Microchannel chip and method for manufacturing microchannel chip

By setting hydrophobic and hydrophilic regions in the microfluidic chip, and using the contact angle control of the silicone-containing polymer layer, the problems of reflux and contamination of the reaction liquid are solved, and the accurate reaction between the test liquid and multiple reagents is achieved. evaluate.

CN118946809APending Publication Date: 2024-11-12TOPPAN HOLDINGS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030761.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-15
Filing Date
2023-03-01
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing microfluidic chips are prone to reflux and contamination of the reaction liquid under the shape of the flow path material, especially due to capillary phenomena and the formation of bubbles.

Method used

The hydrophobic region and the hydrophilic region are arranged in the microfluidic path chip, and the hydrophobic surface is formed by patterning the photosensitive resin, and the action of the droplets is controlled to prevent the reaction liquid from flowing backwards. The contact angle of the silicone-containing polymer layer is controlled at More than 90 degrees and less than 130 degrees.

Benefits of technology

It effectively prevents the reflux and contamination of the reaction liquid in the microfluidic chip, and realizes the accurate reaction evaluation of the test liquid and multiple reagents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946809A_ABST
    Figure CN118946809A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a micro-channel chip and a method for manufacturing a micro-channel chip, whereby it is possible to prevent backflow of reaction liquids in the micro-channel chip and to prevent contamination between the reaction liquids. A representative micro-channel chip according to the present invention is characterized by having an input part into which a liquid is introduced, a channel part through which the liquid flows, and an output part through which the liquid is discharged or a reagent fixing part for bringing the liquid into contact with a reagent ("output part"), the flow path portion has a region (hydrophobic region) in which the contact angle of the surface in contact with the liquid is 90-130 degrees. The flow path part is surrounded by at least a substrate layer, a partition wall layer, and an upper cover layer on a substrate, and the surface of at least one of the substrate layer, the partition wall layer, and the upper cover layer has the hydrophobic region.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a microfluidic chip and a method for manufacturing the microfluidic chip. Background Art

[0002] In recent years, a technology has been proposed that uses photolithography and thick film process technology to form a micro-reaction field and can perform inspections on trace amounts of liquids in the microliter to nanoliter units. This technology using a micro-reaction field is called μ-TAS (Micro Total Analysis System).

[0003] μ-TAS is used in gene testing, chromosome testing, cell testing, drug development, biotechnology, trace substance testing in the environment, investigation of breeding environments for crops, gene testing of crops, etc. By introducing μ-TAS technology, great effects such as automation, high speed, high precision, low cost, rapidity, and reduced environmental impact can be achieved.

[0004] μ-TAS often utilizes micrometer-sized flow paths (microflow paths, microchannels) formed on a substrate for reaction, observation, etc. Such devices are called microflow path chips, etc.

[0005] In the past, such microfluidic chips were made using technologies such as injection molding, mold molding, cutting, and etching. In addition, as the substrate of the microfluidic chip, glass substrates are mainly used because of the ease of manufacturing and optical detection. On the other hand, the development of microfluidic chips using resin materials that are lightweight, not easily broken, and inexpensive compared to glass substrates is also underway. As a method for manufacturing a microfluidic chip using resin materials, there is mainly a method of forming a resin pattern for the flow path by photolithography and bonding a cover material to the pattern to produce a microfluidic chip. According to this method, the formation of a fine flow path pattern, which is also difficult according to the prior art, can also be achieved.

[0006] In addition, the following sensitivity evaluation can be performed based on the microfluidic chip: different types of reagents are pre-fixed at different places in the flow path, and a test liquid is introduced from the entrance of the flow path, so that the test liquid reacts with the reagent to evaluate the sensitivity. It has the advantage of being able to evaluate the reaction of the test liquid with multiple reagents at one time. On the other hand, for such a microfluidic chip, it is important to prevent contamination between the reaction liquids. Because if the reaction liquids are mixed with each other, accurate evaluation cannot be performed. A method for prescribing the shape of a buffer zone in order to prevent contamination between multiple chambers is disclosed. For example, Patent Document 1 discloses that in a fluid processing device in which multiple trapezoidal buffer zones connected to chambers are connected via a flow path, the bottom length of the trapezoid is set to be longer than the waist length, thereby suppressing contamination between chambers.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2021-156780 Summary of the invention

[0010] Technical problem to be solved by the invention

[0011] However, in the prior art where the material constituting the flow path is hydrophilic, backflow of the reaction solution may sometimes occur. In addition, in a structure where the buffer zone and the chamber are connected by a thin flow path, backflow of the reaction solution may easily occur due to capillary phenomena. In addition, bubbles may easily be generated locally in the portion where the shape of the flow path changes, and the bubbles may sometimes be a cause of backflow of the reaction solution.

[0012] The present inventors have conducted intensive studies and found that if a flow channel chip is provided with a hydrophobic region and a hydrophilic region using a material constituting the flow channel, contamination of the reaction solution can be stably prevented.

[0013] Therefore, an object of the present invention is to provide a microchannel chip and a method for manufacturing the microchannel chip which can prevent the backflow of reaction solutions in the microchannel chip and prevent the contamination between reaction solutions.

[0014] Means for solving technical problems

[0015] In order to solve the above-mentioned technical problems, a representative microfluidic chip of the present invention is characterized in that it has: an input part for introducing fluid; a flow path part through which the above-mentioned fluid flows; and an output part for discharging the above-mentioned fluid or a reagent fixing part for contacting the above-mentioned fluid with a reagent (hereinafter collectively referred to as the "output part"), wherein the above-mentioned flow path part has an area where the contact angle of the surface in contact with the above-mentioned fluid is greater than 90 degrees and less than 130 degrees (hereinafter referred to as the "hydrophobic area").

[0016] Effects of the Invention

[0017] According to the present invention, a microchannel chip capable of preventing backflow of reaction reagents in a microchannel chip and preventing contamination between reaction solutions can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1A It is a schematic plan view showing the micro-channel chip according to the first embodiment.

[0019] Figure 1B To indicate the Figure 1A The diagram shows a cross section of the microfluidic chip cut along line AA.

[0020] Figure 1C To indicate the Figure 1AThe cross-section of the microfluidic chip is shown along line BB.

[0021] Figure 1D To indicate the Figure 1A The cross-section of the microfluidic chip is shown along line CC.

[0022] Figure 2 This is a flowchart showing an example of the method for manufacturing the micro-channel chip according to the first embodiment.

[0023] Figure 3A This is a flow chart showing the manufacturing method of Example 1.

[0024] Figure 3B The microfluidic chip manufactured in Example 1 is Figure 1B The cross-sectional view corresponding to the AA cross-sectional view.

[0025] Figure 3C The microfluidic chip manufactured in Example 1 is Figure 1D The CC cross-sectional view corresponds to the cross-sectional view.

[0026] Figure 4A It is a flowchart showing the manufacturing method of Example 2.

[0027] Figure 4B The microfluidic chip manufactured in Example 2 is Figure 1B The cross-sectional view corresponding to the AA cross-sectional view.

[0028] Figure 4C The microfluidic chip manufactured in Example 2 is Figure 1D The CC cross-sectional view corresponds to the cross-sectional view.

[0029] Figure 5A This is a flow chart showing the manufacturing method of Example 3.

[0030] Figure 5B The microfluidic chip manufactured in Example 3 is Figure 1B The cross-sectional view corresponding to the AA cross-sectional view.

[0031] Figure 5C The microfluidic chip manufactured in Example 3 is Figure 1D The CC cross-sectional view corresponds to the cross-sectional view.

[0032] Fig. 6A It is a flowchart showing the manufacturing method of Example 4.

[0033] Figure 6B The microfluidic chip manufactured in Example 4 is Figure 1B The cross-sectional view corresponding to the AA cross-sectional view.

[0034] Figure 6CThe microfluidic chip manufactured in Example 4 is Figure 1D The CC cross-sectional view corresponds to the cross-sectional view.

[0035] Fig. 7A This is a flow chart showing the manufacturing method of Example 5.

[0036] Figure 7B The microfluidic chip manufactured in Example 5 is Figure 1B The cross-sectional view corresponding to the AA cross-sectional view.

[0037] Figure 7C The microfluidic chip manufactured in Example 5 is Figure 1D The CC cross-sectional view corresponds to the cross-sectional view.

[0038] Fig. 8A It is a flow chart showing the manufacturing method of Example 6.

[0039] Figure 8B The microfluidic chip manufactured in Example 6 is Figure 1B The cross-sectional view corresponding to the AA cross-sectional view.

[0040] Figure 8C The microfluidic chip manufactured in Example 6 is Figure 1D The CC cross-sectional view corresponds to the cross-sectional view.

[0041] Fig. 9A This is a flow chart showing the manufacturing method of Example 7.

[0042] Fig. 9B The flow path chip manufactured in Example 7 is Figure 1B The cross-sectional view corresponding to the AA cross-sectional view.

[0043] Fig. 9C The flow path chip manufactured in Example 7 is Figure 1D The CC cross-sectional view corresponds to the cross-sectional view.

[0044] Fig. 10A This is a flow chart showing the manufacturing method of Example 8.

[0045] Fig. 10B The microfluidic chip manufactured in Example 8 is Figure 1B The cross-sectional view corresponding to the AA cross-sectional view.

[0046] Fig. 10C The microfluidic chip manufactured in Example 8 Figure 1D The CC cross-sectional view corresponds to the cross-sectional view.

[0047] Fig.11A This is a flow chart showing the manufacturing method of Example 9.

[0048] Fig. 11B The microfluidic chip manufactured in Example 9 is Figure 1B The cross-sectional view corresponding to the AA cross-sectional view.

[0049] Fig. 11C The microfluidic chip manufactured in Example 9 is Figure 1D The CC cross-sectional view corresponds to the cross-sectional view.

[0050] Fig. 12A It is a flowchart which shows the manufacturing method of comparative example 1.

[0051] Fig. 12B The microfluidic chip manufactured in Comparative Example 1 is Figure 1B The cross-sectional view corresponding to the AA cross-sectional view.

[0052] Fig. 12C The microfluidic chip manufactured in Comparative Example 1 is Figure 1D The CC cross-sectional view corresponds to the cross-sectional view.

[0053] Fig.13 The microfluidic chip of the second embodiment Figure 1D The CC cross-sectional view corresponds to the cross-sectional view.

[0054] Fig.14 A microfluidic chip according to a modified example of the second embodiment Figure 1D The CC cross-sectional view corresponds to the cross-sectional view. DETAILED DESCRIPTION

[0055] After in-depth research, the present inventors found that by providing a hydrophobic region in the flow path of the microfluidic chip, the movement of the droplets can be controlled to prevent contamination between the reaction solutions in the flow path. The formation of the hydrophobic region can be achieved by patterning of a photosensitive resin, so it is a very simple method. Thus, the present inventors invented a microfluidic chip that can prevent contamination between the reaction solutions in the microfluidic chip and a method for manufacturing the microfluidic chip.

[0056] Hereinafter, each configuration of each embodiment of the present invention will be described with reference to the drawings.

[0057] The following embodiments are not intended to limit the scope of the claims. In addition, the combination of features described in the embodiments is not necessarily essential to solving the problem of the invention.

[0058] In the description of the drawings, the same parts are indicated by the same reference numerals. When there are multiple components having the same or identical functions, different suffixes are sometimes attached to the same reference numerals for description. In addition, when there is no need to distinguish these multiple components, the suffixes are sometimes omitted for description.

[0059] In order to facilitate understanding of the invention, the position, size, shape, range, etc. of each component in the drawings may not represent the actual position, size, shape, range, etc. Therefore, the present invention is not necessarily limited to the position, size, shape, range, etc. disclosed in the drawings.

[0060] [First embodiment]

[0061] <Basic structure of microfluidic chip>

[0062] Figure 1A to Figure 1D Schematic diagram for explaining a configuration example of a microfluidic chip 1 according to the first embodiment of the present invention. Specifically, Figure 1A 1 is a schematic top view showing the microfluidic chip 1 according to the first embodiment. Figure 1B To indicate the Figure 1A The cross-sectional view of the microfluidic chip 1 is obtained by cutting the microfluidic chip 1 along the line AA shown. Figure 1C To indicate the Figure 1A The cross-sectional view of the microfluidic chip 1 is obtained by cutting the microfluidic chip 1 along the line BB shown. Figure 1D To indicate the Figure 1A The cross-sectional view of the micro-flow channel chip 1 is shown along line CC.

