondary particle size when they exist in agglomeration. The average particle size is measured as follows. That is, the surface treated steel plate with the coating formed thereon is cut to expose the cross section and then ground. The ground cross section obtained in this manner is observed with a scanning electron microscope to obtain an observation image. Several rust inhibitor particles existing in the field of view of the observation image are randomly selected, and the equivalent circle diameter of each particle is calculated, and the average value thereof is taken as the average particle size. Whether the particles in the observation image are rust inhibitors can be easily determined by performing elemental analysis or the like.
[0067] The content of the rust inhibitor in the coating film as a whole is not particularly limited. For example, the content of the rust inhibitor in the coating film as a whole may be 5.0 volume % or more, 6 volume % or more, 7 volume % or more, or 8 volume % or less, or 15 volume % or less, 14 volume % or less, 13 volume % or less, or 12 volume % or less.
[0068] (Conductive agent)
[0069] The conductive agent has the function of improving the conductivity of the coating film and improving the weldability of the surface-treated steel sheet. 3Ω / cm or less can be used as a conductive agent. As a conductive agent, for example, metals and metal compounds can be listed. Specifically, it can be a metal such as magnesium, aluminum, silicon, calcium, scandium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, gallium, germanium, strontium, yttrium, zirconium, niobium, molybdenum, technetium, ruthenium, rhodium, palladium, silver, cadmium, indium, tin, etc.; an alloy of magnesium, aluminum, silicon, phosphorus, calcium, scandium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, gallium, germanium, arsenic, strontium, yttrium, zirconium, niobium, molybdenum, technetium, ruthenium, rhodium, palladium, silver, cadmium, indium, tin, antimony, tellurium, etc.; or a compound such as an oxide of the above-mentioned metal element. Among them, magnesium, aluminum, silicon, chromium, iron, nickel, zinc, tin, zinc-aluminum alloy, zinc-aluminum-magnesium alloy, zinc-aluminum-magnesium-silicon alloy, zinc-iron alloy, zinc-chromium alloy, zinc-nickel alloy, iron-nickel alloy, iron-chromium alloy, stainless steel, ferrosilicon, ferromanganese, ferrophosphorus, zinc oxide, etc. are easily available. The content of the conductive agent in the coating film is not particularly limited, and can be appropriately determined in consideration of the target weldability and corrosion resistance.
[0070] In particular, when the conductive agent contains doped oxide particles, it is easy to improve corrosion resistance together with conductivity. In this case, the coating film may also contain 5 volume % to 30 volume % of doped oxide particles. Alternatively, the conductive agent may be a Si alloy containing 50 mass % or more of Si, a Si compound containing 50 mass % or more of Si, or a composite thereof.
[0071] In the case where the conductive agent includes doped oxide particles, as a specific example of the doped oxide particles, doped zinc oxide particles can be cited. As doped zinc oxide particles, for example, doped zinc oxide particles whose conductivity is improved by doping zinc oxide particles with at least one doping element selected from elements of Group 13 of the Periodic Table, such as B, Al, Ga, and In, and elements of Group 15 of the Periodic Table, such as P and As. In the case where the doping element is Al or Ga, it is easy to further improve the conductivity. The content of the doping element relative to the undoped zinc oxide particles can be, for example, 0.05 atom% or more or 0.1 atom% or less, and can be 5 atom% or less.
[0072] When the conductive agent includes a Si alloy or a Si compound, a specific example of the Si alloy or Si compound is ferrosilicon containing 70% by mass or more of Si. By including ferrosilicon as a conductive agent in the coating film, it is easy to improve the corrosion resistance together with the conductivity of the coating film. In particular, ferrosilicon containing 70% by mass or more of Si is excellent in corrosion resistance and formability.
