Copolymer, molded body, and injection molded body
By adjusting the content and structure of TFE and PPVE units, a new copolymer was developed, which solved the problem of difficult to obtain durability and wear resistance molded bodies in high temperature and high frequency environments in the prior art, and achieved medium and high injection molding method Production of performance molded bodies.
Patent Information
- Application Number
- CN202380028898.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-08-26
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is difficult to obtain through injection molding method that has abrasion resistance of 60°C, low hydrogen permeability, rigidity at high temperature of 100°C, tensile creep resistance at 230°C, durability to repeated loads and solvent crack resistance. Copolymer molded body.
By adjusting the content, melt flow rate and functional group number of tetrafluoroethylene (TFE) and perfluoro(propyl vinyl ether) (PPVE) units, a copolymer containing TFE and PPVE was developed to ensure that it was at 372°C The melt flow rate below is 11.0 to 16.0 g/10 minutes, and the number of functional groups is 50 or less.
A beautiful molded body of various shapes is achieved through injection molding, with wear resistance of 60°C, low hydrogen permeability, rigidity at high temperature of 100°C, tensile creep resistance at 230°C, and durability to repeated loads It is also a molded body with excellent solvent crack resistance, suitable for high temperature and high frequency environments.
Smart Images

Figure BDA0005051267280000051 
Figure BDA0005051267280000161 
Figure BDA0005051267280000181
Abstract
Description
Technical Field
[0001] The present invention relates to a copolymer, a molded article and an injection-molded article. Background Art
[0002] Patent Document 1 describes a thermoplastic resin composition comprising a mixture of (A) a number average molecular weight of 5×10 2 ~5×10 5 The invention relates to a blend of 0.1 to 99 wt % of a fluoropolymer containing hydroxymethyl group and 1 to 99.9 wt % of a liquid crystal polyester (B), wherein the fluoropolymer containing hydroxymethyl group (A) has a carbon number of 1×10 6 2×10 2 ~1×10 5 At least one of the group consisting of perfluoropolymers having methylol groups.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: International Publication No. 1995 / 029956 Summary of the invention
[0006] Problems to be solved by the invention
[0007] The object of the present invention is to provide a copolymer which can be easily molded into beautiful injection molded products of various shapes by injection molding, and can obtain molded products having excellent wear resistance at 60°C, low hydrogen permeability, rigidity at a high temperature of 100°C, tensile creep resistance at 230°C, durability against repeated loads, solvent crack resistance, and durability against tensile force applied at 230°C.
[0008] Means for solving problems
[0009] According to the present invention, there is provided a copolymer comprising tetrafluoroethylene units and perfluoro(propyl vinyl ether) units, wherein the content of the perfluoro(propyl vinyl ether) units is 4.4 to 5.2% by mass relative to all monomer units, the melt flow rate at 372° C. is 11.0 to 16.0 g / 10 minutes, and the number of functional groups is 10 6 The number of carbon atoms in the main chain is 50 or less.
[0010] Effects of the Invention
[0011] According to the present invention, a copolymer can be provided, which can be easily molded into beautiful injection-molded products of various shapes by injection molding, and can obtain molded products that are excellent in 60°C wear resistance, low hydrogen permeability, rigidity at a high temperature of 100°C, tensile creep resistance at 230°C, durability against repeated loads, solvent crack resistance, and durability against tensile forces applied at 230°C. DETAILED DESCRIPTION
[0012] The specific embodiments of the present invention are described in detail below, but the present invention is not limited to the following embodiments.
[0013] The copolymer of the present invention comprises tetrafluoroethylene (TFE) units and perfluoro(propyl vinyl ether) (PPVE) units.
[0014] Patent document 1 records that perfluorinated fluororesins (such as PTFE, FEP, PFA, etc.) have a wide usable temperature range and are excellent in chemical resistance, alkali resistance, acid resistance, water resistance, weather resistance, corrosion resistance, wear resistance, electrical insulation, etc., and are therefore used in various applications such as lining materials for pipes, valves, pumps, etc., flexible pipes, membranes, chip baskets, pump impellers, mechanical parts, chemical experimental equipment, etc.
[0015] In addition, Patent Document 1 states that perfluororesins often have poor mechanical properties, physical heat resistance represented by load deflection temperature, dimensional stability represented by linear expansion coefficient, moldability, etc. As a solution to this problem, a thermoplastic resin composition comprising a perfluoropolymer having a hydroxymethyl group at the end and a liquid crystal polyester is proposed.
[0016] However, in order to further expand the application range of perfluoro-based fluororesins, it is preferred not to mix other polymers such as liquid crystal polyesters to improve the properties of the perfluoro-based fluororesins themselves.
[0017] It was found that by appropriately adjusting the PPVE unit content, melt flow rate (MFR) and number of functional groups of a copolymer containing TFE units and PPVE units, the moldability of the copolymer can be significantly improved. By using such a copolymer, it is possible to obtain a molded product having excellent abrasion resistance at 60°C, low hydrogen permeability, rigidity at a high temperature of 100°C, tensile creep resistance at 230°C, durability against repeated loads, solvent crack resistance, and durability against tensile force applied at 230°C without mixing other polymers such as liquid crystal polyester into the copolymer.
[0018] For example, by using the copolymer of the present invention, piping members, pipes, valves, etc. that are unlikely to wear and deform even when in contact with a high-temperature fluid whose pressure changes frequently and that are unlikely to be permeated by hydrogen can be produced.
[0019] The copolymer of the present invention is a melt-processable fluororesin. Melt-processability means that the polymer can be melted and processed using existing processing equipment such as an extruder and an injection molding machine.
[0020] The content of the PPVE unit in the copolymer is 4.4 to 5.2% by mass relative to the total monomer units. The content of the PPVE unit in the copolymer is preferably 5.1% by mass or less, more preferably 5.0% by mass or less, further preferably 4.9% by mass or less, and further preferably 4.8% by mass or less. If the content of the PPVE unit in the copolymer is too much, the low hydrogen permeability, rigidity at a high temperature of 100°C, tensile creep resistance at 230°C, and durability to repeated loads will be poor. If the content of the PPVE unit in the copolymer is too little, the wear resistance at 60°C, the resistance to solvent cracking, and the durability to the tensile force applied at 230°C will be poor.
[0021] The content of TFE units in the copolymer is preferably 95.6% by mass or less, preferably 94.8% by mass or more, more preferably 94.9% by mass or more, further preferably 95.0% by mass or more, further preferably 95.1% by mass or more, and particularly preferably 95.2% by mass or more relative to all monomer units. If the content of TFE units in the copolymer is too small, low hydrogen permeability, rigidity at high temperature of 100°C, tensile creep resistance at 230°C, and durability to repeated loads may be poor. If the content of TFE units in the copolymer is too large, wear resistance at 60°C, solvent crack resistance, and durability to tensile force applied at 230°C may be poor.
[0022] In the present invention, the content of each monomer unit in the copolymer is determined by 19 Determined by F-NMR method.
[0023] The copolymer may also contain monomer units derived from monomers copolymerizable with TFE and PPVE. In this case, the content of the monomer units copolymerizable with TFE and PPVE is preferably 0 to 0.8% by mass, more preferably 0.05 to 0.4% by mass, and further preferably 0.1 to 0.3% by mass relative to all monomer units of the copolymer. The content of the monomer units copolymerizable with TFE and PPVE may be 0.1% by mass or less relative to all monomer units of the copolymer.