[0063] like Figure 1A As shown, the microfluidic chip 1 has an input portion 2 (sometimes also referred to as an "inlet") for introducing a fluid (such as a liquid), a flow path portion 3 through which the fluid introduced from the input portion 2 flows, and output portions 4, 5 (sometimes also referred to as an "outlet") for discharging the fluid from the flow path portion 3. In the microfluidic chip 1, the flow path portion 3 is covered by an upper cover layer 13 described later, and the input portion 2 and the output portions 4, 5 are through holes provided in the upper cover layer 13. It should be noted that one flow path of the flow path portion 3 is divided into two flow paths along the output portions 4, 5 at the branch portion 18. The input portion 2 to the branch portion 18 is composed of the main flow path portion 3a, the branch portion 18 to the output portion 4 is composed of the branch flow path portion 3b, and the branch portion 18 to the output portion 5 is composed of the branch flow path portion 3c. In addition, a reagent fixing portion (hereinafter sometimes referred to as "near the outlet" for simplicity) where a fixed reagent is provided near the output portions 4, 5, and the fluid introduced from the input portion 2 contacts the reagent can be provided. When a reagent fixing unit is provided, output units 4 and 5 may not necessarily be provided. Hereinafter, unless otherwise specified, output units 4 and 5 in a narrow sense and reagent fixing units are collectively referred to as "output units." It should be noted that reagents include substances to be tested using a microfluidic chip, and are not limited to chemicals.

[0064] Figure 1A The flow path portion 3 is shown to be visible through the transparent upper cover layer 13. Figure 1AThe micro-channel chip 1 shown is a micro-channel chip having two outlets and a channel branched from an inlet. The micro-channel chip 1 forms a simple channel for simultaneously evaluating the reaction between a test solution and two reagents.

[0065] In the microfluidic chip 1, at least one input part and at least two output parts may be provided. In addition, in the microfluidic chip 1, a plurality of flow path parts 3 may be provided, and the design may be such that the fluid introduced from the input part 2 can be merged or separated.

[0066] Here, the components constituting the flow channel section 3 in the micro-flow channel chip 1 will be described in detail.

[0067] like Figure 1B As shown, the microfluidic chip 1 comprises: a substrate 10, a base material layer 11 provided on the substrate 10, a partition wall layer 12 provided on the base material layer 11 for forming a flow path, and an upper cover layer 13 provided on the surface of the partition wall layer 12 opposite to the substrate 10. The main flow path portion 3a through which the fluid introduced from the input portion 2 flows is an area surrounded by the substrate 10, the base material layer 11, the partition wall layer 12 and the upper cover layer 13. A layer 14 containing a silicone polymer is formed on the surface of any one of the base material layer 11, the partition wall layer 12 and the upper cover layer 13. The layer 14 containing a silicone polymer does not necessarily have a constant thickness. The detailed description of the layer 14 containing a silicone polymer will be described later. As described above, the fluid is introduced from the input portion 2 provided on the upper cover layer 13 to the main flow path portion 3a. The base material layer 11 is sometimes used to improve the adhesion between the substrate 10 and the partition wall layer, or is provided as an area for changing the hydrophobicity in the flow path as described later.

[0068] like Figure 1C As shown, the branch flow path portion 3b is a region surrounded by a base material layer 11, a partition wall layer 12, and an upper cover layer 13 provided on a substrate 10, and its basic structure is similar to that of Figure 1B The fluid flowing through the branch flow path portion 3b is discharged from the output portion 4. It should be noted that in the following description, unless otherwise specified, the description of the branch flow path portion 3b is also applicable to the branch flow path portion 3c.

[0069] The cross-sectional view along the flow path is Figure 1D The basic composition and Figure 1B as well as Figure 1C same.

[0070] The substrate 10 , the base material layer 11 , the partition wall layer 12 , and the cap layer 13 are further described below.

[0071] <Substrate>

[0072] The substrate 10 is a member serving as a base of the micro-channel chip 1 , and the shape of the channel of the channel section 3 is formed by the partition wall layer 12 provided on the substrate 10 .

[0073] The substrate 10 can be formed of any of a translucent material or a non-translucent material. For example, when the state in the flow path portion 3 (e.g., the state of the fluid) is detected and observed by light, a material with excellent transparency to the light can be used. As a translucent material, resin or glass can be used. As a resin for forming a translucent material of the substrate 10, from the viewpoint of being suitable for forming the main body of the microfluidic chip 1, acrylic resin, methacrylic resin, polypropylene, polycarbonate resin, cycloolefin resin, polystyrene resin, polyester resin, polyurethane resin, silicone resin, fluorine resin, etc. can be listed. In addition, among glass substrates, a glass substrate with a surface coated with silicone or fluorine can be used.

[0074] In addition, for example, when it is not necessary to detect or observe the state in the flow path portion 3 (e.g., the state of the fluid) by light, a non-translucent material may be used. Examples of non-translucent materials include silicon wafers, copper plates, etc. The thickness of the substrate 10 is not particularly limited, but is preferably within a range of 10 μm (0.01 mm) or more and 10 mm or less, since a certain degree of rigidity is required in the flow path forming process.

[0075] <Base layer>

[0076] The base material layer 11 is provided on the substrate 10. The base material layer 11 can be formed of a resin material. As the resin material of the base material layer 11, for example, a photosensitive resin can be used.

[0077] The photosensitive resin forming the substrate layer 11 preferably has photosensitivity to light of wavelengths above 190nm and below 400nm in the ultraviolet region. As the photosensitive resin, photoresists such as liquid resists or dry film resists can be used. These photosensitive resins can be any of the positive type dissolved in the photosensitive region or the negative type in which the photosensitive region is insoluble. As a photosensitive resin composition suitable for forming the substrate layer 11 in the microfluidic chip 1, free radical negative photosensitive resins containing alkali-soluble polymers, addition polymerizable monomers and photopolymerization initiators can be listed. For example, as a photosensitive resin material, acrylic resins, acrylic polyurethane resins (polyurethane acrylate resins), epoxy resins, polyamide resins, polyimide resins, polyurethane resins, polyester resins, polyether resins, polyolefin resins, polycarbonate resins, polystyrene resins, norbornene resins, phenol novolac resins, and other resins with photosensitivity can be used alone or mixed with multiple uses or copolymerized.

[0078] In addition, from the viewpoint of promoting the deposition of low molecular weight siloxane volatilized when the polydimethylsiloxane (PDMS) described later is heated, it is more preferred that the resin constituting the base material layer 11 contains polysiloxane and silane coupling agent. By containing these substances, silanol bonds are formed with low molecular weight siloxane, and the layer 14 containing siloxane polymer is easily formed on the surface of the base material layer 11. In addition, the material itself containing the silane coupling agent is also possible from the viewpoint of improving the close fit with the partition wall layer 12. This viewpoint will be described later in other embodiments.

[0079] The thickness of the base material layer 11 is not particularly limited, but does not need to be particularly thick from the viewpoint of improving the adhesion between the substrate 10 and the partition wall layer 12 or exposing the substrate 10 by patterning, and is preferably thin.

[0080] <Partition wall layer>

[0081] The partition wall layer 12 is provided on the substrate and is one of the components forming the flow path portion 3. The partition wall layer 12 can be formed of a resin material. As the resin material of the partition wall layer 12, for example, a photosensitive resin can be used.

[0082] The photosensitive resin forming the partition wall layer 12 is preferably sensitive to light with a wavelength of more than 190nm and less than 400nm in the ultraviolet region. As the photosensitive resin, a photoresist such as a liquid resist or a dry film resist can be used. These photosensitive resins can be any of a positive type that is dissolved in the photosensitive region or a negative type that is insoluble in the photosensitive region. As a photosensitive resin composition suitable for forming the partition wall layer 12 of the microfluidic chip 1, a free radical negative type photosensitive resin containing an alkali-soluble polymer, an addition polymerizable monomer and a photopolymerization initiator can be listed. For example, as a photosensitive resin material, acrylic resin, acrylic polyurethane resin (polyurethane acrylate resin), epoxy resin, polyamide resin, polyimide resin, polyurethane resin, polyester resin, polyether resin, polyolefin resin, polycarbonate resin, polystyrene resin, norbornene resin, phenol novolac resin, and other resins with photosensitivity can be used alone or mixed with multiple uses or copolymerized.

[0083] It should be noted that, in the first embodiment, the resin material of the partition wall layer 12 is not limited to a photosensitive resin, and may be, for example, silicone rubber (PDMS: polydimethylsiloxane) or a synthetic resin. As the synthetic resin, for example, polymethyl methacrylate resin (PMMA), polycarbonate (PC), polystyrene resin (PS), polypropylene (PP), cycloolefin polymer (COP), cycloolefin copolymer (COC), etc. may be used. The resin material of the partition wall layer 12 is preferably selected appropriately according to the application.

[0084] In addition, the thickness of the partition wall layer 12 on the substrate 10, that is, the height of the flow path portion 3, is not particularly limited, but the height of the flow path portion 3 needs to be set to be greater than the substance (e.g., reagent, bacteria, cells, red blood cells, white blood cells, etc.) contained in the fluid introduced into the flow path portion 3 as the analysis / inspection object. Therefore, the thickness of the partition wall layer 12, that is, the height (depth) of the flow path portion 3 is preferably within the range of 1 μm or more and 500 μm or less, more preferably within the range of 10 μm or more and 100 μm, and further preferably within the range of 40 μm or more and 60 μm or less. It should be noted that the height (depth) of the flow path portion is the length in the direction perpendicular to the substrate surface.

[0085] In addition, similarly, the width of the flow path portion 3 needs to be set larger than the substance to be analyzed / inspected, and therefore, the width of the flow path portion 3 defined by the partition wall layer 12 is preferably within the range of 1 μm or more and 1000 μm or less, more preferably within the range of 10 μm or more and 500 μm or less, and further preferably within the range of 10 μm or more and 100 μm or less. It should be noted that the width of the flow path is the length in the direction parallel to the substrate surface and perpendicular to the length direction of the flow path.

[0086] Furthermore, since sufficient reaction time of the reaction solution needs to be ensured, the flow path length determined by the partition wall layer 12 is preferably in the range of 10 mm to 100 mm, more preferably in the range of 30 mm to 70 mm, and further preferably in the range of 40 mm to 60 mm.

[0087] <Upper cover>

[0088] In the micro-flow path chip 1 of the first embodiment, the upper cover layer 13 is Figure 1B The cover material (hereinafter sometimes referred to as the "cover material") covering the flow path portion 3 is shown. As described above, the cover layer 13 is provided on the surface of the partition wall layer 12 opposite to the substrate 10, sandwiching the partition wall layer 12 and facing the substrate 10. More specifically, as Figure 1B As shown, the side ends of the upper cover layer 13 are supported by the partition wall layer 12 , and the central region faces the substrate 10 . The central region defines the upper portion of the flow path portion 3 .

[0089] The upper cover layer 13 can be formed of any of a translucent material or a non-translucent material. For example, when the state in the flow path portion 3 (e.g., the state of the fluid) is detected and observed by light, a material with excellent transparency to the light can be used. As a translucent material, resin or glass can be used. As a resin forming the upper cover layer 13, from the viewpoint of being suitable for forming the main body of the microfluidic chip 1, acrylic resin, methacrylic resin, polypropylene, polycarbonate resin, cycloolefin resin, polystyrene resin, polyester resin, polyurethane resin, silicone resin, fluorine resin, etc. can be listed.

[0090] It should be noted that, in the first embodiment, the resin material of the upper cover layer 13 is not limited to the above, and for example, silicone rubber (PDMS: polydimethylsiloxane) and synthetic resin may also be used. As synthetic resins, for example, polymethyl methacrylate resin (PMMA), polycarbonate (PC), polystyrene resin (PS), polypropylene (PP), polyethylene terephthalate (PET), cycloolefin polymer (COP), cycloolefin copolymer (COC), etc. may be used. The resin material of the upper cover layer 13 is preferably selected according to the intended use. In particular, in the first embodiment, from the viewpoint of forming a layer containing a siloxane polymer on the surface of the flow path portion 3, PDMS is preferably used.