[0073] The conductive agent can be, for example, in the form of particles. In the case where the conductive agent is in the form of particles, its average particle size is not particularly limited, as long as the appropriate size is selected in consideration of the thickness of the coating film, etc. If the particle size of the conductive agent is too small relative to the thickness of the coating film, the conductivity is easily reduced. On the other hand, if the particle size of the conductive agent is too large relative to the thickness of the coating film, the conductive agent becomes easy to fall off from the coating film. In this regard, the average particle size of the conductive agent can be more than 1 / 10 or more than 1 / 5 of the thickness of the coating film, and can also be less than 2 times or less than the same times. The average particle size of the conductive agent can also be, for example, more than 0.1 μm, more than 0.3 μm, more than 0.5 μm, or more than 1.0 μm, and can also be less than 20 μm, less than 10 μm, less than 8.0 μm, less than 6.0 μm, less than 5.0 μm, less than 4.0 μm, or less than 2.5 μm. It should be noted that the so-called "average particle size" of the conductive agent refers to the average primary particle size when the particles present in the coating film exist as primary particles, and refers to the average secondary particle size when they exist in an agglomerated state. The average particle size is measured as follows. That is, the surface-treated steel plate formed with the coating film is cut to expose its cross section and then grind it. The ground cross section obtained by such operation is observed with a scanning electron microscope to obtain an observation image. Several conductive particles present in the field of view of the observation image are randomly selected, and the equivalent circle diameter of each particle is calculated, and the average value thereof is taken as the average particle size. Whether the particles in the observation image are conductive agents can be easily judged by performing elemental analysis, etc.
[0074] The content of the rust inhibitor as a whole in the coating film is not particularly limited. For example, the content of the rust inhibitor as a whole in the coating film may be 5% by volume or more, 6% by volume or more, 7% by volume or more, or 8% by volume or less, or 30% by volume or less, 25% by volume or less, 20% by volume or less, or 15% by volume or less.
[0075] (Other ingredients)
[0076] In the coating film, other components other than the above components may also be included. As other components, various additives may be listed. For example, bright pigments, lubricants, defoamers, thickeners, etc. for the purpose of improving pattern design. The content of other components in the coating film is not particularly limited.
[0077] (average film thickness)
[0078] In the present embodiment, the coating has an average film thickness of 0.5 μm to 5.0 μm. If the coating is too thin, sufficient corrosion resistance may not be obtained. In addition, the barrier property to water vapor is reduced, and the water vapor type is pressed, and it becomes easy to accumulate water at the interface between the coating and the coating, which may cause peeling. On the other hand, if the coating is too thick, the spot weldability may be reduced. The average film thickness of the coating may also be greater than 1.0 μm or greater than 2.0 μm, or less than 4.5 μm or less than 4.0 μm. The average film thickness of the coating is measured as follows. That is, the surface-treated steel plate formed with the coating is cut, and the cross section is exposed and then ground. The ground cross section obtained by such operation is observed with a scanning electron microscope to obtain an observation image. The thickness of the coating present in the field of view of the observation image of more than 10 points is measured at intervals of 1 μm along the surface direction of the plated steel plate, and the average value is taken as the average film thickness. Alternatively, the average thickness of the coating film may be determined by calculating the density of the coating film from the components contained in the coating film and measuring the weight of the coating film on this basis. In the present embodiment, the average thickness of the characteristic film may be 0.5 μm to 5.0 μm by any method.
[0079] (Attachment amount)
[0080] The coating weight is not particularly limited. For example, the coating weight may be 2.0 g / m 2 Above, 3.5g / m 2 Above or 5.0g / m 2 Above, can also be 20g / m 2 Below, 15g / m 2 Below or 10g / m 2 The following. It should be noted that the amount of coating film attached to the surface treated steel sheet can be measured by a weight method or cross-sectional observation. The amount of coating film attached by a weight method can be calculated by the following method: after measuring the initial weight of a steel sheet cut into a specified size, the weight of the steel sheet from which the coating film has been removed by a method of removing the coating film using a solvent capable of dissolving the binder resin or a dedicated agent or by a method of removing the coating film by sandblasting using resin beads is measured, and the difference between the two is obtained.
[0081] 1.2.2 Chemical conversion treatment film
[0082] In the surface treated steel sheet of the present embodiment, the surface treated layer may also have an inorganic or organic-inorganic composite film as an inner layer between the coating film and the plated steel sheet, and the coating film may also have an average film thickness of 0.1 μm to 1.0 μm. The coating film may also be called a chemical conversion treatment film. That is, the surface treated layer may also have a two-layer structure having a coating film as an outer layer and a chemical conversion treatment film as an inner layer.