[0024] Examples of monomers copolymerizable with TFE and PPVE include hexafluoropropylene (HFP), CZ 1 Z 2 =CZ 3 (CF2) n Z 4 (Where Z 1 , Z 2 and Z 3 Same or different, means H or F, Z4 represents H, F or Cl, and n represents an integer of 2 to 10. ) represents a vinyl monomer, CF2=CF-ORf 1 (Where Rf 1 Perfluoro(alkyl vinyl ether) [PAVE] (excluding PPVE) represented by a perfluoroalkyl group having 1 to 8 carbon atoms, and CF2=CF-OCH2-Rf 1 (Where Rf 1 represents a perfluoroalkyl group having 1 to 5 carbon atoms. ) and the like. Among them, HFP is preferred.
[0025] The copolymer is preferably at least one selected from the group consisting of a copolymer consisting only of a TFE unit and a PPVE unit and a TFE / HFP / PPVE copolymer, and more preferably a copolymer consisting only of a TFE unit and a PPVE unit.
[0026] The melt flow rate (MFR) of the copolymer is 11.0 to 16.0 g / 10 minutes. The MFR of the copolymer is preferably 11.1 g / 10 minutes or more, more preferably 11.5 g / 10 minutes or more, further preferably 12.0 g / 10 minutes or more, particularly preferably 12.5 g / 10 minutes or more, and most preferably 13.0 g / 10 minutes or more, preferably 15.8 g / 10 minutes or less, more preferably 15.6 g / 10 minutes or less, further preferably 15.4 g / 10 minutes or less, particularly preferably 15.2 g / 10 minutes or less, and most preferably 15.0 g / 10 minutes or less. If the MFR of the copolymer is too high, the wear resistance at 60°C, the solvent crack resistance, and the durability to the tensile force applied at 230°C will be poor. If the MFR of the copolymer is too low, it is not easy to obtain beautiful injection molded products of various shapes by injection molding. On the other hand, when the MFR of the copolymer is too low, hydrogen permeability, rigidity at a high temperature of 100° C., and durability against repeated loads are poor.
[0027] In the present invention, MFR is a value obtained as the mass (g / 10 minutes) of a polymer flowing out from a nozzle having an inner diameter of 2.1 mm and a length of 8 mm at 372° C. and a load of 5 kg per 10 minutes using a melt flow indexer in accordance with ASTM D1238.
[0028] The MFR can be adjusted by adjusting the type and amount of the polymerization initiator, the type and amount of the chain transfer agent, etc., used when polymerizing the monomers.
[0029] Each 10 6 The number of functional groups per main chain carbon atom is 50 or less. 6The number of functional groups per main chain carbon atom is preferably 40 or less, more preferably 30 or less, further preferably 20 or less, further preferably 15 or less, particularly preferably 10 or less, and most preferably less than 6. If the number of functional groups is too large, hydrogen permeability and 230°C tensile creep resistance are poor.
[0030] The identification of the types of the functional groups and the measurement of the number of the functional groups can be performed using infrared spectroscopy.
[0031] The number of functional groups is specifically determined by the following method. First, the copolymer is formed by cold pressing to produce a film with a thickness of 0.25 mm to 0.30 mm. The film is analyzed by Fourier transform infrared spectroscopy to obtain an infrared absorption spectrum of the copolymer and a differential spectrum from a background spectrum of complete fluorination without the presence of functional groups. The number of functional groups per 1×10 6 The number of functional groups N per carbon atom.
[0032] N=I×K / t(A)
[0033] I: Absorbance
[0034] K: Correction coefficient
[0035] t: film thickness (mm)
[0036] For reference, absorption frequencies, molar absorption coefficients, and correction coefficients for some functional groups are shown in Table 1. The molar absorption coefficients were determined from FT-IR measurement data of low-molecular model compounds.
[0037] [Table 1]
[0038] Table 1
[0039]
[0040] The absorption frequencies of -CH2CF2H, -CH2COF, -CH2COOH, -CH2COOCH3, and -CH2CONH2 are several tens of kaise (cm2) lower than the absorption frequencies of -CF2H, -COF, free -COOH, and bound -COOH, -COOCH3, and -CONH2 shown in the table, respectively. -1 ).
[0041] For example, the functional group number of -COF is the absorption frequency 1883 cm due to -CF2COF. -1 The number of functional groups obtained from the absorption peak at 1840 cm-1 due to -CH2COF -1The total number of functional groups found from the absorption peak at .
[0042] The functional groups are functional groups present at the main chain end or side chain end of the copolymer and functional groups present in the main chain or side chain. The number of functional groups can be the total number of -CF=CF2, -CF2H, -COF, -COOH, -COOCH3, -CONH2 and -CH2OH.
[0043] The functional groups are introduced into the copolymers, for example, by chain transfer agents or polymerization initiators used when manufacturing the copolymers. For example, when alcohol is used as a chain transfer agent or a peroxide having a -CH2OH structure is used as a polymerization initiator, -CH2OH is introduced into the main chain end of the copolymer. In addition, by polymerizing monomers having functional groups, the functional groups are introduced into the side chain ends of the copolymers.
[0044] By fluorinating the copolymer having such functional groups, a copolymer having the number of functional groups within the above range can be obtained. That is, the copolymer of the present invention is preferably fluorinated. The copolymer of the present invention also preferably has a -CF3 terminal group.
[0045] The melting point of the copolymer is preferably 295 to 315° C., more preferably 298° C. or higher, further preferably 300° C. or higher, particularly preferably 301° C. or higher, most preferably 302° C. or higher, and more preferably 308° C. or lower. When the melting point is within the above range, a copolymer can be obtained that can provide a molded product that is more excellent in 60° C. wear resistance, low hydrogen permeability, rigidity at a high temperature of 100° C., 230° C. tensile creep resistance, durability against repeated loads, solvent crack resistance, and durability against tensile force applied at 230° C.
[0046] In the present invention, the melting point can be measured using a differential scanning calorimeter [DSC].
[0047] The hydrogen permeability coefficient of the copolymer is preferably 2140 cm 3 mm / (m 2 ·24h·atm) or less, more preferably 2000cm 3 mm / (m 2 The copolymer of the present invention has excellent low hydrogen permeability because the content of PPVE units, melt flow rate (MFR) and number of functional groups of the copolymer containing TFE units and PPVE units are appropriately adjusted.
[0048] In the present invention, the hydrogen permeability coefficient can be measured under the conditions of a test temperature of 60° C. and a test humidity of 0% RH. The specific measurement of the hydrogen permeability coefficient can be carried out by the method described in the Examples.
[0049] The copolymer of the present invention can be produced by polymerization methods such as suspension polymerization, solution polymerization, emulsion polymerization, bulk polymerization, etc. As the polymerization method, emulsion polymerization or suspension polymerization is preferred. In these polymerizations, various conditions such as temperature and pressure, polymerization initiator, and other additives can be appropriately set according to the composition and amount of the copolymer.