[0091] The thickness of the upper cover layer 13 is not particularly limited, but is preferably within a range of 10 μm to 10 mm, in view of the through holes corresponding to the input part 2 and the output parts 4, 5, which are respectively provided on the upper cover layer 13. In addition, it is preferred that the upper cover layer 13 is preliminarily provided with holes corresponding to the input part 2 for introducing fluid and the output parts 4, 5 for discharging fluid, respectively, before being bonded to the partition wall layer 12.

[0092] <Manufacturing method>

[0093] Next, a method for manufacturing the micro-channel chip 1 according to the first embodiment will be described. Figure 2 It is a flowchart showing an example of the method for manufacturing the micro-channel chip 1 according to the first embodiment.

[0094] Here, the case where the base material layer 11 and the partition wall layer 12 are formed by using a photosensitive resin is described as an example.

[0095] Figure 2 In the method for manufacturing a microfluidic chip, the steps of forming a base layer 11 (step S101), forming a partition wall layer 12 (step S102), surface modification treatment (UV treatment) (step S13), and bonding of a cover layer 13 (step S14) are included. The step of forming the base layer 11 (step S101) includes steps S1 to S6 described later. In addition, the step of forming the partition wall layer (step S102) includes steps S7 to S12 described later.

[0096] (Step S1)

[0097] The method for manufacturing the micro-flow channel chip 1 according to the first embodiment first performs a step of applying a resin onto the substrate 10 . Thus, a resin layer for forming the base material layer 11 is provided on the substrate 10 .

[0098] The method of forming the base material layer on the substrate 10 can be performed by, for example, coating the substrate 10 with a photosensitive resin. The coating can be performed by, for example, spin coating, spray coating, rod coating, etc., and spin coating is preferred from the viewpoint of film thickness controllability. The photosensitive resin in various forms such as liquid, solid, gel, and film can be coated on the substrate 10. For example, forming the photosensitive resin layer by a liquid resist is one of the preferred methods.

[0099] The resin (eg, photosensitive resin) may be applied onto the substrate 10 so that the thickness of the resin layer (eg, photosensitive resin layer), that is, the thickness of the base material layer 11, is within a range of 1 μm to 10 μm.

[0100] (Step S2)

[0101] After the photosensitive resin is formed on the substrate 10, a heat treatment (prebaking treatment) process is then performed for the purpose of removing the solvent contained in the resin (e.g., photosensitive resin) coated on the substrate 10. It should be noted that in the manufacturing method of the microfluidic chip 1 of the first embodiment, the prebaking process is not a necessary process, and it can be performed at the most suitable temperature and time according to the characteristics of the resin. For example, when the resin layer on the substrate 10 is a photosensitive resin, the prebaking temperature and time are appropriately performed under the most suitable conditions according to the characteristics of the photosensitive resin.

[0102] (Step S3)

[0103] Next, a process of exposing the resin (e.g., photosensitive resin) coated on the substrate 10 is performed. Specifically, a flow path pattern is drawn on the photosensitive resin coated on the substrate 10 by exposure. The exposure can be performed by, for example, an exposure device using ultraviolet rays as a light source, or a laser drawing device. For example, exposure using a proximity exposure or contact exposure device using ultraviolet rays as a light source is one of the preferred methods. In the case of a proximity exposure device, exposure is performed through a photomask having a flow path pattern arrangement in the microfluidic chip 1. The photomask may be a photomask having a two-layer structure of chromium and chromium oxide as a light-shielding film.

[0104] As described above, the base material layer 11 uses a photosensitive resin that is sensitive to light with a wavelength of 190 nm to 400 nm in the ultraviolet region. Therefore, in this step (exposure step), the photosensitive resin coated on the substrate 10 is sensitive to light with a wavelength of 190 nm to 400 nm.

[0105] When the photosensitive resin coated on the substrate 10 is a positive resist, the exposed area is dissolved to expose the substrate 10, and the photosensitive resin remaining in the unexposed area becomes the base layer 11. In addition, when the photosensitive resin coated on the substrate 10 is a negative resist, the photosensitive resin remaining in the exposed area becomes the base layer 11, and the unexposed area is dissolved to expose the substrate 10. Thus, the method for manufacturing the microfluidic chip 1 of the first embodiment can form the base layer 11 on the substrate 10 using photolithography.

[0106] (Step S4)

[0107] Next, a step of developing the exposed photosensitive resin to form a flow path pattern is performed.

[0108] The development is performed by a reaction between the photosensitive resin and the developer using a developing device such as spray, dip, or puddle. The developer can be, for example, an aqueous sodium carbonate solution, tetramethylammonium hydroxide, potassium hydroxide, an organic solvent, or the like. The developer can be the most suitable developer suitable for the characteristics of the photosensitive resin, but is not limited thereto. In addition, the concentration and the development treatment time can be appropriately adjusted to the most suitable conditions according to the characteristics of the photosensitive resin.

[0109] (Step S5)

[0110] Next, a step of removing the developer used for development from the resin layer (photosensitive resin layer) on the substrate 10 by washing is performed. Washing can be performed by a washing device such as a spray, shower, or immersion. As washing water, for example, the most suitable washing water for removing the developer used in the development process can be appropriately used from pure water, isopropyl alcohol, etc. After washing, drying is performed by a spin dryer, an IPA steam dryer, natural drying, etc.

[0111] (Step S6)

[0112] Next, a step of heat treatment (post-baking) is performed on the base material layer 11. The post-baking treatment removes residual moisture during development and washing. The post-baking treatment is performed using, for example, a hot plate, an oven, etc. In the case of insufficient drying in the washing process of the above-mentioned step S5, sometimes the developer and moisture during washing remain in the base material layer 11. In addition, sometimes the solvent that has not been removed by the pre-baking treatment also remains in the base material layer 11. By performing the post-baking treatment, they can be removed.

[0113] (Step S7)

[0114] Next, a step of applying a resin onto the base layer 11 is performed. Thus, a resin layer for forming the partition wall layer 12 is provided on the base layer 11. In the method for manufacturing the microfluidic chip 1 of the first embodiment, a resin layer (photosensitive resin layer) made of a photosensitive resin is formed on the base layer 11, for example.

[0115] The photosensitive resin layer on the base material layer 11 can be formed by, for example, applying a photosensitive resin to the base material layer 11. The application can be carried out by, for example, spin coating, spray coating, rod coating, etc., and spin coating is preferred from the viewpoint of film thickness controllability. The photosensitive resin in various forms such as liquid, solid, gel, and film can be applied to the base material layer 11. For example, forming the photosensitive resin layer by a liquid resist is one of the preferred methods.

[0116] The resin (eg, photosensitive resin) may be applied onto the base material layer 11 so that the thickness of the resin layer (eg, photosensitive resin layer), that is, the thickness of the partition wall layer 12, is within a range of 5 μm to 100 μm.

[0117] (Step S8)

[0118] After the photosensitive resin is formed on the base layer 11, a heat treatment (prebaking treatment) process is then performed for the purpose of removing the solvent contained in the resin (e.g., photosensitive resin) coated on the base layer 11. It should be noted that in the manufacturing method of the microfluidic chip 1 of the first embodiment, the prebaking process is not a necessary process, and it can be performed at the most suitable temperature and time according to the characteristics of the resin. For example, in the case where the resin layer on the base layer 11 is a photosensitive resin, the prebaking temperature and time are appropriately performed under the most suitable conditions according to the characteristics of the photosensitive resin.

[0119] (Step S9)

[0120] Next, a process of exposing the resin (e.g., photosensitive resin) coated on the base layer 11 is performed. Specifically, by exposure, a flow path pattern is drawn on the photosensitive resin coated on the base layer 11. The exposure can be performed by, for example, an exposure device using ultraviolet rays as a light source, or a laser drawing device. For example, exposure using a proximity exposure or contact exposure device using ultraviolet rays as a light source is one of the preferred methods. In the case of a proximity exposure device, exposure is performed through a photomask having a flow path pattern arrangement in the microfluidic chip 1. The photomask may be a photomask having a two-layer structure of chromium and chromium oxide as a light-shielding film.

[0121] As described above, the partition wall layer 12 uses a photosensitive resin that is sensitive to light with a wavelength of 190 nm to 400 nm in the ultraviolet region. Therefore, in this step (exposure step), the photosensitive resin coated on the base layer 11 is sensitized to light with a wavelength of 190 nm to 400 nm.

[0122] When the photosensitive resin coated on the base layer 11 is a positive resist, the exposed area is dissolved to form the flow path section 3, and the photosensitive resin remaining in the unexposed area is the partition wall layer 12. In addition, when the photosensitive resin coated on the base layer 11 is a negative resist, the photosensitive resin remaining in the exposed area is the partition wall layer 12, and the unexposed area is dissolved to form the flow path section 3. Thus, the manufacturing method of the microfluidic chip 1 of the first embodiment can form the partition wall layer 12 constituting the flow path section 3 on the base layer 11 using the photolithography method.

[0123] When the resin layer on the base layer 11 is formed using a chemically amplified resist or the like, a heat treatment (post-exposure bake: PEB) may be further performed after exposure in order to promote the catalytic reaction of the acid generated by exposure.

[0124] (Step S10)

[0125] Next, a step of developing the exposed photosensitive resin to form a flow path pattern is performed.

[0126] The development is performed by a reaction between the photosensitive resin and the developer using a developing device such as spray, dip, or puddle. The developer can be, for example, an aqueous sodium carbonate solution, tetramethylammonium hydroxide, potassium hydroxide, an organic solvent, or the like. The developer can be the most suitable developer suitable for the characteristics of the photosensitive resin, but is not limited thereto. In addition, the concentration and the development treatment time can be appropriately adjusted to the most suitable conditions according to the characteristics of the photosensitive resin.

[0127] (Step S11)

[0128] Next, a step of completely removing the developer used for development from the resin layer (photosensitive resin layer) on the base material layer 11 by washing is performed. Washing can be performed by a washing device such as spraying, showering, or dipping. As washing water, the most suitable washing water for removing the developer used for development treatment can be appropriately used from, for example, pure water, isopropyl alcohol, etc. After washing, drying is performed by a spin dryer, an IPA steam dryer, natural drying, etc.

[0129] (Step S12)

[0130] Next, a process of heating the partition wall layer 12 that forms the flow path pattern and the flow path portion 3 (post-baking) is performed. The residual moisture during development and washing is removed by the post-baking process. The post-baking process is performed using, for example, a hot plate, an oven, etc. Sometimes, the drying in the washing process of the above-mentioned step S11 is insufficient, or the developer or the moisture during washing remains in the partition wall layer 12. In addition, sometimes, the solvent that is not removed in the pre-baking process also remains in the partition wall layer 12. By performing the post-baking process, they can be removed.

[0131] (Step S13)

[0132] After the post-baking treatment, a process of surface modification treatment is performed on the partition wall layer 12 and the upper cover layer 13 (cover material) before being bonded to the partition wall layer 12. As an example of the surface modification treatment, UV treatment is performed. It should be noted that the surface modification treatment can be appropriately implemented as needed, and it is not a necessary process in the manufacturing method of the microfluidic chip 1 of the first embodiment.

[0133] (Step S14)

[0134] Next, a process of bonding the upper cover layer 13 to the partition wall layer 12 after the post-baking process is performed. Figure 1B to Figure 1D As shown, the upper cover layer 13 is bonded to the surface of the partition wall layer 12 on the opposite side from the substrate 10. Thus, the flow path section 3 is covered with the upper cover layer 13, and the micro-flow path chip 1 is formed.

[0135] As a method for bonding the substrates subjected to the surface modification treatment in step S13, for example, thermal compression bonding using a hot press or a hot roller can be used. However, when a flexible material such as PDMS is used as the cover material, bonding can be performed without applying pressure.

[0136] Preferably, holes corresponding to the fluid input part 2 and output parts 4 and 5 are provided in the upper cover layer 13 before being bonded to the partition wall layer 12. This can suppress the generation of garbage and pollution compared to the case where holes are opened after bonding to the partition wall layer 12.

[0137] When heating is performed, the conditions are preferably adjusted according to the properties of the materials. For example, the bonding can be performed using a heating means such as a hot plate at 40° C. or higher for 5 minutes or longer.