[0083] (Composition ingredients)
[0084] By providing a chemical conversion treatment film as an inner layer on the surface of the plated steel sheet, and then providing the above-mentioned coating film on the surface of the chemical conversion treatment film, the adhesion of the coating film to the plated steel sheet is improved. The chemical conversion treatment film can also be a layer that does not substantially contain chromium (chromate-free layer). As the chromate-free treatment liquid used in the chemical conversion treatment, liquid silica, gas phase silica, silica-based treatment liquid with silicon compounds such as silicates as the main component, zircon-based treatment liquid with zircon-based compounds as the main component, and mixtures thereof can be listed. The chemical conversion treatment film can also contain a binder resin. For example, the chemical conversion treatment film can also contain at least one of the substances exemplified as the binder resin that can constitute the above-mentioned coating film. The content of the binder resin in the chemical conversion treatment film and the content of the components other than the binder resin are not particularly limited. For example, the content of the binder resin in the chemical conversion treatment film can also be 0% by volume to 50% by volume, and the content of the components other than the binder resin can also be 50% by volume to 100% by volume. The chemical conversion treatment film as the inner layer can be an inorganic film containing an inorganic component as a binder, or can be an organic-inorganic composite film. Various additives can also be included in the chemical conversion treatment film. For example, bright pigments, lubricants, defoamers, thickeners, etc. for the purpose of improving pattern design. The content of other components in the chemical conversion treatment film is not particularly limited.
[0085] (average film thickness)
[0086] The average film thickness of the chemical conversion treatment film is not particularly limited. From the viewpoint of further improving the adhesion between the plated steel sheet and the coating film, further improving the corrosion resistance, weldability, etc., the average film thickness of the chemical conversion treatment film is preferably 0.1μm to 1.0μm. The average film thickness of the chemical conversion treatment film can be measured in the same way as the average film thickness of the coating film. That is, the surface-treated steel plate formed with the chemical conversion treatment film is cut, and the cross section is exposed and then polished, and the polished cross section obtained by such operation is observed with a scanning electron microscope to obtain an observation image. The thickness of the chemical conversion treatment film present in the field of view of the observation image of more than 10 points is measured at intervals of 1μm along the surface direction of the plated steel sheet, and the average value is taken as the average film thickness. Alternatively, the density of the chemical conversion treatment film can be calculated from the components contained in the chemical conversion treatment film, and the weight of the chemical conversion treatment film is measured on this basis to determine the average film thickness of the chemical conversion treatment film.
[0087] (Attachment amount)
[0088] In the surface treated steel sheet, the amount of the chemical conversion coating applied is not particularly limited. For example, in the case where the amount of the chemical conversion coating applied is 200 mg / m 2 ~2000mg / m 2 In the case of, it is easy to further improve the corrosion resistance of the surface treated steel sheet. It should be noted that the adhesion amount of the chemical conversion treatment film in the surface treated steel sheet can be measured by fluorescent X-ray and cross-sectional analysis. Specifically, a standard wire plate is made for each chemical conversion treatment. The chemical conversion treatment plate and the standard wire plate are measured by fluorescent X-ray, and the adhesion amount of the produced chemical conversion treatment plate is calculated from the X-ray intensity of the contained elements and the X-ray intensity of the standard wire plate.
[0089] 1.3 Effect
[0090] As described above, in the surface-treated steel plate of the present embodiment, by making the coating film contain a phenolic resin in a semi-crosslinked state, the phenolic resin can be cross-linked by heating during the electroplating coating. That is, when a certain outermost layer (e.g., an electroplating coating film) is provided for the coating film, the adhesion between the coating film and the outermost layer can be improved. As a result, blisters and peeling of the coating film in SDT can be suppressed, and excellent corrosion resistance can be ensured even after SDT. In addition, by making the average film thickness of the coating film below a certain level, excellent weldability can also be ensured. In this way, the surface-treated steel plate of the present embodiment has excellent weldability, corrosion resistance, and adhesion of the coating film after electroplating coating, and exerts excellent effects, for example, when used for electroplating coating.
[0091] In addition, as described above, in the surface-treated steel plate of the present embodiment, by using phenolic resin as a semi-crosslinked resin, the coating becomes hard and the adhesion becomes excellent. As a result, in the surface-treated steel plate of the present embodiment, for example, a coating with excellent scratch resistance can be formed. For example, when the scratch resistance of the coating is evaluated according to JIS K5600 using a pencil with a hardness of H, the surface-treated steel plate of the present embodiment will not produce coating defects in the scratched portion, and will not peel off the coating. That is, the scratch hardness of the coating of the surface-treated steel plate of the present embodiment, for example, obtained by the pencil method specified in JIS K5600-5-4, can also be a hardness of H or above.