[0050] As the polymerization initiator, an oil-soluble radical polymerization initiator or a water-soluble radical polymerization initiator can be used.
[0051] The oil-soluble radical polymerization initiator may be a known oil-soluble peroxide, and the following may be cited as representative examples:
[0052] Dialkyl peroxydicarbonates such as di-n-propyl peroxydicarbonate, di-isopropyl peroxydicarbonate, di-sec-butyl peroxydicarbonate and di-2-ethoxyethyl peroxydicarbonate;
[0053] Peroxyesters such as tert-butyl peroxyisobutyrate and tert-butyl peroxypivalate;
[0054] Dialkyl peroxides such as di-tert-butyl peroxide;
[0055] Di[fluoro(or chlorofluoro)acyl]peroxides; etc.
[0056] Examples of the di[fluoro(or fluorochloro)acyl]peroxides include diacyl peroxides represented by [(RfCOO)-]2 (Rf is a perfluoroalkyl group, an ω-hydroperfluoroalkyl group or a fluorochloroalkyl group).
[0057] Examples of the di[fluoro(or chlorofluoro)acyl]peroxides include di(ω-hydro-dodecafluoroheptanoyl)peroxide, di(ω-hydro-tetrafluorooctanoyl)peroxide, di(ω-hydro-hexafluorononanoyl)peroxide, di(perfluoropropionyl)peroxide, di(perfluorobutyryl)peroxide, di(perfluoropentanoyl)peroxide, di(perfluorohexanoyl)peroxide, di(perfluoroheptanoyl)peroxide, di(perfluorooctanoyl)peroxide, di(perfluorononanoyl)peroxide, di(ω-chloro-hexafluorobutyryl)peroxide, di(perfluorohexanoyl ... (ω-chloro-decafluorohexanoyl) peroxide, bis(ω-chloro-tetrafluorooctanoyl) peroxide, ω-hydro-dodecafluoroheptanoyl-ω-hydrohexafluorononanoyl-peroxide, ω-chloro-hexafluorobutyryl-ω-chloro-decafluorohexanoyl-peroxide, ω-hydro-dodecafluoroheptanoyl-peroxide, ω-hydro-dodecafluoroheptanoyl-perfluorobutyryl-peroxide, bis(dichloropentafluorobutyryl) peroxide, bis(trichlorooctafluorohexanoyl) peroxide, bis(tetrachloroundecanoyl) peroxide, bis(pentachlorotetrafluorodecanoyl) peroxide, bis(undecachlorotriacontafluorodocosanoyl) peroxide, and the like.
[0058] The water-soluble free radical polymerization initiator may be a known water-soluble peroxide, for example, ammonium salts, potassium salts, sodium salts of persulfuric acid, perboric acid, perchloric acid, perphosphoric acid, percarbonic acid, etc., organic peroxides such as disuccinic acid peroxide and diglutaric acid peroxide, tert-butyl permaleate, tert-butyl hydroperoxide, etc. A reducing agent such as sulfite may be used in combination with the peroxide, and the amount used may be 0.1 to 20 times that of the peroxide.
[0059] A surfactant, a chain transfer agent, and a solvent may be used in the polymerization, and conventionally known surfactants may be used.
[0060] As the surfactant, known surfactants can be used, such as nonionic surfactants, anionic surfactants, cationic surfactants, etc. Among them, fluorinated anionic surfactants are preferred, and more preferred are fluorinated anionic surfactants that may contain ether-bonded oxygen (i.e., oxygen atoms may be inserted between carbon atoms) and have a linear or branched carbon number of 4 to 20. The amount of surfactant added (relative to polymerization water) is preferably 50 to 5000 ppm.
[0061] Examples of chain transfer agents include hydrocarbons such as ethane, isopentane, n-hexane, and cyclohexane; aromatics such as toluene and xylene; ketones such as acetone; acetates such as ethyl acetate and butyl acetate; alcohols such as methanol and ethanol; mercaptans such as methyl mercaptan; halogenated hydrocarbons such as carbon tetrachloride, chloroform, dichloromethane, and chloromethane, etc. The amount of chain transfer agent added can vary depending on the chain transfer constant of the compound used, and is usually used in the range of 0.01 to 20% by mass relative to the polymerization solvent.
[0062] Examples of the solvent include water and a mixed solvent of water and alcohol.
[0063] In suspension polymerization, in addition to water, fluorine-based solvents can also be used. Examples of fluorine-based solvents include hydrochlorofluoroalkanes such as CH3CClF2, CH3CCl2F, CF3CF2CCl2H, CF2ClCF2CFHCl, etc.; chlorofluoroalkanes such as CF2ClCFClCF2CF3, CF3CFClCFClCF3, etc.; hydrofluoroalkanes such as CF3CFHCFHCF2CF2CF3, CF2HCF2CF2CF2CF2H, CF3CF2CF2CF2CF2CF2CF2H, etc.; CH3OC2F5, CH 3OC3F5CF3CF2CH2OCHF2, CF3CHFCF2OCH3, CHF2CF2OCH2F, (CF3)2CHCF2OCH3, CF3CF2CH2OCH2CHF2, CF3CHFCF2OCH2CF3 and other hydrofluoroethers; perfluorocyclobutane, CF3CF2CF2CF3, CF3CF2CF2CF2CF3, CF3CF2CF2CF2CF2CF3 and other perfluoroalkanes, among which perfluoroalkanes are preferred. From the viewpoint of suspension and economy, the amount of fluorine-based solvent used is preferably 10 to 100% by mass relative to the aqueous medium.
[0064] The polymerization temperature is not particularly limited and may be 0 to 100° C. The polymerization pressure is appropriately determined depending on the type and amount of the solvent used and other polymerization conditions such as vapor pressure and polymerization temperature, and may generally be 0 to 9.8 MPaG.
[0065] In the case of obtaining an aqueous dispersion comprising a copolymer by polyreaction, the copolymer can be recovered by precipitating, cleaning, and drying the copolymer contained in the aqueous dispersion. In addition, in the case of obtaining a copolymer in the form of a slurry by polyreaction, the copolymer can be recovered by taking out the slurry from a reaction vessel and cleaning and drying. By drying, the copolymer can be recovered in the form of a powder.
[0066] The copolymer obtained by polymerization can be formed into pellets. There is no particular limitation on the molding method for forming the pellets, and a conventionally known method can be used. For example, there can be cited a method in which the copolymer is melt-extruded using a single-screw extruder, a twin-screw extruder, or a tandem extruder, and the copolymer is cut into a predetermined length to form pellets. The extrusion temperature during melt extrusion needs to be changed according to the melt viscosity and the manufacturing method of the copolymer, and is preferably the melting point of the copolymer + 20°C to the melting point of the copolymer + 140°C. There is no particular limitation on the method for cutting the copolymer, and conventionally known methods such as a wire cutting method, a heat cutting method, an underwater cutting method, and a sheet cutting method can be used. The volatile components in the pellets can also be removed by heating the obtained pellets (degassing treatment). The obtained pellets can also be treated by contacting with warm water at 30°C to 200°C, steam at 100°C to 200°C, or hot air at 40°C to 200°C.