[0138] The method of joining the partition wall layer 12 and the upper cover layer 13 is not limited to the above-mentioned thermal compression bonding, and can also be implemented by a method using an adhesive or a method of performing circuit bonding by surface modification treatment of the bonding surface of the partition wall layer 12 and the upper cover layer 13 without using an adhesive.

[0139] When an adhesive is used for bonding, the adhesive can be determined based on affinity with the materials constituting the partition wall layer 12 and the upper cover layer 13. The adhesive is not particularly limited as long as it can bond the partition wall layer 12 to the upper cover layer 13. For example, as the adhesive in the first embodiment, an acrylic resin adhesive, a polyurethane resin adhesive, an epoxy resin adhesive, etc. can be used.

[0140] In addition, as a method of bonding by surface modification without using an adhesive, there are UV treatment, plasma treatment, corona discharge treatment, excimer laser treatment, etc. In this case, the reactivity of the surface of the partition wall layer 12 is improved, and the most suitable treatment method can be appropriately selected according to the affinity between the partition wall layer 12 and the upper cover layer 13 and the compatibility of bonding. It should be noted that in the case of bonding by surface modification, the bonding of the partition wall layer 12 and the upper cover layer 13 in the above step S13 can be performed.

[0141] Here, an example of coating a photosensitive resin on the substrate 10 and using photolithography to form the partition wall layer 12 for constituting the flow path portion 3 is described, but the present invention is not limited to this. The resin used to form the resin layer that becomes the partition wall layer 12 on the substrate 10 may also be, for example, silicone rubber (PDMS) or a synthetic resin (PMMA, PC, PS, PP, COP, COC, etc.). For example, when the partition wall layer 12 is formed using silicone rubber, a cast film of a flow path pattern may be formed using photolithography, and the cast film of the flow path pattern may be transferred to the silicone rubber to form the flow path pattern (the partition wall layer 12 constituting the flow path portion 3).

[0142] [Example of the first embodiment]

[0143] The following describes an example of the first embodiment in which a siloxane polymer-containing layer 14 is provided on the surface of at least one of the base layer 11, the partition wall layer 12, and the cap layer 13. Therefore, first, the siloxane polymer and the contact angle, which are important for achieving hydrophobicity, are described.

[0144] <Volatilization of silicone components by heating of PDMS>

[0145] Regarding the layer 14 containing the siloxane polymer, the source of the siloxane is discussed. It is known that siloxane is produced from common silicone products. The siloxane produced as an exhaust gas (hereinafter referred to as "exhaust gas") is a component that is easily volatile and easily adheres to a substrate or the like. The siloxane has the property of volatilizing in trace amounts even at room temperature, but the amount of exhaust gas of the volatile siloxane increases by heating, and the higher the heating temperature, the more components with a larger polymerization number volatilize. The present disclosure focuses on the hydrophobicization brought about by the deposition of such low molecular weight siloxanes on the surface of the substrate. Depending on the material of PDMS, low molecular weight siloxane polymers such as cyclic siloxanes D3 to D20 and chain siloxanes M2 to M20 will volatilize. From the implementation of the examples of the first embodiment, it is important to confirm in advance the temperature dependence of the low molecular weight siloxane volatilized from PDMS.

[0146] <Measurement method of low molecular weight siloxane>

[0147] The determination of low molecular weight siloxane volatilized from PDMS and low molecular weight siloxane deposited on the substrate surface preferably uses thermal extraction gas chromatography-mass spectrometry (GC / MS). GC / MS is a composite device that combines a gas chromatograph (GC) that separates the vaporized mixture into a single component and a mass spectrometer (MS) that performs qualitative-quantitative analysis by ionizing the separated components and obtaining a mass spectrum, and is a preferred device for the quantitative analysis of low molecular weight siloxane. By changing the heating temperature during analysis, the temperature dependence of the volatile siloxane component can be determined. The quantitative method is that, for cyclic siloxanes, the relative standard concentration using decamethylcyclopentasiloxane (D5) as a standard substance is calculated. For chain siloxanes, the relative standard concentration using octamethyltrisiloxane (M3) as a standard substance is calculated.

[0148] <Contact angle change during the microfluidic chip manufacturing process>

[0149] As an example of an indicator indicating whether a specific layer is hydrophobic or hydrophilic, there is a contact angle. The change in the contact angle of the layer during the process of the manufacturing method of the above-mentioned microfluidic chip is described. Generally, the contact angle varies due to the contact angle (set to θ1) in the process of forming the partition wall layer 12 for forming the flow path portion 3 (step S102), the contact angle (set to θ2) after the process (step S13) of surface modification treatment of the upper cover layer 13 (cover material) before bonding with the partition wall layer 12, and the contact angle (set to θ3) after the process (step S14) of bonding the upper cover layer 13 to the partition wall layer 12. θ1 represents the contact angle of the raw material itself. Therefore, from the viewpoint of suppressing the backflow of droplets, it is preferred to use a material with a high contact angle. Next, in step S13, hydrophilic groups (-C=O, -OH, -COOH) are formed on the surface by oxygen radicals (O·) and hydroxyl radicals (HO·) generated by the surface modification treatment. Therefore, the surface of the raw material is hydrophilized, and the contact angle of θ2 becomes smaller (θ1>θ2). There is an effect that the higher the irradiation energy or the longer the irradiation time, the smaller the contact angle becomes (hydrophilicity is improved). Then, due to the heat treatment during bonding in step S14, the low molecular weight siloxane volatilized from PDMS is deposited on the surface of the raw material and is hydrophobicized, and the contact angle of θ3 becomes larger (θ2<θ3). There is an effect that the higher the temperature of the heating conditions and the longer the treatment time, the more the amount of low molecular weight siloxane deposited on the surface increases, and the larger the contact angle becomes (hydrophobicity is improved). After in-depth research, the present inventors have found that by controlling the surface modification treatment conditions in step S13, and the heating conditions (temperature, time) in the above-mentioned step S14, or the heating conditions (temperature, time) using a heating furnace described later, the contact angle of the raw material surface in the flow path of the microfluidic chip can be arbitrarily controlled. It is recognized that the control of the heating conditions of step S14 is particularly important. The present disclosure achieves arbitrary control of the contact angle through the heating conditions of PDMS.

[0150] <Contact angle measurement method>

[0151] The contact angle is measured by filling a syringe with water and attaching it to the contact angle meter. Set parameters such as the waiting time [msec] until measurement, the measurement interval [msec], and the number of consecutive measurements [times]. Water is dripped from the syringe onto the sample surface, and an image is taken to measure the contact angle of the droplet. The static contact angle is measured using the droplet method. The droplet method is a method that uses the assumption that the droplet is a part of a sphere and calculates the contact angle θ based on the radius r and height h of the droplet after it is dropped.

[0152] The amount of liquid used in the usual contact angle measurement is usually 1 to 2 μL, but at this amount of liquid, droplets with a diameter of more than 1 mm are formed on the solid surface. The measurement area in the microfluidic chip is mostly a tiny area at the level of several microns. It is preferred to use a device that can drip picoliter droplets and evaluate the wetting behavior of the tiny area instead of a usual contact angle meter. For example, a piezoelectric titration device is used to generate droplets of picoliter units, and tiny droplets can be measured by using a high-magnification camera with an objective lens. In addition, since tiny droplets evaporate very quickly, it is more preferred to use a high-speed camera.

[0153] Next, main combinations and formation methods of the first photosensitive resin forming the base layer 11 and the second photosensitive resin forming the partition wall layer 12 used in the examples are described.

[0154] <Combination 1>

[0155] An example of a combination of a first photosensitive resin and a second photosensitive resin is shown in Table 1. The composition (ingredient) of the first photosensitive resin used as the base layer 11 includes polysiloxane and an acrylic monomer. The contact angle θ1 of the first photosensitive resin is 100°. The composition (ingredient) of the second photosensitive resin used as the partition wall layer 12 includes polysiloxane and an acrylic monomer. The contact angle θ1 of the second photosensitive resin is 100°.

[0156] The formation of the base material layer 11 (step S101) is described. When the first photosensitive resin is applied to the substrate 10 (step S1), spin coating is performed, and the coating speed of the wafer during coating is set to 700 rpm, and the coating is performed for 10 seconds. The pre-baking treatment (step S2) is to heat the wafer to 90°C and perform the treatment for 60 seconds. The exposure amount of the exposure of the pattern of the base material layer 11 (step S3) is set to 70mJ / cm 2 The developing solution for developing the pattern of the base material layer 11 (step S4) is a sodium carbonate aqueous solution, and the developing time is set to 90 seconds. The pattern of the base material layer 11 is washed with water for 60 seconds (step S5). The post-baking treatment (step S6) is performed at 230°C for 30 minutes.

[0157] The formation of the partition wall layer 12 (step S102) is described. When the second photosensitive resin is applied to the base layer 11 (step S7), spin coating is performed with the coating rotation angle set to 500 rpm for 10 seconds. The pre-baking treatment (step S8) is performed at 130°C for 180 seconds. The exposure amount of the flow path pattern exposure (step S9) is set to 60 mJ / cm 2 The developer for developing the flow path pattern (step 10) was a sodium carbonate aqueous solution, the development time was set to 180 seconds, and the washing was performed for 60 seconds. The washing of the flow path pattern (step S11) was performed for 60 seconds. The post-baking treatment (step S12) was performed at 230°C for 30 minutes.

[0158] Table 1

[0159]

[0160] <Combination 2>

[0161] An example of another combination of the first photosensitive resin and the second photosensitive resin is shown in Table 2. The composition (ingredients) of the first photosensitive resin used as the base layer 11 includes an acrylic resin and an epoxy resin. The contact angle θ1 of the first photosensitive resin is 60°. The composition (ingredients) of the second photosensitive resin used as the partition wall layer 12 includes polysiloxane and an acrylic monomer. The contact angle of the second photosensitive resin is 100°.

[0162] The conditions for forming the base material layer 11 (step S101 ) and the conditions for forming the partition wall layer 12 (step S102 ) are the same as those in Table 1.

[0163] Table 2

[0164]

[0165] <Combination 3>

[0166] An example of another combination of the first photosensitive resin and the second photosensitive resin is shown in Table 3. The composition (ingredient) of the first photosensitive resin used as the base layer 11 includes polysiloxane and acrylic monomer. The contact angle θ1 of the first photosensitive resin is 100°. The composition (ingredient) of the second photosensitive resin used as the partition wall layer 12 includes acrylic resin and acrylic monomer. The contact angle θ1 of the second photosensitive resin is 70°.

[0167] The formation of the base material layer 11 (step S101) is described below. A first photosensitive resin ( Figure 2 In the case of step S1), the coating is carried out by spin coating, and the coating speed of the wafer is set to 1100 rpm for 30 seconds. Figure 2 Step S2) is to heat the wafer to 90°C for 90 seconds. The pattern of the substrate layer 11 is exposed ( Figure 2 The exposure amount in step S3) is set to 100 mJ / cm 2 . Development of the pattern of the substrate layer 11 ( Figure 2 Step S4) uses a sodium carbonate developer, and the developing time is set to 180 seconds. Washing of the pattern of the substrate layer 11 ( Figure 2 Step S5) is washed with water for 60 seconds. Post-baking treatment ( Figure 2 Step S6) is performed at 230°C for 30 minutes.

[0168] The conditions for forming the partition wall layer 12 (step S102 ) are the same as those in Table 1.

[0169] Table 3

[0170]

[0171] <Combination 4>

[0172] An example of another combination of the first photosensitive resin and the second photosensitive resin is shown in Table 4. The composition (ingredients) of the first photosensitive resin used as the base layer 11 includes an acrylic resin and an epoxy resin. The contact angle θ1 of the first photosensitive resin is 60°. The composition (ingredients) of the second photosensitive resin used as the partition wall layer 12 includes an acrylic resin and an acrylic monomer. The contact angle θ1 of the second photosensitive resin is 70°.

[0173] The conditions for forming the base material layer 11 (step S101 ) and the conditions for forming the partition wall layer 12 (step S102 ) are the same as those in Table 1.

[0174] Table 4

[0175]

[0176] (Example 1)

[0177] In Example 1, the micro-channel chip was fabricated using the first photosensitive resin in Table 1 as the base layer and PDMS as the member corresponding to the partition layer and the upper cover layer.