[0092] 2. Manufacturing method of surface treated steel plate
[0093] The surface treated steel sheet mentioned above can be manufactured, for example, by the following method. That is, the manufacturing method of the surface treated steel sheet can also include:
[0094] obtaining a coated steel sheet having a zinc-containing coating; and
[0095] The coating film is formed by applying a coating material including a binder resin, a rust preventive agent, and a conductive agent to at least one main surface of the plated steel sheet.
[0096] Alternatively, the method for manufacturing a surface-treated steel sheet may include:
[0097] Obtaining a coated steel sheet having a zinc-containing coating;
[0098] forming a chemical conversion treatment film by subjecting at least one main surface of the plated steel sheet to a chemical conversion treatment; and
[0099] The coating film is formed by applying a coating material including a binder resin, a rust preventive agent and a conductive agent to the surface of the chemical conversion treatment film.
[0100] 2.1 Preparation of coated steel sheets
[0101] The plated steel sheet having a Zn-containing plated layer can be obtained, for example, by the following steps: obtaining a slab by continuous casting; hot rolling the slab to obtain a hot-rolled sheet; coiling the hot-rolled sheet; cold rolling the hot-rolled sheet to obtain a cold-rolled sheet; annealing the cold-rolled sheet; plating the annealed steel sheet; and optionally performing skin pass rolling. The continuous casting conditions, hot rolling conditions, coiling conditions, cold rolling conditions, annealing conditions, and plating conditions may be conventionally known general conditions.
[0102] 2.2 Chemical conversion treatment
[0103] In the manufacturing method disclosed herein, a chemical conversion coating as an inner layer may be formed by subjecting at least one main surface of the plated steel sheet obtained as described above to chemical conversion treatment. The chemical conversion treatment may be performed by applying various treatment solutions as described above to the surface of the steel sheet and drying the solution.
[0104] 2.3 Film formation
[0105] In the manufacturing method disclosed in the present invention, a coating film as an outer layer can also be formed by applying a coating material including an adhesive resin, a rust inhibitor and a conductive agent on the surface of a plated steel sheet obtained by the above operation or on the surface of a chemical conversion treatment film formed by the above operation and drying the coating film. Here, by adjusting the type of rust inhibitor contained in the coating film, the content of the rust inhibitor, the thickness of the coating film, etc., the surface-treated steel sheet of the above-mentioned embodiment can be obtained. However, in the present embodiment, it is important that the phenolic resin contained in the coating film is in a semi-crosslinked state as described above. In order to obtain such a phenolic resin in a semi-crosslinked state, in the manufacturing method of the present embodiment, for example, it is preferred to adjust the heating temperature and the heating time for production.
[0106] 3. Manufacturing method of components
[0107] The technology disclosed in the present invention also has an aspect of being a method for manufacturing a component. That is, the method for manufacturing a component disclosed in the present invention includes:
[0108] preparing the surface-treated steel sheet of the present disclosure; and
[0109] By laminating the outermost layer on the surface of the coating film of the surface-treated steel sheet and then heating it, the phenolic resin is cross-linked, and the coating film and the outermost layer are bonded together.
[0110] The type of the outermost layer can be any type as long as it is bonded to the coating film by heating. Various types can be used. When the outermost layer is stacked relative to the coating film, heating is utilized to improve the adhesion of the coating film to the outermost layer by the bonding reaction between the semi-crosslinked phenolic resin and the resin terminal group of the outermost layer in addition to the crosslinking of the semi-crosslinked phenolic resin in the coating film. In particular, as described above, it is easy to obtain excellent effects when an electrodeposition coating film is stacked on the surface of the coating film as the outermost layer. The electrodeposition coating conditions (type of electrodeposition coating, voltage, etc.) in this case only need to adopt general conditions. In the manufacturing method disclosed in the present invention, for example, after the surface-treated steel plate is subjected to electrodeposition coating, the electrodeposition coating film is baked, so that the phenolic resin in the semi-crosslinked state contained in the coating film of the surface-treated steel plate can be crosslinked, and a bonding reaction with the resin in the electrodeposition coating film can be obtained. Thus, the adhesion of the coating film to the electrodeposition coating film is improved. The baking temperature is, for example, 150° C. to 190° C., and the baking time is, for example, 10 minutes to 40 minutes.