[0067] The copolymer obtained by polymerization can also be subjected to fluorination treatment. Fluorination treatment can be carried out by contacting the copolymer that has not been subjected to fluorination treatment with a fluorine-containing compound. Through fluorination treatment, thermally unstable functional groups such as -COOH, -COOCH3, -CH2OH, -COF, -CF=CF2, -CONH2 and thermally relatively stable functional groups such as -CF2H of the copolymer can be converted into extremely thermally stable -CF3. As a result, the total number (number of functional groups) of COOH, -COOCH3, -CH2OH, -COF, -CF=CF2, -CONH2 and -CF2H of the copolymer can be easily adjusted to the above range.
[0068] The fluorine-containing compound is not particularly limited, and a fluorine radical source that generates fluorine radicals under fluorination conditions can be cited. As the above-mentioned fluorine radical source, F2 gas, CoF3, AgF2, UF6, OF2, N2F2, CF3OF, fluorinated halogens (such as IF5, ClF3), etc. can be cited.
[0069] The fluorine free radical source such as F2 gas can be 100% concentration, but from the aspect of safety, it is preferably mixed with an inert gas and diluted to 5% to 50% by mass for use, and more preferably diluted to 15% to 30% by mass for use. As the above-mentioned inert gas, nitrogen, helium, argon, etc. can be cited, and nitrogen is preferred from the aspect of economy.
[0070] The conditions of the fluorination treatment are not particularly limited, and the copolymer in a molten state may be brought into contact with the fluorine-containing compound, but it may be generally carried out at a temperature below the melting point of the copolymer, preferably at 20°C to 240°C, and more preferably at 100°C to 220°C. The above-mentioned fluorination treatment is generally carried out for 1 hour to 30 hours, preferably for 5 hours to 25 hours. The fluorination treatment is preferably a treatment in which the copolymer that has not been fluorinated is brought into contact with fluorine gas (F2 gas).
[0071] The copolymer of the present invention may also be mixed with other components as required to obtain a composition. Other components include fillers, plasticizers, processing aids, mold release agents, pigments, flame retardants, lubricants, light stabilizers, weather stabilizers, conductive agents, antistatic agents, ultraviolet absorbers, antioxidants, foaming agents, fragrances, oils, softeners, dehydrofluorination agents, etc.
[0072] As fillers, for example, silicon dioxide, kaolin, clay, organic clay, talc, mica, aluminum oxide, calcium carbonate, calcium terephthalate, titanium oxide, calcium phosphate, calcium fluoride, lithium fluoride, cross-linked polystyrene, potassium titanate, carbon, boron nitride, carbon nanotubes, glass fibers, etc. can be cited. As conductive agents, carbon black, etc. can be cited. As plasticizers, dioctyl phthalate, pentaerythritol, etc. can be cited. As processing aids, carnauba wax, sulfone compounds, low molecular weight polyethylene, fluorine-based additives, etc. can be cited. As dehydrofluorination agents, organic onium, amidines, etc. can be cited.
[0073] As the other components, other polymers other than the above copolymers may be used. Examples of the other polymers include fluororesins, fluororubbers, and non-fluorinated polymers other than the above copolymers.
[0074] Examples of the method for producing the composition include a method of dry-mixing the copolymer and other components; a method of preliminarily mixing the copolymer and other components with a mixer and then melt-kneading them with a kneader, melt extruder or the like; and the like.
[0075] The copolymer of the present invention or the above-mentioned composition can be used as a processing aid, a molding material, etc., and is preferably used as a molding material. The aqueous dispersion, solution, suspension, and copolymer / solvent system of the copolymer of the present invention can also be utilized, and they can be applied as a coating, or used for encapsulation, impregnation, or film casting. However, the copolymer of the present invention is preferably used as the above-mentioned molding material because it has the above-mentioned characteristics.
[0076] The copolymer of the present invention or the above-mentioned composition may be molded to obtain a molded product.
[0077] The method for molding the copolymer or the composition is not particularly limited, and examples thereof include injection molding, extrusion molding, compression molding, blow molding, transfer molding, rotational molding, and roto-lining molding. As the molding method, extrusion molding, compression molding, injection molding, or transfer molding are preferred, and injection molding, extrusion molding, or transfer molding are more preferred because molded bodies can be produced at high productivity, and injection molding is further preferred. That is, as a molded body, an extrusion molded body, a compression molded body, an injection molded body, or a transfer molded body are preferred, and injection molded bodies, extrusion molded bodies, or transfer molded bodies are more preferred because they can be produced at high productivity, and injection molded bodies are further preferred.
[0078] Examples of the molded article containing the copolymer of the present invention include nuts, bolts, joints, films, bottles, washers, wire coatings, tubes, hoses, pipes, valves, sheets, seals, gaskets, tanks, rollers, containers, cocks, connectors, filter housings, filter covers, flow meters, pumps, wafer carriers, wafer boxes, and the like.
[0079] The molded product containing the copolymer of the present invention has excellent 60°C wear resistance, low hydrogen permeability, rigidity at a high temperature of 100°C, 230°C tensile creep resistance, durability against repeated loads, solvent crack resistance, and durability against tensile force applied at 230°C, and is therefore particularly suitable for use in piping components, valves, membranes, pipes, wire coverings, and the like.
[0080] The copolymer of the present invention, the composition or the molded article can be used, for example, in the following applications.
[0081] Films for food packaging, lining materials for fluid delivery pipelines used in food manufacturing processes, gaskets, sealing materials, sheets and other fluid delivery components for food manufacturing equipment;
[0082] Chemical plugs, packaging films, lining materials, gaskets, sealing materials, sheets and other liquid delivery components for fluid delivery pipelines used in chemical manufacturing processes;
[0083] Lining components for the inner surface of liquid tanks and piping in chemical equipment and semiconductor factories;
[0084] O (square) rings / tubes / gaskets, valve core materials, hoses, sealing materials, etc. used in automobile fuel systems and peripheral devices; fuel delivery components such as hoses and sealing materials used in automobile AT devices;
[0085] Flange gaskets, shaft seals, valve stem seals, sealing materials, hoses, etc. used in car engines and peripheral devices of automobiles; other automobile components such as automobile brake hoses, air conditioning hoses, radiator hoses, wire covering materials, etc.;
[0086] Semiconductor manufacturing equipment O (square) rings, tubes, gaskets, valve core materials, hoses, sealing materials, rollers, gaskets, diaphragms, joints and other semiconductor device liquid delivery components;
[0087] Coating rollers, hoses, tubes, ink containers and other coating and ink components for coating equipment;
[0088] Food and beverage conveying components such as tubes or hoses for food and beverages, tubes, hoses, belts, gaskets, joints, etc., food packaging materials, and glass cooking equipment;
[0089] Waste liquid transmission components such as pipes and hoses used for waste liquid transmission;
[0090] Components for high-temperature liquid transmission such as pipes and hoses used for high-temperature liquid transmission;
[0091] Steam piping components such as pipes and hoses used for steam piping;
[0092] Pipe corrosion protection tapes such as tapes wrapped around pipes on ship decks, etc.