[0178] Figure 3A is a flow chart showing the manufacturing method of Example 1. In which, the step S101a of forming the base material layer corresponds to Figure 2 Step S101. Figure 2 The compositions and steps of the present invention may sometimes simplify or omit compositions and steps having the same corresponding relationship.

[0179] Step S102a is different from step S102 in that the partition wall layer and the upper cover layer are integrally formed by a mold. First, 100 g of two-component potting liquid silicone rubber TSE3032 (A) and 10 g of two-component potting liquid silicone rubber TSE3032 (B) (both manufactured by MOMENTIVE) are measured and stirred at 500 rpm for 15 minutes using a stirrer. After that, the silicone rubber is poured into the mold with the flow path pattern cut out, and heated in an oven at 150°C for 30 minutes to cure.

[0180] In step 13a, the bonding surface of the substrate layer and the bonding surface of the molded part formed by the mold are irradiated with UV. The UV irradiation dose is 1000mJ / cm 2It should be noted that after UV irradiation, it was confirmed that the contact angle θ2 of the base material layer decreased to 30°, and the contact angle θ2 of PDMS serving as both the partition wall layer and the cover material decreased to 60°.

[0181] In step S14a, the upper cover layer integrally formed with the partition wall layer is bonded to the substrate side as a cover material (hereinafter referred to as "cover material also serving as a partition wall layer") 1213, which is different from step S14. In step S14a, the cover material also serving as a partition wall layer 1213 is bonded by heating at 200°C for 10 minutes on a hot plate with the bonding surfaces bonded to each other.

[0182] Figure 3B The microfluidic chip manufactured in Example 1 is Figure 1B The AA section view corresponds to the cross-sectional view. In addition, Figure 3C The microfluidic chip manufactured in Example 1 is Figure 1D It should be noted that for Figure 1C The cross-sectional view corresponding to the BB cross-sectional view of Figure 3B The structure is the same as that of , so it is omitted.

[0183] A base material layer 11a is formed on the surface of the substrate 10a. The cover material 1213, which also serves as a partition wall layer, is bonded to the base material layer 11a in a manner that surrounds the flow path portion 3. It should be noted that, by GC / MS analysis (gas chromatography-mass spectrometry), it was confirmed that a layer 14a containing a siloxane polymer was formed on the surface of the cover material 1213, which also serves as a partition wall layer, and the surface of the base material layer 11a. The contact angle θ3 of the base material layer 11a is 90°, and the contact angle θ3 of the cover material 1213, which also serves as a partition wall layer, is 90°.

[0184] It is to be noted that GC / MS analysis confirmed that the siloxane polymer-containing layer 14a formed on either the base layer 11a or the cover material 1213 also serving as a partition layer contained D3 to D20 of the siloxane polymer (see Table 6 described below).

[0185] also, Figure 3C The following shows a state where the reaction evaluation between the reagent 15 and the test solution 16 is performed. Figure 3C In the process, reagent 15 is added from outlet 4 in advance, test liquid 16 is injected from inlet 2, and the test liquid is pushed to the vicinity of the outlet by air.

[0186] After this state, the microfluidic chip was placed in an incubator at a temperature of 50°C and a humidity of 80% for 1 hour in order to promote the reaction between the reagent 15 and the test solution 16. After 1 hour, the microfluidic chip was taken out for observation, and the droplets remained in the state near the outlet, and the droplets did not flow back to the branching part 18 of the flow path.

[0187] As can be seen from the above, it is possible to evaluate the reaction between the test solution and two reagents without contaminating the reaction solutions that react with the respective reagents.

[0188] (Example 2)

[0189] In Example 2, the first photosensitive resin and the second photosensitive resin shown in Table 1 were used for the base layer and the partition wall layer. PDMS was used for the cover layer. A microfluidic chip was prepared under the same conditions as in Example 1 except for the above.

[0190] Figure 4A It is a flowchart showing the manufacturing method of Example 2.

[0191] In step 13b, it was confirmed that the contact angle θ2 of the base layer decreased to 30° after UV irradiation, and the contact angle θ2 of the partition wall layer decreased to 40°.

[0192] In step S14b, the bonding surfaces are heated at 200°C for 10 minutes using a hot plate in a state where they are bonded to each other, thereby bonding the upper cover layer.

[0193] Figure 4B The microfluidic chip manufactured in Example 2 is Figure 1B The AA section view corresponds to the cross-sectional view. In addition, Figure 4C The microfluidic chip manufactured in Example 2 is Figure 1D It should be noted that for Figure 1C The cross-sectional view corresponding to the BB cross-sectional view of Figure 4B The structure is the same as that of , so it is omitted.

[0194] A base layer 11b is formed on the surface of the substrate 10b. The upper cover layer 13b that divides the flow path 3 by the partition wall layer 12b is bonded to the partition wall layer 12b in a manner that surrounds the flow path portion 3. It should be noted that GC / MS analysis (gas chromatography-mass spectrometry) confirmed that a layer 14b containing a siloxane polymer is formed on the surface of the base layer 11b, the partition wall layer 12b, and the upper cover layer 13b. The contact angle θ3 of the base layer 11b is 100°, the contact angle of the partition wall layer 12b is 90°, and the contact angle of the upper cover layer 13b is 130°.

[0195] It is to be noted that GC / MS analysis confirmed that the siloxane polymer-containing layer 14b formed on any of the base layer 11b, the partition wall layer 12b, and the cap layer 13b contained D3 to D20 of the siloxane polymer (see Table 6 described below).

[0196] also, Figure 4C The following shows a state where the reaction evaluation between the reagent 15 and the test solution 16 is performed. Figure 4CIn the process, the reagent 15 is added from the outlet 4 in advance, the test liquid 16 is injected from the inlet 2, and the test liquid 16 is pushed to the vicinity of the outlet by air.

[0197] After this state, the microfluidic chip was placed in an incubator at a temperature of 50°C and a humidity of 80% for 1 hour in order to promote the reaction between the reagent 15 and the test solution 16. After 1 hour, the microfluidic chip was taken out for observation, and the droplets remained in the state near the outlet, and the droplets did not flow back to the branching part 18 of the flow path.

[0198] As can be seen from the above, it is possible to evaluate the reaction between the test solution and two reagents without contaminating the reaction solutions that react with the respective reagents.

[0199] (Example 3)

[0200] In Example 3, the base material layer and the partition wall layer used the first photosensitive resin and the second photosensitive resin shown in Table 1. The cover layer used acrylic resin.

[0201] Figure 5A : is a flow chart showing the manufacturing method of Example 3. Example 3 includes a step of standing in a siloxane atmosphere (step S103c). A microchannel chip was manufactured under the same conditions as Example 1 except for the above.

[0202] In step 13c, it was confirmed that the contact angle θ2 of the base layer decreased to 30° after UV irradiation, and the contact angle θ2 of the partition wall layer decreased to 40°.

[0203] In step 103c, after the PDMS is heated to 200°C in a heating furnace and allowed to stand for 5 minutes, the substrate having the base material layer and the partition wall layer is allowed to stand in the heating furnace for 10 minutes. It should be noted that the standing time of the base material layer is not limited to this. For example, it can also be set to more than 5 minutes.

[0204] In step S14c, the bonding surfaces are heated at 200°C for 10 minutes using a hot plate in a state where they are bonded to each other, thereby bonding the upper cover layer.

[0205] Figure 5B The microfluidic chip manufactured in Example 3 is Figure 1B The AA section view corresponds to the cross-sectional view. In addition, Figure 5C The microfluidic chip manufactured in Example 3 is Figure 1D It should be noted that for Figure 1C The cross-sectional view corresponding to the BB cross-sectional view of Figure 5B The structure is the same as that of , so it is omitted.

[0206] A base layer 11c is formed on the surface of the substrate 10c. The upper cover layer 13c that divides the flow path portion 3 by the partition wall layer 12c is bonded to the partition wall layer 12c in a manner that surrounds the flow path portion 3. It should be noted that GC / MS analysis (gas chromatography-mass spectrometry) confirmed that a layer 14c containing a siloxane polymer is formed on the surface of the base layer 11c and the partition wall layer 12c. The contact angle θ3 of the base layer 11c is 110°, the contact angle θ3 of the partition wall layer 12c is 90°, and the contact angle θ3 of the upper cover layer 13c is 40°.

[0207] It was confirmed by GC / MS analysis that the siloxane polymer-containing layer 14c formed on either the base layer 11c or the partition wall layer 12c contained D3 to D20 of the siloxane polymer (see Table 6 described later).

[0208] also, Figure 5C The following shows a state where the reaction evaluation between the reagent 15 and the test solution 16 is performed. Figure 5C In the process, the reagent 15 is added from the outlet 4 in advance, the test liquid 16 is injected from the inlet 2, and the test liquid 16 is pushed to the vicinity of the outlet by air.

[0209] After this state, the microfluidic chip was placed in an incubator at a temperature of 50°C and a humidity of 80% for 1 hour in order to promote the reaction between the reagent 15 and the test solution 16. After 1 hour, the microfluidic chip was taken out for observation, and the droplets remained in the state near the outlet, and the droplets did not flow back to the branching part 18 of the flow path.

[0210] As can be seen from the above, it is possible to evaluate the reaction between the test solution and two reagents without contaminating the reaction solutions that react with the respective reagents.

[0211] (Example 4)

[0212] In Example 4, the first photosensitive resin and the second photosensitive resin shown in Table 2 were used as the base layer and the partition wall layer. PDMS was used as the cover layer. A microfluidic chip was prepared under the same conditions as in Example 1 except for the above.

[0213] Fig. 6A It is a flowchart showing the manufacturing method of Example 4.

[0214] Figure 6B The microfluidic chip manufactured in Example 4 is Figure 1B The AA section view corresponds to the cross-sectional view. In addition, Figure 6C The microfluidic chip manufactured in Example 4 is Figure 1D It should be noted that for Figure 1C The cross-sectional view corresponding to the BB cross-sectional view of Figure 6BThe structure is the same as that of , so it is omitted.

[0215] A base material layer 11d is formed on the surface of the substrate 10d. The upper cover layer 13d, which is divided into the flow path portion 3 by the partition wall layer 12d, is bonded to the partition wall layer 12b in a manner of surrounding the flow path portion 3. It should be noted that GC / MS analysis (gas chromatography-mass spectrometry) confirmed that a layer 14d containing a siloxane polymer is formed on the surface of the partition wall layer 12d and the upper cover layer 13d. The contact angle θ3 of the base material layer 11d is 60°, the contact angle of the partition wall layer 12d is 90°, and the contact angle of the upper cover layer 13d is 110°.

[0216] It is to be noted that GC / MS analysis confirmed that the siloxane polymer-containing layer 14d formed on either the partition wall layer 12d or the cap layer 13d contained D3 to D20 of the siloxane polymer (see Table 6 described later).

[0217] also, Figure 6C The following shows a state where the reaction evaluation between the reagent 15 and the test solution 16 is performed. Figure 8C In the process, the reagent 15 is added from the outlet 4 in advance, the test liquid 16 is injected from the inlet 2, and the test liquid 16 is pushed to the vicinity of the outlet by air.

[0218] After this state, the microfluidic chip was placed in an incubator at a temperature of 50°C and a humidity of 80% for 1 hour in order to promote the reaction between the reagent 15 and the test solution 16. After 1 hour, the microfluidic chip was taken out for observation, and the droplets remained in the state near the outlet, and the droplets did not flow back to the branching part 18 of the flow path.

[0219] As can be seen from the above, it is possible to evaluate the reaction between the test solution and two reagents without contaminating the reaction solutions that react with the respective reagents.

[0220] (Example 5)

[0221] In Example 5, the base layer and the partition wall layer used the first photosensitive resin and the second photosensitive resin shown in Table 3. The cover layer used PDMS.

[0222] Fig. 7A : is a flow chart showing the manufacturing method of Example 5. Example 5 includes a step of standing in a siloxane atmosphere (step S103e). A microchannel chip was manufactured under the same conditions as Example 1 except for the above.

[0223] In step 103e, after the PDMS is heated to 200°C in a heating furnace and allowed to stand for 5 minutes, the substrate with the base material layer formed thereon is allowed to stand in the heating furnace for 10 minutes.