[0111] The type of the component is not particularly limited, and for example, the component may be the electrodeposition-coated component as described above, or may be another component.
[0112] Example
[0113] Hereinafter, the present invention will be further described by showing examples, but the present invention is not limited to the following examples. The present invention can adopt various conditions as long as it does not deviate from the gist of the present invention and achieves the purpose of the present invention.
[0114] 1. Manufacture of surface treated steel plates
[0115] 1.1 Preparation of alloyed hot-dip galvanized steel sheet
[0116] The following five types of zinc-plated steel sheets and cold-rolled steel sheets were prepared, immersed in an aqueous solution (2.5 mass %, 40° C.) of an aqueous alkaline degreasing agent (FC-301 manufactured by Nihon Parkerizing Co., Ltd.) for 2 minutes to degrease the surface, and then washed with water and dried to prepare substrate metal sheets for surface treatment.
[0117] GA: alloyed hot-dip galvanized steel sheet (sheet thickness 0.8 mm, 10 mass% Fe, coating weight 45 g / m 2 )
[0118] ZA1: Zn-Al-Mg ternary hot-dip galvanized steel sheet (Zn-11% Al-3% Mg-0.2% Si) (sheet thickness 0.8 mm, 10% Fe by mass, coating weight 60 g / m 2 )
[0119] ZA2: Zn-Al-Mg 3-element hot-dip galvanized steel sheet (Zn-6% Al-3% Mg) (sheet thickness 0.8 mm, 10% Fe by mass, coating weight 60 g / m 2 )
[0120] ZL: Zn-10 mass% Ni alloy electroplated steel plate (plate thickness 0.8 mm, plating weight 40 g / m 2 )
[0121] GI: Hot-dip galvanized steel sheet (sheet thickness 0.8 mm, coating weight 60 g / m 2 )
[0122] EG: Electrogalvanized steel sheet (sheet thickness 0.8 mm, coating weight 40 g / m 2 )
[0123] CR: Cold rolled steel plate (thickness 0.8mm, no plating)
[0124] 1.2 Formation of the inner layer (chemical conversion treatment film)
[0125] Next, the following treatment liquid S for chemical conversion treatment was prepared, and the treatment liquid was applied to the above-mentioned base metal plate while changing the number of the bar coating, and then dried and air-dried in a hot air furnace so that the surface temperature of the metal plate reached 70° C., thereby forming a chemical conversion treatment film on the surface of the metal plate. The average film thickness of the chemical conversion treatment film was 0.2 μm.
[0126] S: Treatment liquid for chemical conversion treatment containing Zr compound, silane coupling agent, silica particles, and Nv10% of polyester resin
[0127] 1.3 Formation of outer layer (coating film)
[0128] Next, in order to form a coating film having the composition ratio (volume %) shown in Table 1, each component is mixed in a manner to form the same solid content concentration as Table 1, and a coating composition for coating film formation is prepared. While changing the number and dilution rate of the rod coating, the coating composition is applied to a substrate metal plate or a chemical conversion treatment film with a rod coater, and an oven is used to dry the coating film under the condition that the maximum reaching temperature (PMT) becomes 140°C, 160°C, 180°C, and 200°C, thereby forming a coating film as an outer layer. Here, the crosslinking degree of the phenolic resin in the coating film is adjusted by the maximum reaching temperature during drying. The average film thickness of the coating film is the film thickness (μm) shown in Table 2. It should be noted that the components contained in the coating composition are shown below.