[0093] Various covering materials such as wire covering materials, optical fiber covering materials, transparent surface covering materials and back-side agents provided on the light incident side surface of photovoltaic elements of solar cells;
[0094] Diaphragms of diaphragm pumps and sliding components such as various sealing gaskets;
[0095] Weather-resistant covers for agricultural films, various roofing materials, sidewalls, etc.;
[0096] Interior materials used in the construction field, non-combustible fireproof safety glass and other glass covering materials;
[0097] Lining materials for laminated steel sheets used in the home appliance field, etc.
[0098] Further examples of the fuel delivery member used in the fuel system of the above-mentioned automobile include fuel hoses, filler hoses, evaporator hoses, etc. The above-mentioned fuel delivery member can also be used as a fuel delivery member for sour gasoline, alcohol fuel, and fuel added with gasoline additives such as methyl tert-butyl ether resistance and amine resistance.
[0099] The chemical plug and packaging film have excellent chemical resistance to acids, etc. In addition, as the chemical liquid conveying member, there can also be mentioned a corrosion-resistant tape wound around the piping of chemical equipment.
[0100] Examples of the molded article include automobile radiator water chambers, chemical tanks, bellows, partitions, rollers, gasoline tanks, waste liquid transport containers, high temperature liquid transport containers, fisheries and fish farming tanks, and the like.
[0101] Examples of the molded bodies include automobile bumpers, door trims, instrument panels, food processing equipment, cooking machines, waterproof and oil-proof glass, lighting-related instruments, indicator panels and housings of OA instruments, electrically illuminated signboards, display screens, liquid crystal display screens, mobile phones, printer chassis, electrical and electronic components, groceries, trash cans, bathtubs, integrated bathrooms, ventilation fans, lighting frames, and the like.
[0102] The molded article containing the copolymer of the present invention can be suitably used as a compressed member such as a gasket or a seal. The compressed member of the present invention may be a gasket or a seal.
[0103] The size and shape of the compressed member of the present invention can be appropriately set according to the purpose, and there is no particular limitation. The shape of the compressed member of the present invention can be, for example, annular. In addition, the compressed member of the present invention can have a circular, elliptical, quadrilateral with rounded corners, etc. shape when viewed from above, and has a through hole in its central portion.
[0104] The compressed member of the present invention is preferably used as a member for constituting a non-aqueous electrolyte battery. The compressed member of the present invention is particularly suitable as a member used in a state of contact with a non-aqueous electrolyte in a non-aqueous electrolyte battery. That is, the compressed member of the present invention may have a liquid contact surface with the non-aqueous electrolyte in the non-aqueous electrolyte battery.
[0105] The nonaqueous electrolyte battery is not particularly limited as long as it is a battery having a nonaqueous electrolyte, and examples thereof include lithium ion secondary batteries, lithium ion capacitors, etc. In addition, members constituting the nonaqueous electrolyte battery include sealing members, insulating members, and the like.
[0106] The non-aqueous electrolyte is not particularly limited, and one or more of known solvents such as propylene carbonate, ethylene carbonate, butylene carbonate, γ-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, etc. can be used. The non-aqueous electrolyte battery can further include an electrolyte. The electrolyte is not particularly limited, and LiClO4, LiAsF6, LiPF6, LiBF4, LiCl, LiBr, CH3SO3Li, CF3SO3Li, cesium carbonate, etc. can be used.
[0107] The compressed member of the present invention can be preferably used as a sealing member such as a sealing gasket or a sealing pad, or an insulating member such as an insulating gasket or an insulating pad. A sealing member is a member used to prevent leakage of liquid or gas or intrusion of liquid or gas from the outside. An insulating member is a member used for electrical insulation. The compressed member of the present invention can also be a member used for both sealing and insulation purposes.
[0108] The copolymer of the present invention can be suitably used as a material for forming an electric wire coating.
[0109] The covered electric wire comprises a core wire and a covering layer disposed around the core wire and containing the copolymer of the present invention. For example, an extrusion molded body formed by melt extrusion molding the copolymer of the present invention on the core wire can be used as the covering layer. The covered electric wire is suitable for high-frequency transmission cables, flat cables, heat-resistant cables, etc., and is suitable for high-frequency transmission cables.
[0110] As the material of the core wire, a metal conductor material such as copper or aluminum can be used. The core wire preferably has a diameter of 0.02 mm to 3 mm. The core wire diameter is more preferably 0.04 mm or more, further preferably 0.05 mm or more, and particularly preferably 0.1 mm or more. The core wire diameter is more preferably 2 mm or less.
[0111] As specific examples of the core wire, AWG (American Wire Gauge)-46 (solid copper wire with a diameter of 40 μm), AWG-26 (solid copper wire with a diameter of 404 μm), AWG-24 (solid copper wire with a diameter of 510 μm), AWG-22 (solid copper wire with a diameter of 635 μm), etc. can be used.
[0112] The thickness of the coating layer is preferably 0.1 mm to 3.0 mm, and the thickness of the coating layer is also preferably 2.0 mm or less.
[0113] As a high-frequency transmission cable, a coaxial cable can be cited. A coaxial cable generally has a structure in which an inner conductor, an insulating coating, an outer conductor layer and a protective coating are sequentially stacked from the core to the periphery. A molded body containing the copolymer of the present invention can be suitably used as an insulating coating containing a copolymer. The thickness of each layer in the above structure is not particularly limited. Generally, the diameter of the inner conductor is about 0.1 mm to 3 mm, the thickness of the insulating coating is about 0.3 mm to 3 mm, the thickness of the outer conductor layer is about 0.5 mm to 10 mm, and the thickness of the protective coating is about 0.5 mm to 2 mm.
[0114] The coating layer may contain air bubbles, and the air bubbles are preferably uniformly distributed in the coating layer.
[0115] The average bubble diameter of the bubbles is not limited, and is, for example, preferably 60 μm or less, more preferably 45 μm or less, further preferably 35 μm or less, further preferably 30 μm or less, particularly preferably 25 μm or less, and particularly preferably 23 μm or less. In addition, the average bubble diameter is preferably 0.1 μm or more, more preferably 1 μm or more. The average bubble diameter can be obtained by obtaining an electron microscope image of a cross section of the wire, calculating the diameter of each bubble by image processing, and averaging them.
[0116] The foaming rate of the coating layer may be 20% or more. More preferably, it is 30% or more, further preferably, it is 33% or more, and further preferably, it is 35% or more. The upper limit is not particularly limited, for example, it is 80%. The upper limit of the foaming rate may be 60%. The foaming rate is a value calculated as ((specific gravity of the wire coating material - specific gravity of the coating layer) / specific gravity of the wire coating material) × 100. The foaming rate can be appropriately adjusted according to the application by, for example, adjusting the amount of gas inserted in the extruder described later, or by selecting the type of dissolved gas.
[0117] The covered electric wire may also have other layers between the core wire and the covering layer, and may further have other layers (outer layers) around the covering layer. When the covering layer contains bubbles, the electric wire of the present invention may also be a two-layer structure (skin-foam) in which a non-foam layer is inserted between the core wire and the covering layer; a two-layer structure (foam-skin) in which a non-foam layer is covered on the outer layer; and a three-layer structure (skin-foam-skin) in which a non-foam layer is covered on the outer layer of the skin-foam. The non-foam layer is not particularly limited, and may be a resin layer composed of TFE / HFP copolymers, TFE / PAVE copolymers, TFE / ethylene copolymers, vinylidene fluoride polymers, polyolefin resins such as polyethylene [PE], and polyvinyl chloride [PVC].