[0224] Figure 7B The microfluidic chip manufactured in Example 5 is Figure 1B The cross-sectional view corresponding to the AA cross-sectional view. Figure 7B The microfluidic chip manufactured in Example 5 is Figure 1B The AA section view corresponds to the cross-sectional view. In addition, Figure 7C The microfluidic chip manufactured in Example 5 is Figure 1D It should be noted that for Figure 1C The cross-sectional view corresponding to the BB cross-sectional view of Figure 7B The structure is the same as that of , so it is omitted.

[0225] A base layer 11e is formed on the surface of the substrate 10e. The upper cover layer 13e, which defines the flow path 3 by the partition wall layer 12e, is bonded to the partition wall layer 12e in a manner that surrounds the flow path 3. It should be noted that GC / MS analysis (gas chromatography-mass spectrometry) confirmed that a layer 14e containing a siloxane polymer is formed on the surface of the base layer 11e and the upper cover layer 13e. The contact angle θ3 of the base layer 11e is 100°, the contact angle θ3 of the partition wall layer 12e is 70°, and the contact angle θ3 of the upper cover layer 13e is 110°.

[0226] It is to be noted that GC / MS analysis confirmed that the siloxane polymer-containing layer 14e formed on either the base layer 11e or the cap layer 13e contained D3 to D20 of the siloxane polymer (see Table 6 described later).

[0227] also, Figure 7C The following shows a state where the reaction evaluation between the reagent 15 and the test solution 16 is performed. Figure 7C In the process, the reagent 15 is added from the outlet 4 in advance, the test liquid 16 is injected from the inlet 2, and the test liquid 16 is pushed to the vicinity of the outlet by air.

[0228] After this state, the microfluidic chip was placed in an incubator at a temperature of 50°C and a humidity of 80% for 1 hour in order to promote the reaction between the reagent 15 and the test solution 16. After 1 hour, the microfluidic chip was taken out for observation, and the droplets remained in the state near the outlet, and the droplets did not flow back to the branching part 18 of the flow path.

[0229] As can be seen from the above, it is possible to evaluate the reaction between the test solution and two reagents without contaminating the reaction solutions that react with the respective reagents.

[0230] (Example 6)

[0231] In Example 6, the base material layer and the partition wall layer used the first photosensitive resin and the second photosensitive resin shown in Table 3. The cover layer used acrylic resin.

[0232] Fig. 8AFlow chart showing the manufacturing method of Example 6. Example 6 includes a step of standing in a siloxane atmosphere (step S103f). In addition, for the bonding of the upper cover layer (step S14f), the heating conditions using a hot plate are set to 50°C and 10 minutes. In addition, the microfluidic chip is manufactured under the same conditions as Example 1.

[0233] In step 103f, after the PDMS is heated to 200°C in a heating furnace and allowed to stand for 5 minutes, the substrate with the base material layer formed thereon is allowed to stand in the heating furnace for 10 minutes.

[0234] Figure 8B The microfluidic chip manufactured in Example 6 is Figure 1B The AA section view corresponds to the cross-sectional view. In addition, Figure 8C The microfluidic chip manufactured in Example 6 is Figure 1D It should be noted that for Figure 1C The cross-sectional view corresponding to the BB cross-sectional view of Figure 8B The structure is the same as that of , so it is omitted.

[0235] A base material layer 11f is formed on the surface of the substrate 10f. The upper cover layer 13f, which is divided into the flow path portion 3 by the partition wall layer 12f, is bonded to the partition wall layer 12f in a manner of surrounding the flow path portion 3. It should be noted that a layer 14f containing a siloxane polymer is formed on the surface of the base material layer 11f by GC / MS analysis (gas chromatography-mass spectrometry). The contact angle θ3 of the base material layer 11f is 100°, the contact angle θ3 of the partition wall layer 12f is 70°, and the contact angle θ3 of the upper cover layer 13f is 40°.

[0236] It was confirmed by GC / MS analysis that the siloxane polymer-containing layer 14f formed on the base material layer 11f contained siloxane polymers D3 to D20 (see Table 6 described later).

[0237] also, Figure 8C The following shows a state where the reaction evaluation between the reagent 15 and the test solution 16 is performed. Figure 8C In the process, reagent 15 is added from outlet 4 in advance, test liquid is injected from inlet 2, and the test liquid is pushed to the vicinity of the outlet by air.

[0238] After this state, the microfluidic chip was placed in an incubator at a temperature of 50°C and a humidity of 80% for 1 hour in order to promote the reaction between the reagent 15 and the test solution 16. After 1 hour, the microfluidic chip was taken out for observation, and the droplets remained in the state near the outlet, and the droplets did not flow back to the branching part 18 of the flow path.

[0239] As can be seen from the above, it is possible to evaluate the reaction between the test solution and two reagents without contaminating the reaction solutions that react with the respective reagents.

[0240] (Example 7)

[0241] In Example 7, the base material layer and the partition wall layer used the first photosensitive resin and the second photosensitive resin shown in Table 2. The cover layer used acrylic resin.

[0242] Fig. 9A Flow chart showing the manufacturing method of Example 7. Example 7 includes a step of standing in a siloxane atmosphere (step S103g). In addition, for the bonding of the upper cover layer (step S14g), the heating conditions using a hot plate are set to 50°C and 10 minutes. In addition, the microfluidic chip is manufactured under the same conditions as Example 1.

[0243] In step 103g, after the PDMS is heated to 200°C in a heating furnace and allowed to stand for 5 minutes, the substrate on which the base material layer and the partition wall layer are formed is allowed to stand in the heating furnace for 10 minutes.

[0244] Fig. 9B The flow path chip manufactured in Example 7 is Figure 1B The AA section view corresponds to the cross-sectional view. In addition, Fig. 9B The flow path chip manufactured in Example 7 is Figure 1D It should be noted that for Figure 1C The cross-sectional view corresponding to the BB cross-sectional view of Fig. 9B The structure is the same as that of , so it is omitted.

[0245] A base material layer 11g is formed on the surface of the substrate 10g. The upper cover layer 13g, which is divided into the flow path portion 3 by the partition wall layer 12g, is bonded to the partition wall layer 12g in a manner that surrounds the flow path portion 3. It should be noted that a layer 14g containing a siloxane polymer is formed on the surface of the partition wall layer 12g by GC / MS analysis (gas chromatography-mass spectrometry). The contact angle θ3 of the base material layer 11g is 60°, the contact angle θ3 of the partition wall layer 12g is 90°, and the contact angle θ3 of the upper cover layer 13g is 40°.

[0246] It was confirmed by GC / MS analysis that the siloxane polymer-containing layer 14g formed on the partition wall layer 12g contained siloxane polymers D3 to D20 (see Table 6 described later).

[0247] also, Fig. 9C 2 shows a state where the reaction evaluation between the reagent 15 and the test solution 16 is performed. Figure 8CIn the process, reagent 15 is added from outlet 4 in advance, test liquid is injected from inlet 2, and the test liquid is pushed to the vicinity of the outlet by air.

[0248] After this state, the microfluidic chip was placed in an incubator at a temperature of 50°C and a humidity of 80% for 1 hour in order to promote the reaction between the reagent 15 and the test solution 16. After 1 hour, the microfluidic chip was taken out for observation, and the droplets remained in the state near the outlet, and the droplets did not flow back to the branching part 18 of the flow path.

[0249] As can be seen from the above, it is possible to evaluate the reaction between the test solution and two reagents without contaminating the reaction solutions that react with the respective reagents.

[0250] (Example 8)

[0251] In Example 8, the base layer and the partition wall layer used the first photosensitive resin and the second photosensitive resin shown in Table 4. The cover layer used acrylic resin.

[0252] Fig. 10A Flow chart showing the manufacturing method of Example 8. Example 8 includes a step of standing in a siloxane atmosphere (step S103h). In addition, for the bonding of the upper cover layer (step S14h), the heating conditions using a hot plate are set to 80°C and 10 minutes. Otherwise, the microfluidic chip is manufactured under the same conditions as Example 1.

[0253] In step 103h, the PDMS is heated to 200°C in a heating furnace and allowed to stand for 5 minutes, and then the upper cover layer is allowed to stand for 10 minutes in the heating furnace.

[0254] Fig. 10B The microfluidic chip manufactured in Example 8 is Figure 1B The AA section view corresponds to the cross-sectional view. In addition, Fig. 10C The microfluidic chip manufactured in Example 8 is Figure 1D It should be noted that the cross-sectional view corresponding to the CC cross-sectional view of Figure 1C The cross-sectional view corresponding to the BB cross-sectional view is Fig. 10B The structure is the same as that of , so it is omitted.

[0255] A base material layer 11h is formed on the surface of the substrate 10h. The upper cover layer 13h, which is divided into the flow path portion 3 by the partition wall layer 12h, is bonded to the partition wall layer 12h in a manner of surrounding the flow path portion 3. It should be noted that a layer 14h containing a siloxane polymer is formed on the surface of the upper cover layer 13h by GC / MS analysis (gas chromatography-mass spectrometry). The contact angle θ3 of the base material layer 11h is 60°, the contact angle θ3 of the partition wall layer 12h is 70°, and the contact angle θ3 of the upper cover layer 13h is 90°.

[0256] It is to be noted that GC / MS analysis confirmed that the siloxane polymer-containing layer 14h formed on the upper cover layer 13h contained siloxane polymers D3 to D20 (see Table 6 described later).

[0257] also, Fig. 10C 2 shows a state where the reaction evaluation between the reagent 15 and the test solution 16 is performed. Figure 8C In the process, reagent 15 is added from outlet 4 in advance, test liquid is injected from inlet 2, and the test liquid is pushed to the vicinity of the outlet by air.

[0258] After this state, the microfluidic chip was placed in an incubator at a temperature of 50°C and a humidity of 80% for 1 hour in order to promote the reaction between the reagent 15 and the test solution 16. After 1 hour, the microfluidic chip was taken out for observation, and the droplets remained in the state near the outlet, and the droplets did not flow back to the branching part 18 of the flow path.

[0259] As can be seen from the above, it is possible to evaluate the reaction between the test solution and two reagents without contaminating the reaction solutions that react with the respective reagents.

[0260] (Example 9)

[0261] In Example 9, the base material layer and the partition wall layer used the first photosensitive resin and the second photosensitive resin shown in Table 4. Glass was used as the upper cover layer.

[0262] Fig.11A Flow chart showing the manufacturing method of Example 9. Example 9 includes a step of standing in a siloxane atmosphere (step S103i). In addition, for the bonding of the upper cover layer (step S14i), the heating conditions using a hot plate are set to 120°C and 10 minutes. In addition, the microfluidic chip is manufactured under the same conditions as Example 1.

[0263] In step 103i, the PDMS is heated to 200°C in a heating furnace and allowed to stand for 5 minutes, and then the upper cover layer is allowed to stand in the heating furnace for 10 minutes.

[0264] Fig. 11B The microfluidic chip manufactured in Example 9 is Figure 1B The AA section view corresponds to the cross-sectional view. In addition, Fig. 11C The microfluidic chip manufactured in Example 9 is Figure 1D It should be noted that for Figure 1C The cross-sectional view corresponding to the BB cross-sectional view of Fig. 11B The structure is the same as that of , so it is omitted.

[0265] A base material layer 11i is formed on the surface of the substrate 10i. The upper cover layer 13i, which is divided into the flow path portion 3 by the partition wall layer 12i, is bonded to the partition wall layer 12i in a manner of surrounding the flow path portion 3. It should be noted that GC / MS analysis (gas chromatography-mass spectrometry) confirmed that a layer 14i containing a siloxane polymer is formed on the surface of the partition wall layer 12i and the upper cover layer 13i. The contact angle θ3 of the base material layer 11i is 60°, the contact angle θ3 of the partition wall layer 12i is 70°, and the contact angle θ3 of the upper cover layer 13i is 100°.

[0266] It is to be noted that GC / MS analysis confirmed that the siloxane polymer-containing layer 14i formed on the upper cover layer 13i contained D3 to D20 of the siloxane polymers (see Table 6 described later).