[0129] (Anti-rust pigment)
[0130] MgO: magnesium oxide (average particle size 3 μm)
[0131] Mg(OH) 2 : Magnesium hydroxide (average particle size: 3 μm)
[0132] PA: Aluminum tripolyphosphate (oil absorption 10ml / 100g, particle size 2μm)
[0133] (Conductive Pigments)
[0134] ZnO: doped zinc oxide particles (23-Kt manufactured by Hakusui Tech Co., Ltd., average particle size 0.5 μm)
[0135] FeSi: ferrosilicon particles (average particle size 3 μm, containing 70 mass % or more of Si)
[0136] SUS: SUS particles (average particle size 5 μm)
[0137] (Binder resin)
[0138] B1: Phenolic resin (DIC water-soluble resol type phenolic resin GG-1490)
[0139] B2: Phenolic resin (DIC resol phenolic resin 5010)
[0140] B3: Polyurethane resin (SUPERFLEX 150 manufactured by Daiichi Kogyo Seiyaku Co., Ltd.)
[0141] B4: Polyester resin (VYLONAL MD1480 manufactured by BYRON)
[0142] B5: Melamine resin (CYMEL 325 manufactured by Allnex)
[0143] 2. Performance evaluation test
[0144] The following performance evaluation tests were performed on each surface-treated steel sheet.
[0145] 2.1 Determination of crosslinking degree
[0146] When a phenolic resin was used as a binder in the coating film, the degree of crosslinking of the phenolic resin contained in the coating film was measured as follows.
[0147] (Method for determining the degree of crosslinking of phenolic resin)
[0148] The surface treated steel plate prepared as described above was cut into two pieces of a predetermined size by shearing, one of which was used as sample A, and the remaining was placed in an oven set at 200°C for 1 hour and then cooled to form sample B. The two samples were used to determine the 3200 to 3400 cm-1 mass in the coating film by FT-IR. -1 Transmittance (%) of hydroxyl group A ,I B After that, the coating films of samples A and B were removed by resin shot blasting or solvent, and the 3200 to 3400 cm -1 Transmittance (%) of hydroxyl group A0 ,I B0 Determination A0 -I A ) / (I B0 -I B )×100) is taken as “degree of crosslinking of phenolic resin (%)”.
[0149] 2.2 Salt water immersion test (SDT)
[0150] (Preparation)
[0151] For each surface-treated steel plate, surface conditioning was performed for 20 seconds at room temperature using the surface conditioning agent PREPALENE X (trade name) manufactured by Nihon Parkerizing Co., Ltd. Furthermore, chemical conversion treatment (phosphate treatment) was performed using the chemical conversion treatment liquid (zinc phosphate treatment liquid) "Parbond 3020 (trade name)" manufactured by Nihon Parkerizing Co., Ltd. The temperature of the chemical conversion treatment liquid was set to 43°C, and the hot-pressed formed material was immersed in the chemical conversion treatment liquid for 120 seconds, and then washed and dried. After the above-mentioned chemical conversion treatment (phosphate treatment) was performed, the cationic electrodeposition paint manufactured by NIPPONPAINT Co., Ltd. was electroplated by energizing at a ramp voltage of 160V, and then baked at a baking temperature of 170°C for 20 minutes. The average film thickness of the electrodeposition coating film after electrodeposition coating was 10μm in any sample.
[0152] (Corrosion resistance at SDT (area ratio of blister scars))
[0153] After the above-mentioned electrodeposition coating, the end face of the surface-treated steel plate was sealed with a tape and immersed in a 3% NaCl aqueous solution at a temperature of 50°C for 500 hours. The sample taken out after the immersion test was dried, and the area ratio of the blisters present on the surface of the electrodeposition coating was determined by visual inspection. In the corrosion resistance test, in the case of "3", it was judged to have a certain degree of corrosion resistance, and in the case of "4" or "5", it was judged to have excellent corrosion resistance. The results are shown in Table 2.
[0154] 1: The area ratio of blisters generated on the evaluation surface is 50% or more
[0155] 2: The area ratio of blisters generated on the evaluation surface is 5% or more and less than 50%
[0156] 3: The area ratio of blisters generated on the evaluation surface is 1% or more and less than 5%
[0157] 4: Although blisters are generated on the evaluation surface, they are less than 1%
[0158] 5: No blisters or scars
[0159] 2.3 Corrosion resistance test after SDT
[0160] The electrodeposition-coated surface-treated steel sheet subjected to the warm salt water immersion test was subjected to a cyclic corrosion test under the following cyclic conditions for 120 cycles.
[0161] (Loop condition)
[0162] The treatment was carried out by setting one cycle of salt water spraying (SST, 5% NaCl, 35°C atmosphere) for 2 hours, drying (60°C) for 2 hours, and wetting (50°C, 98% RH) for 4 hours.