[0118] The covered electric wire can be produced, for example, by heating a copolymer using an extruder and extruding the copolymer onto a core wire in a molten state to form a covering layer.
[0119] When forming the coating, it is also possible to heat the copolymer and, under the state where the copolymer is molten, introduce gas into the copolymer to form the above-mentioned coating containing bubbles. As the gas, for example, a mixture of gases such as chlorodifluoromethane, nitrogen, carbon dioxide or the like or the above-mentioned gases can be used. The gas can be introduced into the heated copolymer in the form of pressurized gas, or it can be produced by mixing a chemical foaming agent in the copolymer. The gas dissolves in the copolymer in a molten state.
[0120] Furthermore, the copolymer of the present invention can be suitably used as a material for products for high-frequency signal transmission.
[0121] The high-frequency signal transmission product is not particularly limited as long as it is a product used for the transmission of high-frequency signals, and examples thereof include (1) insulating plates of high-frequency circuits, insulating materials of connecting components, molded plates such as printed wiring boards, (2) molded bodies such as bases and antenna covers of high-frequency vacuum tubes, and (3) coated wires such as coaxial cables and LAN cables. The high-frequency signal transmission product can be suitably used in equipment that utilizes microwaves, particularly 3 GHz to 30 GHz microwaves, such as satellite communication equipment and mobile phone base stations.
[0122] In the above-mentioned products for high-frequency signal transmission, the copolymer of the present invention can be suitably used as an insulator because of its low dielectric loss tangent.
[0123] As the above-mentioned (1) molded plate, a printed wiring board is preferred from the aspect of obtaining good electrical characteristics. The above-mentioned printed wiring board is not particularly limited, and examples thereof include printed wiring boards of electronic circuits such as mobile phones, various computers, and communication equipment. As the above-mentioned (2) molded body, a radome is preferred from the aspect of low dielectric loss.
[0124] The molded product containing the copolymer of the present invention can be suitably used as a film or a sheet.
[0125] The film of the present invention is useful as a release film. The release film can be produced by molding the copolymer of the present invention by melt extrusion molding, calendaring molding, press molding, cast molding, etc. From the perspective of obtaining a uniform film, the release film can be produced by melt extrusion molding.
[0126] The film of the present invention can be applied to the surface of a roller used in OA equipment. In addition, the copolymer of the present invention can be formed into a necessary shape by extrusion molding, compression molding, press molding, etc., and formed into a sheet, film, or tube, and used as a surface material for OA equipment rollers or OA equipment belts, etc. In particular, thin-walled tubes and films can be produced by melt extrusion molding.
[0127] The molded article containing the copolymer of the present invention can be suitably used as bottles, tubes, joints, valves, piping members, etc. These can be used for storage and distribution of chemical solutions.
[0128] Although the embodiments have been described above, it should be understood that various modifications may be made to the embodiments and details without departing from the spirit and scope of the claims.
[0129] <1> According to a first aspect of the present invention, there is provided a polymer comprising tetrafluoroethylene units and perfluoro(propyl vinyl ether) units,
[0130] The content of the perfluoro(propyl vinyl ether) unit is 4.4 to 5.2% by mass relative to the total monomer units, and the melt flow rate at 372° C. is 11.0 to 16.0 g / 10 minutes.
[0131] The number of functional groups per 10 6 The number of carbon atoms in the main chain is 50 or less.
[0132] <2> According to a second aspect of the present invention, there is provided the copolymer according to the first aspect, wherein the content of the perfluoro(propyl vinyl ether) unit is 4.4% by mass to 5.0% by mass based on all monomer units.
[0133] <3> According to a third aspect of the present invention, there is provided the copolymer according to the first or second aspect, wherein the melt flow rate at 372° C. is 12.0 g / 10 min to 15.0 g / 10 min.
[0134] <4> According to a fourth aspect of the present invention, there is provided an injection-molded article comprising the copolymer according to any one of the first to third aspects.
[0135] <5> According to a fifth aspect of the present invention, there is provided a molded article comprising the copolymer according to any one of the first to third aspects, wherein the molded article is a piping member, a valve, a film, a pipe, or an electric wire coating.
[0136] Example
[0137] Next, embodiments of the present invention will be described with reference to examples, but the present invention is not limited to the examples.
[0138] Each numerical value in the examples was measured by the following method.
[0139] (Content of monomer units)
[0140] The content of each monomer unit is measured using an NMR analyzer (for example, AVANCE300 high temperature probe manufactured by Bruker BioSpin).
[0141] (Melt Flow Rate (MFR))
[0142] The mass (g / 10 min) of the polymer flowing out from a nozzle having an inner diameter of 2.1 mm and a length of 8 mm at 372° C. and a load of 5 kg per 10 minutes was determined using a melt flow indexer G-01 (manufactured by Toyo Seiki Seisaku-sho, Ltd.) in accordance with ASTM D1238.
[0143] (Number of functional groups)
[0144] The pellets of the copolymer were formed by cold pressing to produce a film with a thickness of 0.25 mm to 0.30 mm. The film was scanned 40 times by a Fourier transform infrared spectrometer [FT-IR (Spectrum One, manufactured by PerkinElmer)] and analyzed to obtain an infrared absorption spectrum, which was a difference spectrum from the background spectrum of complete fluorination without the presence of functional groups. From the absorption peak of the specific functional group appearing in the differential spectrum, the following formula (A) was used to calculate the absorption peak of each 1×10 6 The number of functional groups N per carbon atom.
[0145] N=I×K / t(A)
[0146] I: Absorbance
[0147] K: Correction coefficient
[0148] t: film thickness (mm)
[0149] For reference, regarding the functional groups in the present invention, the absorption frequency, molar absorption coefficient and correction coefficient are shown in Table 2. The molar absorption coefficient is determined from the FT-IR measurement data of a low molecular weight model compound.
[0150] [Table 2]
[0151] Table 2
[0152]
[0153] (Melting Point)
[0154] Using a differential scanning calorimeter (trade name: X-DSC7000, manufactured by Hitachi High-Tech Science Co., Ltd.), the temperature was increased from 200°C to 350°C for the first time at a heating rate of 10°C / min, then cooled from 350°C to 200°C at a cooling rate of 10°C / min, and the temperature was increased from 200°C to 350°C for the second time at a heating rate of 10°C / min. The melting point was determined from the peak of the melting curve generated in the second heating process.
[0155] Comparative Example 1
[0156] 51.8L of pure water was put into a 174L autoclave with a stirrer. After fully replacing with nitrogen, 40.9kg of perfluorocyclobutane, 1.79kg of perfluoro(propyl vinyl ether) (PPVE) and 4.30kg of methanol were added, and the temperature in the system was maintained at 35°C. Next, tetrafluoroethylene (TFE) was pressed into 0.64MPa, and 0.051kg of a 50% methanol solution of di-n-propyl peroxydicarbonate was added to initiate polymerization. As the polymerization proceeded, the pressure in the system decreased, so TFE was continuously supplied to keep the pressure constant. For every 1kg of TFE supplied, 0.042kg of PPVE was added. The polymerization was terminated when the additional amount of TFE reached 40.9kg. The unreacted TFE was released, and after returning the pressure in the autoclave to atmospheric pressure, the obtained reaction product was washed with water and dried to obtain 42.5kg of powder.