[0267] also, Fig. 11C The following shows a state where the reaction evaluation between the reagent 15 and the test solution 16 is performed. Fig. 11C In the process, reagent 15 is added from outlet 4 in advance, test liquid is injected from inlet 2, and the test liquid is pushed to the vicinity of the outlet by air.

[0268] After this state, the microfluidic chip was placed in an incubator at a temperature of 50°C and a humidity of 80% for 1 hour in order to promote the reaction between the reagent 15 and the test solution 16. After 1 hour, the microfluidic chip was taken out for observation, and the droplets remained in the state near the outlet, and the droplets did not flow back to the branching part 18 of the flow path.

[0269] As can be seen from the above, it is possible to evaluate the reaction between the test solution and two reagents without contaminating the reaction solutions that react with the respective reagents.

[0270] (Comparative Example 1)

[0271] In Comparative Example 1, the first photosensitive resin and the second photosensitive resin shown in Table 4 were used for the base material layer and the partition wall layer. Acrylic resin was used for the upper cover layer.

[0272] Fig. 12A Flowchart showing the manufacturing method of Comparative Example 1. In Comparative Example 1, the heating conditions for the bonding of the upper cover layer (step S14j) using the hot plate were set to 80°C for 10 minutes. A microchannel chip was manufactured under the same conditions as in Example 1 except for the above. Fig. 12A The manufacturing method shown is made by Figure 2 The manufacturing method shown has the same process structure.

[0273] Fig. 12B The microfluidic chip manufactured in Comparative Example 1 is Figure 1B The AA section view corresponds to the cross-sectional view. In addition, Fig. 12C The microfluidic chip manufactured in Comparative Example 1 is Figure 1DIt should be noted that for Figure 1C The BB cross-sectional view corresponds to the cross-sectional view, because it is Fig. 12B The structure is the same as that of , so it is omitted.

[0274] A base layer 11j is formed on the surface of the substrate 10j. The upper cover layer 13j, which is divided into the flow path portion 3 by the partition wall layer 12j, is bonded to the partition wall layer 12j in a manner of surrounding the flow path portion 3. It should be noted that according to GC / MS analysis (gas chromatography-mass spectrometry), no layer 14j containing a siloxane polymer is formed on the surface of any of the base layer 11j, the partition wall layer 12j, and the upper cover layer 13j. The contact angle θ3 of the base layer 11j is 60°, the contact angle θ3 of the partition wall layer 12j is 70°, and the contact angle θ3 of the upper cover layer 13j is 40°.

[0275] also, Fig. 12C The following shows a state where the reaction evaluation between the reagent 15 and the test solution 16 is performed. Figure 8C In the process, reagent 15 is added from outlet 4 in advance, test liquid is injected from inlet 2, and the test liquid is pushed to the vicinity of the outlet by air.

[0276] After this state, the microfluidic chip was placed in an incubator at a temperature of 50°C and a humidity of 80% for 1 hour in order to promote the reaction between the reagent 15 and the test solution 16. After 1 hour, the microfluidic chip was taken out for observation, and it was confirmed that the droplets flowed back to the inlet, and the reaction solution reacting with each reagent was contaminated.

[0277] <Evaluation Results>

[0278] Table 5 shows the manufacturing conditions and evaluation results of Example 1 to Comparative Example 1. Table 5 shows the composition / ingredients of the materials of the substrate layer, the partition wall layer, and the upper cover layer, the objects placed in the siloxane gas atmosphere during the manufacturing process, the bonding conditions of the cover material, the contact angle (the contact angle θ3 after bonding of the upper cover layer), the detected polymer, the detected polymer, and the evaluation results. The evaluation method is the content described in each embodiment and comparative example. In addition, based on the observed results, the contamination between the branched reaction liquids in the microfluidic chip is evaluated using the two levels of "0" and "×" according to the following evaluation criteria.

[0279] <Evaluation Criteria>

[0280] ○: The reaction liquid remaining near the outlet 4 did not flow back to the branching portion 18 of the flow path, and no contamination between the reaction liquids occurred.

[0281] ×: The reaction liquid that stayed near the outlet 4 flowed back to the branching portion 18 of the flow path, and contamination between the reaction liquids occurred.

[0282] Table 5

[0283]

[0284] Table 6 shows the relationship between the type of siloxane polymer contained in the siloxane polymer-containing layer 14 and the heating conditions. The heating conditions indicate the temperature and time when the cover material is attached or when the siloxane is left standing in the siloxane atmosphere of the heating furnace. The n-mer low molecular weight siloxane polymer is abbreviated as Dn.

[0285] Table 6

[0286] Unit: ppm (w / w)

[0287]

[0288] In this way, when a siloxane polymer-containing layer (hydrophobic region) having a contact angle of 90 degrees or more and 130 degrees or less is formed on the surface of any component of the microfluidic chip, backflow of the reaction solution in the microfluidic chip is prevented, and contamination between the reaction solutions is prevented.

[0289] [Second embodiment]

[0290] <Basic structure of microfluidic chip>

[0291] In the second embodiment, two regions, hydrophobic and hydrophilic, are formed on the substrate layer of the microfluidic chip, which is fundamentally different from the first embodiment. The following description focuses on the structure different from the first embodiment, and the description of the same structure as the first embodiment is simplified or omitted.

[0292] Fig.13 The microfluidic chip 101 of the second embodiment Figure 1D The microfluidic chip 101 has a base material layer 11k formed on a substrate 10k from the input portion 2 to the branch portion 18. Furthermore, a base material layer 11k is provided from the branch portion 18 to the middle portion 19 toward the output portion 4, but no base material layer 11k is provided from the middle portion 19 to the output portion 4, and the substrate 10k is exposed. Fig.13 As shown, the siloxane polymer-containing layer 14k is formed on both the cap layer 13k and the base layer 11k, but the exposed area of ​​the substrate 10k exhibits hydrophilicity, while the area where the base layer 11k is formed exhibits hydrophobicity.

[0293] As described above, the micro-flow channel chip 101 of the second embodiment is characterized in that the base material layer 11 k on the substrate 10 k is patterned so that a hydrophilic region different from a hydrophobic region is provided in a region close to the output portion 4 .

[0294] [Modification of the Second Embodiment]

[0295] Fig.14 The micro-channel chip 101 of the modified example of the second embodiment Figure 1D The microfluidic chip 101 does not have a base material layer 111 from the input part 2 to the branch part 18 and from the branch part 18 to the middle part 19 toward the output part 4, and the substrate 101 is exposed. The base material layer 111 is provided from the middle part 19 to the output part 4, which is different from the second embodiment. Fig.14 As shown, a layer 141 containing a siloxane polymer is formed on either the upper cover layer 131 or the base layer 111, but the area where the base layer 111 is formed shows hydrophilicity. On the other hand, the area where the substrate 101 is exposed shows hydrophobicity. As described later, a silicon coating 211 is applied to the substrate 101. In this way, the microfluidic chip 101 of the modified example of the second embodiment is characterized in that a hydrophilic area different from a hydrophobic area is provided in an area close to the output portion 4 by patterning the base layer 111 on the substrate 101 to which the silicon coating 211 is applied.

[0296] <Manufacturing method>

[0297] The manufacturing method of the microfluidic chip 101 of the second embodiment or its modified example is the same as the manufacturing method of the first embodiment, but in the formation of the base material layer (step 101), a pattern corresponding to different types of regions of the hydrophobic region and the hydrophilic region is formed, which is different from the manufacturing method of the first embodiment. In the following description, the steps corresponding to the manufacturing method of the first embodiment are referred to as needed, and the same steps as the first embodiment are marked with the same reference numerals, and the description is simplified or omitted.

[0298] [Examples of the Second Embodiment or Its Modifications]

[0299] The micro-channel chip of the second embodiment or its modified example will be described using specific examples. It should be noted that the present invention is not limited to the following examples.

[0300] The first photosensitive resin used as the base layer and the second photosensitive resin used as the partition wall layer used in the embodiments are described. The first photosensitive resin in Table 7 contains polysiloxane and acrylic monomer, and the contact angle θ1 is 100°. The first photosensitive resin in Table 8 contains a silane coupling agent and an acrylic monomer, and the contact angle θ1 is 60°. The first photosensitive resin in Table 9 contains an acrylic polymer and an acrylic monomer, and the contact angle θ1 is 100°. The first photosensitive resin in Table 10 contains an acrylic resin and an epoxy resin, and the contact angle θ1 is 60°.

[0301] The second photosensitive resin is shown in Table 11, and contains an acrylic resin and an acrylic monomer, and has a contact angle θ1 of 70°.

[0302] Table 7

[0303]

[0304] Substrate A

[0305] Table 8

[0306]

[0307] Substrate B

[0308] Table 9

[0309]

[0310] Substrate C

[0311] Table 10

[0312]

[0313] Table 11

[0314]

[0315] (Example 10)

[0316] In Example 10 of the second embodiment, the first photosensitive resin in Table 7 was used as the base layer, and the second photosensitive resin in Table 11 was used as the partition wall layer. PDMS was used as the cover layer to produce a microchannel chip.

[0317] First, a transparent first photosensitive resin is coated on a glass substrate to form a base material layer (step S1). The first photosensitive resin is coated on the glass substrate at a rotation speed of 1100 rpm for 30 seconds using a spin coater. The rotation speed and time are adjusted so that the film thickness reaches 2 μm. Next, a heat treatment (pre-baking) is performed on a hot plate for the purpose of removing the residual solvent contained in the photosensitive resin (step S2). The pre-baking is performed at a temperature of 90° C. for 90 seconds.

[0318] Next, the photosensitive resin layer on the glass substrate is exposed (step S3). Specifically, the photosensitive resin is pattern-exposed in the microchannel through a photomask having a pattern for setting a hydrophobic area and a hydrophilic area. The photomask uses a two-layer structure of chromium and chromium oxide as a light-shielding film. A proximity exposure device is used for exposure. The exposure device uses a high-pressure mercury lamp as a light source, and the exposure wavelength is a broadband including g, h, and i lines. The exposure amount is set to 100mJ / cm 2 .

[0319] Next, the exposed photosensitive resin layer is developed to form a pattern (step S4). Specifically, the photosensitive resin layer is developed for 180 seconds using a sodium carbonate developer to dissolve the unexposed portion and form a pattern.

[0320] Next, the photosensitive resin layer on the substrate is washed with a shower of ultrapure water to remove the developer, and then dried with a spin dryer (step S5).

[0321] Next, the substrate is subjected to a heat treatment (post-baking) at 230° C. for 30 minutes in an oven (step S6 ). Thus, a pattern of the base material layer corresponding to the hydrophobic region and the hydrophilic region is formed on the substrate.

[0322] Next, a second photosensitive resin of a transparent body is coated on the substrate and the base material layer to form a partition wall layer. First, a second photosensitive resin is coated on the glass substrate and the base material layer with a spin coater at a rotation speed of 500 rpm for 10 seconds (step S7). The rotation speed and time are adjusted in such a way that the film thickness reaches 50 μm. Next, a heat treatment (pre-baking) is performed on a hot plate for the purpose of removing the residual solvent contained in the photosensitive resin (step S8). The pre-baking is performed at a temperature of 130°C for 180 seconds.

[0323] Next, the glass substrate and the photosensitive resin layer on the base layer are exposed (step S9). Specifically, the photosensitive resin is pattern-exposed through a photomask having a flow path pattern. The photomask uses a two-layer structure of chromium and chromium oxide as a light-shielding film. A proximity exposure device is used for exposure. The exposure device uses a high-pressure mercury lamp as a light source, and the exposure wavelength is a broadband including g, h, and i lines. The exposure amount is set to 60mJ / cm 2 .

[0324] Next, the exposed photosensitive resin layer is developed to form a flow path pattern (step S10 ). Specifically, the photosensitive resin layer is developed for 180 seconds using a sodium carbonate developer to dissolve the unexposed portion and pattern it.

[0325] Next, the photosensitive resin layer on the substrate is washed with a spray of ultrapure water to remove the developer, and then dried with a spin dryer (step S11).

[0326] Next, the substrate was heated (post-baked) at 230° C. for 30 minutes in an oven (step S12). Thus, a flow path portion (flow path pattern) defined by the partition wall layer was formed on the substrate. The minimum width of the opposing partition wall layers, i.e., the minimum width of the flow path, was set to 50 μm.