[0163] Thereafter, the corrosion state generated in the flat surface portion was observed and the following scores were assigned. In the above-mentioned corrosion resistance test, when the score was "3", "4" or "5", it was judged that the corrosion resistance was excellent. The results are shown in Table 2.
[0164] 1: The area ratio of white rust on the evaluation surface is 50% or more, or red rust is confirmed on the evaluation surface 2: The area ratio of white rust on the evaluation surface is 10% or more and less than 50%
[0165] 3: The area ratio of white rust on the evaluation surface is 5% or more and less than 10%
[0166] 4: The area ratio of white rust on the evaluation surface is 1% or more and less than 5%
[0167] 5: The area ratio of white rust generated on the evaluation surface is less than 1%
[0168] 2.4 Spot weldability
[0169] For each surface treated steel plate, a CF type Cr-Cu electrode with a tip diameter of 5 mm and R40 was used to perform a continuous spot welding test with a pressure of 1.96 kN, a welding current of 8 kA, and a power-on time of 12 cycles / 50 Hz to find the number of spots before the nugget diameter is about to be less than 3√t (t is the plate thickness). The following evaluation points are used to evaluate the quality of spot weldability. In the weldability test, when it is "4", "5" or "6", it is judged that the weldability is excellent. The results are shown in Table 2.
[0170] 1: No nugget is generated and welding cannot be performed at any point, or the number of points is less than 10 points.
[0171] 2: The number of RBI is more than 10 RBI and less than 50 RBI
[0172] 3: The number of RBI is more than 50 RBI and less than 200 RBI
[0173] 4: The number of points is more than 200 and less than 1000
[0174] 5: The number of points is more than 1000 and less than 2000
[0175] 6: The number of points is more than 2000
[0176] 2.5 Scratch resistance
[0177] A scratch test was performed on the coating of each surface treated steel plate using a pencil with a hardness of H manufactured by Mitsubishi Uni in accordance with JIS K5600. The coating condition after scratching was observed, and the scratch resistance was evaluated using the following evaluation points. In the scratch resistance test, when the score was "2" or "3", it was judged that the scratch resistance was excellent. The results are shown in Table 2.
[0178] 1: The coating peels off in part or all of the scratched area
[0179] 2: Although there is a coating defect at the scratched part, there is no coating peeling
[0180] 3: There is no coating defect on the scratched part
[0181] (Table 1)
[0182]
[0183] (Table 2)
[0184]
[0185] 3. Results and Investigation
[0186] From the results shown in Tables 1 and 2, the following matters were found.
[0187] Regarding No. 13, the coating film does not contain an anti-rust pigment, and the corrosion resistance after SDT is inferior.
[0188] Regarding No. 14, the coating film did not contain a conductive pigment and the spot weldability was inferior.
[0189] Regarding No. 19, the binder constituting the coating film was not a phenolic resin, and not only did blisters form during SDT, but the corrosion resistance after SDT was also inferior.
[0190] Regarding No. 23, since the film thickness of the coating film was too thin at 0.2 μm, the corrosion resistance after SDT was inferior.
[0191] Regarding No. 28, since the coating film thickness was too thick at 10 μm, the spot weldability was inferior.
[0192] Regarding No. 34, since a steel sheet without a Zn-containing plating layer was used, the corrosion resistance after SDT was inferior.
[0193] Regarding No. 41 to 44, although phenolic resin was used as a binder constituting the coating film, the crosslinking degree of the phenolic resin was too high, so the crosslinking of the phenolic resin could not be carried out during the electrodeposition coating, and the adhesion between the coating film and the electrodeposition coating film was poor. Therefore, not only did blisters occur during SDT, but the corrosion resistance after SDT was also poor.
[0194] In No. 45, since the cross-linking degree of the phenolic resin in the coating film was as low as 20%, the hardness and adhesion of the coating film were not sufficient.
[0195] Regarding No. 46, since an uncrosslinked polyester resin was used, the hardness and adhesion of the coating were not sufficient. In addition, the electrode adhered to the coating during welding, and proper welding could not be performed. In addition, the coating peeled off during the scratch test.