[0157] The obtained powder was melt-extruded at 360° C. using a screw extruder (trade name: PCM46, manufactured by Ikegai Co., Ltd.) to obtain pellets of the copolymer. The PPVE content was measured using the obtained pellets by the above-mentioned method.
[0158] The obtained pellets are placed in a vacuum vibration reactor VVD-30 (manufactured by Ohkawara Manufacturing Co., Ltd.) and heated to 210°C. After evacuation, F2 gas diluted with N2 gas to 20 volume % is introduced to atmospheric pressure. 0.5 hours after the introduction of F2 gas, the system is temporarily evacuated and F2 gas is introduced again. Furthermore, 0.5 hours later, the system is evacuated again and F2 gas is introduced again. After that, the above-mentioned F2 gas introduction and evacuation operations are continued once every hour, and the reaction is carried out at a temperature of 210°C for 10 hours. After the reaction is completed, the reactor is fully replaced with N2 gas to terminate the fluorination reaction. Various physical properties are measured using the fluorinated pellets by the above-mentioned method.
[0159] Comparative Example 2
[0160] Fluorinated pellets were obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 1.92 kg, methanol to 4.79 kg, and 0.044 kg of PPVE was additionally added per 1 kg of TFE supplied to obtain 42.7 kg of dry powder.
[0161] Comparative Example 3
[0162] Fluorinated pellets were obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 2.05 kg, methanol to 0.33 kg, 50% methanol solution of di-n-propyl peroxydicarbonate to 0.103 kg, and 0.046 kg of PPVE was additionally added per 1 kg of TFE supplied to obtain 42.8 kg of dry powder.
[0163] Comparative Example 4
[0164] Fluorinated pellets were obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 2.69 kg, methanol to 2.48 kg, and 0.057 kg of PPVE was additionally added per 1 kg of TFE supplied to obtain 43.2 kg of dry powder.
[0165] Comparative Example 5
[0166] Fluorinated pellets were obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 2.43 kg, methanol to 1.75 kg, and 0.053 kg of PPVE was additionally added per 1 kg of TFE supplied to obtain 41.0 kg of dry powder.
[0167] Comparative Example 6
[0168] Unfluorinated pellets were obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 2.43 kg, methanol to 3.36 kg, and 0.053 kg of PPVE was additionally charged per 1 kg of TFE supplied to obtain 43.1 kg of dry powder.
[0169] Example 1
[0170] Fluorinated pellets were obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 2.05 kg, methanol to 3.43 kg, and 0.046 kg of PPVE was additionally added per 1 kg of TFE supplied to obtain 42.8 kg of dry powder.
[0171] Example 2
[0172] Fluorinated pellets were obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 2.17 kg, methanol to 3.45 kg, and 0.048 kg of PPVE was additionally added per 1 kg of TFE supplied to obtain 42.9 kg of dry powder.
[0173] Example 3
[0174] Fluorinated pellets were obtained in the same manner as in Comparative Example 1 except that PPVE was changed to 2.30 kg, methanol to 3.24 kg, and 0.050 kg of PPVE was additionally added per 1 kg of TFE supplied to obtain 43.0 kg of dry powder.
[0175] Example 4
[0176] PPVE was changed to 2.43 kg, methanol to 3.19 kg, 0.053 kg of PPVE was added for every 1 kg of TFE supplied, the heating temperature of the vacuum vibration reactor was changed to 180°C, and the reaction was carried out at 180°C for 10 hours to obtain 43.1 kg of dry powder. Except for this, fluorinated pellets were obtained in the same manner as Comparative Example 1.
[0177] The pellets obtained in Examples and Comparative Examples were used to measure various physical properties by the above-mentioned methods.
[0178] [Table 3]
[0179] Table 3
[0180]
[0181] The expression “<6” in Table 3 means that the number of functional groups is less than 6.
[0182] Next, the following properties were evaluated using the obtained pellets. The results are shown in Table 4.
[0183] (Abrasion test)
[0184] Using pellets and a hot press molding machine, a sheet test piece with a thickness of about 0.2 mm was made, from which a 10 cm × 10 cm test piece was cut. The test piece was fixed on the test bench of a Taber abrasion tester (No. 101 Special Taber Wear Tester, manufactured by Yasuda Seiki Manufacturing Co., Ltd.), and a wear test was performed using the Taber abrasion tester under the conditions of a test piece surface temperature of 60°C, a load of 500g, a wear wheel CS-10 (grinded with abrasive paper #240 for 20 turns), and a rotation speed of 60rpm. The weight of the test piece after 1000 turns was measured, and the weight of the test piece was further measured after the same test piece was tested at 6500 turns. The amount of wear was calculated using the following formula.
[0185] Wear amount (mg) = M1 - M2
[0186] M1: Test piece weight after 1000 revolutions (mg)
[0187] M2: Test piece weight after 6500 revolutions (mg)
[0188] (Hydrogen permeability coefficient)
[0189] Using the pellets and a hot press molding machine, a sheet test piece with a thickness of about 0.1 mm was prepared. The obtained test piece was used to measure the hydrogen permeability according to the method described in JIS K7126-1:2006 using a differential pressure gas permeability meter (L100-5000 gas permeability meter, manufactured by Systech Illinois). The permeation area was 50.24 cm 2 , the value of the hydrogen permeability at a test temperature of 60°C and a test humidity of 0% RH. The hydrogen permeability coefficient was calculated by the following formula using the obtained hydrogen permeability and the thickness of the test piece.
[0190] Hydrogen permeability coefficient (cm 3 mm / (m 2 ·24h·atm))=GTR×d
[0191] GTR: Hydrogen permeability (cm 3 / (m 2 24h atm)
[0192] d: Test piece thickness (mm)
[0193] (100℃ load deflection)
[0194] Using pellets and a hot press molding machine, a sheet test piece with a thickness of about 3.0 mm was made, from which a test piece of 80×10 mm was cut out and heated at 100°C for 20 hours in an electric furnace. In addition to using the obtained test piece, the test was carried out using a heat deformation tester (manufactured by Yasuda Seiki Manufacturing Co., Ltd.) according to the method described in JIS K-K7191-1, at a test temperature of 30°C to 150°C, a heating rate of 120°C / hour, a bending stress of 1.8MPa, and a flat method. The load deflection rate was calculated by the following formula. The sheet with a small load deflection rate at 100°C has excellent rigidity at high temperature.
[0195] Load deflection (%) = a2 / a1×100
[0196] a1: Thickness of the test piece before the test (mm)
[0197] a2: Deflection at 100°C (mm)
[0198] (Tensile creep test)
[0199] The tensile creep strain was measured using a Hitachi High-Tech TMA-7100. A pellet and a hot press were used to make a sheet with a thickness of about 0.1 mm, and a sample with a width of 2 mm and a length of 22 mm was made from the sheet. The sample was mounted on a measuring fixture with a distance of 10 mm between the fixtures. For the sample, a cross-sectional load of 2.63 N / mm 2 The sample was loaded in a manner of 230°C, and the sample length displacement (mm) was measured from 90 minutes after the start of the test to 555 minutes after the start of the test, and the ratio of the length displacement (mm) to the initial sample length (10 mm) was calculated (tensile creep strain (%)). The sheet with a small tensile creep strain (%) measured at 230°C and 555 minutes is not easy to elongate even when loaded with a tensile load in a very high temperature environment, and has excellent high-temperature tensile creep properties.