[0196] Regarding No. 47, since polyester resin and melamine resin as a cross-linking agent were used as semi-cross-linked resins in the coating film, the adhesion of the coating film was insufficient. In addition, the electrode adhered to the coating film during welding, and proper welding could not be performed. In addition, the coating film peeled off during the scratch test.
[0197] In contrast, regarding Nos. 1 to 12, 15 to 18, 20 to 22, 24 to 27, 29 to 33, and 35 to 40, almost no blisters were generated during SDT, and the corrosion resistance after SDT was excellent, and the spot weldability and scratch resistance were also excellent. Regarding Nos. 1 to 12, 15 to 18, 20 to 22, 24 to 27, 29 to 33, and 35 to 40, the surface-treated steel sheets are as follows: (1) a plated steel sheet having a Zn-containing plating layer; (2) a coating film as a surface-treated layer having an average film thickness of 0.5 μm to 5.0 μm; (3) the coating film contains a binder resin, a rust-proof pigment, and a conductive pigment; (4) the binder resin contains a phenolic resin having a crosslinking degree of 40% to 80%. That is, it is believed that the inclusion of a rust-proof pigment and a conductive pigment in the coating film improves the corrosion resistance and spot weldability. In addition, it is believed that by using a phenolic resin in a semi-crosslinked state as a binder resin, the phenolic resin can be crosslinked by heating during electrodeposition coating, thereby improving the adhesion between the coating film and the electrodeposition coating film. In addition, it is believed that by using a phenolic resin as a semi-crosslinked resin in the coating film, the coating film becomes hard and has excellent adhesion, and the scratch resistance is improved.
[0198] From the above results, it can be said that the surface-treated steel sheet satisfying the following requirements has excellent weldability and corrosion resistance.
[0199] A surface treated steel plate comprising:
[0200] A coated steel sheet having a Zn-containing coating; and
[0201] A surface treatment layer provided on at least one main surface of the plated steel sheet,
[0202] The surface treatment layer has at least a coating film as an outer layer.
[0203] The coating film has an average film thickness of 0.5 μm to 5.0 μm.
[0204] The coating film comprises a binder resin, a rust inhibitor and a conductive agent.
[0205] The binder resin includes a phenolic resin having a cross-linking degree of 40% to 80%.
Claims
1. A surface treated steel plate comprising: A coated steel sheet having a Zn-containing coating; and a surface treatment layer provided on at least one main surface of the plated steel sheet, The surface treatment layer has at least a coating film as an outer layer, The coating film has an average film thickness of 0.5 μm to 5.0 μm, The coating film comprises a binder resin, a rust inhibitor and a conductive agent, The binder resin includes a phenolic resin having a cross-linking degree of 40% to 80%. 2 . The surface-treated steel sheet according to claim 1 , which is a surface-treated steel sheet for electrodeposition coating.
3. The surface-treated steel sheet according to claim 1 or 2, in, The conductive agent comprises doped oxide particles, The coating film contains 5 volume % to 30 volume % of the doped oxide particles.
4. The surface-treated steel sheet according to claim 3, in, The doped oxide particles are doped zinc oxide particles.
5. The surface-treated steel sheet according to any one of claims 1 to 4, in, The rust inhibitor comprises at least one magnesium compound selected from magnesium hydroxide and magnesium oxide. The coating film contains 5 volume % to 15 volume % of the magnesium compound.
6. The surface-treated steel sheet according to any one of claims 1 to 5, in, The surface treatment layer has an inorganic or organic-inorganic composite film as an inner layer between the coating film and the plated steel sheet. The film has an average film thickness of 0.1 μm to 1.0 μm.
7. A manufacturing method, which is a method for manufacturing a component, comprising: preparing a surface-treated steel sheet according to any one of claims 1 to 6; and By laminating the outermost layer on the surface of the coating film of the surface-treated steel sheet and then heating it, the phenolic resin is cross-linked, and the coating film and the outermost layer are bonded together. 8 . The production method according to claim 7 , wherein an electrodeposition coating film is laminated on the surface of the coating film as the outermost layer.
Citation Information
Patent Citations
Zinc-plated steel plate with excellent blackening resistance and corrosion resistance and manufacturing method therefor
CN105793468A
Surface-treated steel sheet and coated member
CN110073034A
Method of processing metal material
JP1977036558A