[0200] (Tensile strength after 80,000 cycles)
[0201] The tensile strength after 80,000 cycles was measured using a fatigue testing machine MMT-250NV-10 manufactured by Shimadzu Corporation. A sheet with a thickness of about 2.4 mm was made using pellets and a hot press molding machine, and a dumbbell-shaped sample (thickness 2.4 mm, width 5.0 mm, measuring portion length 22 mm) was made using an ASTM D1708 micro dumbbell. The sample was mounted on a measuring fixture, and the measuring fixture was placed in a constant temperature bath at 150°C with the sample mounted. Stretching in a uniaxial direction was repeated with a stroke of 0.2 mm and a frequency of 100 Hz, and the tensile strength of each stretch (tensile strength when the stroke is +0.2 mm) was measured. The tensile strength after 80,000 cycles was calculated from the measured value according to the following formula. In this embodiment, the cross-sectional area of the sample is 12.0 mm 2 .
[0202] Tensile strength after 80,000 cycles (mN / mm 2 ) = tensile strength (80,000 times) (mN) / cross-sectional area of sample (mm 2 )
[0203] The tensile strength after 80,000 cycles is the ratio of the tensile strength to the cross-sectional area of the sample when the load is applied 80,000 times. A sheet with a high tensile strength after 80,000 cycles maintains a high tensile strength even after the load is applied 80,000 times, and has excellent durability against repeated loads.
[0204] (85% phosphoric acid immersion crack test (chemical immersion crack test))
[0205] Using pellets and a hot press molding machine, a molded body with a thickness of about 2 mm was made. Using a 13.5mm×38mm rectangular dumbbell, the obtained piece was punched to obtain three test pieces. In the center of the long side of each test piece obtained, a 19mm×0.45mm blade was used to cut a notch according to ASTM D1693. Three notched test pieces and 25g of 85% phosphoric acid aqueous solution were placed in a 100mL container, and after heating at 120°C in an electric furnace for 20 hours, the notched test piece was taken out. The three notched test pieces obtained were installed in a stress crack test fixture according to ASTM D1693, and after heating at 200°C in an electric furnace for 24 hours, the notch and its surroundings were visually observed to count the number of cracks. The piece without cracks also has excellent solvent crack resistance after being immersed in the liquid.
[0206] ○: The number of cracks is 0
[0207] ×: The number of cracks is 1 or more
[0208] (Injection moldability)
[0209] ·condition
[0210] The copolymer was injection molded using an injection molding machine (manufactured by Sumitomo Heavy Industries, Ltd., SE50EV-A) with a barrel temperature of 390°C, a mold temperature of 200°C, and an injection speed of 10 mm / s. As a mold, a mold (100 mm×100 mm×2 mm, side gate) in which HPM38 was plated with Cr was used. The obtained injection molded body was observed and evaluated according to the following criteria. The presence or absence of surface roughness was confirmed by contacting the surface of the injection molded body.
[0211] Evaluation (visual)
[0212] 2: The surface is smooth as a whole, and no flow marks are observed on the entire molded body.
[0213] 1: Surface roughness is confirmed within 1 cm from the location of the mold gate, or flow marks are observed within 1 cm from the location of the mold gate, but the surface of the other range is smooth as a whole and no flow marks are observed.
[0214] 0: Surface roughness was confirmed within 4 cm from the site where the gate of the mold was located, or flow marks were observed within 4 cm from the site where the gate of the mold was located.
[0215] (230℃ tensile strength)
[0216] The pellets and a hot press molding machine were used to obtain a 2.0 mm thick test piece (compression molding). A dumbbell-shaped test piece was punched out from the test piece using an ASTM V-type dumbbell, and the obtained dumbbell-shaped test piece was used to measure the tensile strength at 230° C. under the conditions of 50 mm / min using Autograph (AG-I 300 kN manufactured by Shimadzu Corporation) according to ASTM D638.
[0217] A molded body having a high tensile strength at 230°C is not easily broken even when a tensile force is applied at a high temperature.
[0218] (Film formability)
[0219] Use the obtained pellets to The film was produced using a T-die by an extruder (manufactured by Imoto Seisakusho Co., Ltd.) The extrusion molding conditions were as follows.
[0220] a) Winding speed: 1m / min
[0221] b) Roller temperature: 120°C
[0222] c) Film width: 70mm
[0223] d)Thickness: 0.10mm
[0224] e) Extrusion conditions:
[0225] · Single screw extruder with barrel diameter = 14mm, L / D = 20
[0226] Extruder set temperature: barrel C-1 (330°C), barrel C-2 (350°C), barrel C-3 (370°C), T-die head (380°C)
[0227] The obtained film was visually inspected and confirmed to have no problem in appearance.
[0228] (Wire coating molding conditions)
[0229] pass A wire coating molding machine (manufactured by TANABE PLASTIC MACHINERY CO., LTD.) was used to extrusion coat a copper conductor having a conductor diameter of 0.50 mm with the following coating thickness to obtain a coated wire. The wire coating extrusion molding conditions were as follows.
[0230] a) Core conductor: conductor diameter 0.50mm
[0231] b) Coating thickness: 0.20mm
[0232] c) Diameter of coated wire: 0.90mm
[0233] d) Wire pulling speed: 50m / min
[0234] e) Extrusion conditions:
[0235] · Single screw extruder with barrel diameter = 30mm, L / D = 22
[0236] ·Mold (inner diameter) / sheet (outer diameter) = 8.0mm / 5.0mm
[0237] The set temperatures of the extruder were: barrel C-1 (330°C), barrel C-2 (360°C), barrel C-3 (375°C), head H (390°C), die head D-1 (405°C), die head D-2 (395°C). The core wire preheating was set to 80°C.
[0238] The obtained electric wire was visually checked to confirm that there was no problem with the appearance.
[0239] [Table 4]
[0240]
Claims
1. A copolymer comprising tetrafluoroethylene units and perfluoro(propyl vinyl ether) units, The content of the perfluoro(propyl vinyl ether) unit is 4.4% to 5.2% by mass based on the total monomer units. The melt flow rate at 372°C is 11.0 g / 10 min to 16.0 g / 10 min. The number of functional groups per 10 6 The number of carbon atoms in the main chain is 50 or less.
2. The copolymer according to claim 1, wherein The content of the perfluoro(propyl vinyl ether) unit is 4.4% by mass to 5.0% by mass based on all monomer units.
3. The copolymer according to claim 1 or 2, wherein The melt flow rate at 372° C. is 12.0 g / 10 min to 15.0 g / 10 min. 4 . An injection-molded article comprising the copolymer according to claim 1 .
5. A molded product comprising the copolymer according to any one of claims 1 to 3, wherein The molded body is a piping member, a valve, a membrane, a tube or a wire coating.
Citation Information
Patent Citations
Thermoplastic resin composition
WO1995029956A1