[0327] After the flow path pattern is formed, the cover material is attached to manufacture the microfluidic chip. The cover material uses PDMS, and before attaching, both the partition wall layer of the flow path pattern and the PDMS attaching surface are irradiated with UV (step S13). The UV irradiation dose is set to 1000mJ / cm 2 Thereafter, the lid material was bonded by heating the bonding surfaces at 200° C. for 10 minutes on a hot plate (step S14 ). Thus, the micro-channel chip 101 was obtained.

[0328] It was confirmed by GC / MS analysis that a siloxane polymer-containing layer containing the low-molecular siloxanes D3 to D20 was formed on both the surface of the bed material and the surface of the cover material at this time.

[0329] Furthermore, the contact angle inside the flow channel 3 in the micro-flow channel chip 101 of Example 10 was measured using a microtiter contact angle meter DSM100M (manufactured by KRUSS Corporation). Fig.13 The contact angle θ3 of the region (hydrophobic region) where the substrate layer 11k is formed is 110°, and the contact angle θ3 of the glass substrate region (hydrophilic region) where the substrate layer 11k is not formed is 70°, confirming that two types of hydrophobic regions and hydrophilic regions with different contact angles are formed. It should be noted that the contact angle of the partition wall layer is 70°, and the contact angle of the cover material is 110°.

[0330] It should be noted that at the time of forming the substrate layer 11k, the initial contact angle θ1 of the substrate layer 11k is 100°, and the contact angle θ1 of the glass substrate is 20°. The contact angle θ2 of the substrate layer 11k after surface modification is 60°, and the contact angle θ2 of the glass substrate is 5°.

[0331] (Example 11)

[0332] In Example 11 of the second embodiment, the first photosensitive resin in Table 7 was used as the base layer, and the second photosensitive resin in Table 11 was used as the partition wall layer. PDMS was used as the cover layer to produce a microchannel chip.

[0333] The heating conditions for the bonding of the upper cover layer in Example 11 (step S14) were set to 150°C for 5 minutes using a hot plate. A microchannel chip was produced under the same conditions as in Example 10 except for the above.

[0334] GC / MS analysis confirmed that a siloxane polymer-containing layer containing low molecular weight siloxanes D3 to D20 was formed on both the surface of the bed material and the surface of the cover material. Fig.13 The contact angle θ3 of the region where the primer layer 11 k is formed (hydrophobic region) is 100°, and the contact angle θ3 of the region of the glass substrate where the primer layer 11 k is not formed (hydrophilic region) is 20°.

[0335] It should be noted that at the time of forming the substrate layer 11k, the initial contact angle θ1 of the substrate layer 11k is 100°, the contact angle θ1 of the glass substrate is 20°, the contact angle θ2 of the substrate layer 11k after surface modification is 60°, and the contact angle θ2 of the glass substrate area is 5°.

[0336] (Example 12)

[0337] In Example 12 of the second embodiment, the first photosensitive resin in Table 8 was used for the base layer, and the second photosensitive resin in Table 11 was used for the partition wall layer. PDMS was used for the cover layer. A microfluidic chip was prepared under the same conditions as in Example 10 except for this.

[0338] GC / MS analysis confirmed that a siloxane polymer-containing layer containing low molecular weight siloxanes D3 to D20 was formed on both the surface of the bed material and the surface of the cover material. Fig.13 The contact angle θ3 of the region where the primer layer 11 k is formed (hydrophobic region) is 95°, and the contact angle θ3 of the region of the glass substrate where the primer layer 11 k is not formed (hydrophilic region) is 70°.

[0339] It should be noted that at the time of forming the substrate layer, the contact angle θ1 of the initial substrate layer 11k area is 60°, and the contact angle θ1 of the glass substrate area is 20°. The contact angle θ2 of the substrate layer 11k area after surface modification is 25°, and the contact angle θ2 of the glass substrate area is 5°.

[0340] (Example 13)

[0341] In Example 13 of the modification of the second embodiment, the base layer used the first photosensitive resin in Table 8, and the partition wall layer used the second photosensitive resin in Table 11. PDMS was used as the upper cover layer.

[0342] The glass substrate 101 used had a silicon coating 211 on its surface. In the bonding step (step S14) of the upper cover layer 131, the heating conditions using the hot plate were set to 100°C for 10 minutes. Other than this, the microchannel chip was produced under the same conditions as in Example 10.

[0343] GC / MS analysis confirmed that a siloxane polymer-containing layer containing low molecular weight siloxanes D4 to D10 was formed on both the surface of the bed material and the surface of the cover material. Fig.14 The contact angle θ3 of the glass substrate region where the base material layer 111 is not formed but the silicon coating layer 211 is formed (hydrophobic region) is 90°, and the contact angle θ3 of the region where the base material layer 111 is formed (hydrophilic region) is 55°.

[0344] It should be noted that at the time point of forming the substrate layer 111, the contact angle θ1 of the initial substrate layer 111 area is 20°, and the contact angle θ1 of the glass substrate area is 95°. The contact angle θ2 of the substrate layer 111 area after surface modification is 25°, and the contact angle θ2 of the glass substrate is 80°.

[0345] (Example 14)

[0346] In Example 14 of the second embodiment, the base layer used the first photosensitive resin in Table 7, and the partition layer used the second photosensitive resin in Table 11. The upper cover layer used PMMA. The contact angle θ1 of PMMA was 80°.

[0347] Example 14 includes a step of standing in a siloxane atmosphere. In addition, for the bonding of the upper cover layer 13k (step S14), the heating conditions using the hot plate are set to 40°C and 5 minutes. If PMMA is bonded under high temperature conditions, the warping of the substrate is significant, so the bonding is performed at low temperature for a short time. In addition, the microfluidic chip is manufactured under the same conditions as in Example 10.

[0348] In the step of standing in a siloxane atmosphere, PDMS was left standing in a heating furnace at 200° C. for 10 minutes. In the state in which the heating furnace was set to a low-molecular siloxane atmosphere, the glass substrate having the flow path pattern formed thereon was exposed to the low-molecular siloxane atmosphere.

[0349] GC / MS analysis confirmed that a siloxane polymer-containing layer containing low molecular weight siloxanes D4 to D20 was formed on both the surface of the bed material and the surface of the cover material. Fig.13 The contact angle θ3 of the region where the primer layer 11k is formed (hydrophobic region) is 110°, and the contact angle θ3 of the region of the glass substrate where the primer layer 11k is not formed (hydrophilic region) is 70°.

[0350] It should be noted that at the time point of forming the substrate layer 11k, the contact angle θ1 of the initial region of the substrate layer 11k is 100°, and the contact angle θ1 of the glass substrate is 20°. The contact angle θ2 of the region of the substrate layer 11k after surface modification is 60°, and the contact angle θ2 of the glass substrate is 5°.

[0351] (Example 15)

[0352] In Example 15 of the modification of the second embodiment, the base layer used the first photosensitive resin in Table 10, and the partition layer used the second photosensitive resin in Table 11. PDMS was used as the upper cover layer.

[0353] The glass substrate 101 used had a silicon coating 211 on its surface. In the upper cover layer bonding step (step S14), the heating conditions using the hot plate were set to 150° C. for 5 minutes. A microchannel chip was produced under the same conditions as in Example 10 except for the above.

[0354] Fig.14 The contact angle θ3 of the glass substrate area where the base material layer 111 is not formed but the silicon coating 211 is formed (hydrophobic area) is 95°, and the contact angle θ3 of the area where the base material layer 111 is formed (hydrophilic area) is 60°.

[0355] It should be noted that the contact angle θ1 of the initial region of the base material layer 111 at the time of forming the base material layer 111 was 60°.

[0356] (Comparative Example 2)

[0357] In Comparative Example 2, the base layer used the first photosensitive resin in Table 7, and the partition wall layer used the second photosensitive resin in Table 11. The upper cover layer used PDMS.

[0358] In Comparative Example 2, the microchannel chip was produced under the same conditions as in Example 10 except that the heating conditions using the hot plate in the upper cover layer bonding step (step S14) were set to 100°C for 10 minutes.

[0359] GC / MS analysis confirmed that at this time, a layer of siloxane polymer containing low molecular weight siloxanes D4 to D10 was formed on both the surface of the bed material and the surface of the cover material. In addition, the contact angle θ3 of the area where the base material layer was formed was 80°, and the contact angle θ3 of the glass substrate area where the base material layer was not formed was 55°.

[0360] It should be noted that for the substrate layer, the contact angle θ1 of the initial substrate layer area at the time of forming the substrate layer is 100°, the contact angle θ1 of the glass substrate is 20°, the contact angle θ2 of the substrate layer area after surface modification is 60°, and the contact angle θ2 of the glass substrate is 5°.

[0361] (Comparative Example 3)

[0362] In Comparative Example 3, the base layer used the first photosensitive resin in Table 8, and the partition wall layer used the second photosensitive resin in Table 11. The upper cover layer used PDMS.

[0363] In Comparative Example 3, the microchannel chip was produced under the same conditions as in Example 12 except that the heating conditions using the hot plate in the bonding step of the upper cover layer (step S14) were set to 100°C for 10 minutes.

[0364] GC / MS analysis confirmed that at this time, a layer of siloxane polymer containing low molecular weight siloxanes D4 to D10 was formed on both the surface of the bed material and the surface of the cover material. In addition, the contact angle θ3 of the area where the base material layer was formed was 70°, and the contact angle θ3 of the glass substrate area where the base material layer was not formed was 55°.

[0365] It should be noted that, for the substrate layer 11k, the contact angle θ1 of the initial region of the substrate layer 11k at the time of forming the substrate layer is 60°, the contact angle θ1 of the glass substrate is 20°, the contact angle θ2 of the region of the substrate layer 11k after surface modification is 25°, and the contact angle θ2 of the glass substrate is 5°.

[0366] (Comparative Example 4)

[0367] In Comparative Example 4, the base layer used the first photosensitive resin in Table 7, and the partition wall layer used the second photosensitive resin in Table 11. The upper cover layer used a synthetic resin containing PMMA.

[0368] Comparative Example 4 includes a step of standing still in a siloxane atmosphere. A microchannel chip was prepared under the same conditions as in Example 14 except for the above.

[0369] In the step of standing in a siloxane atmosphere, PDMS was left standing in a heating furnace at 100° C. for 10 minutes, and the glass substrate having the flow path pattern formed thereon was exposed to the low molecular weight siloxane atmosphere in the heating furnace.

[0370] GC / MS analysis confirmed that at this time, a layer of siloxane polymer containing low molecular weight siloxanes D4 to D10 was formed on both the surface of the bed material and the surface of the cover material. In addition, the contact angle θ3 of the area where the base material layer was formed was 80°, and the contact angle θ3 of the glass substrate area where the base material layer was not formed was 55°.

[0371] It should be noted that the contact angle θ1 of the initial substrate layer area at the time of forming the substrate layer is 100°, the contact angle θ1 of the glass substrate is 20°, the contact angle θ2 of the substrate layer area after surface modification is 60°, and the contact angle θ2 of the glass substrate is 5°.

[0372] <Evaluation Results>

[0373] For the microfluidic chips of Examples 10 to 15 and Comparative Examples 2 to 4, the same evaluation method as in the first embodiment was used. The reagent was added from the outlet 4 of the flow path in advance, the test liquid was injected from the inlet 2, and the test liquid was pushed to the vicinity of the outlet 4 by air. Then, in order to promote the reaction between the test liquid and the reagent, the microfluidic chip was placed in an incubator at a temperature of 50°C and a humidity of 80% and left for 1 hour. After 1 hour, the microfluidic chip was taken out and observed. Table 12 shows the manufacturing conditions and evaluation results of Examples 10 to Comparative Example 4.

[0374] Table 12

[0375]

[0376] As shown in Table 12, it was confirmed that the contact angle decreased after UV irradiation, and that a layer containing low molecular weight siloxane was formed on the surface after PDMS was fired in the bonding step of the upper cover layer, so that the contact angle increased.

[0377] The results of contamination of the microfluidic chips of Examples 10 to 15 were all qualified ("0"). That is, in the microfluidic chips of Examples 10 to 15, the reaction solution remained in a state near the outlet, and the reaction solution did not flow back to the branching portion 18 of the flow path. Therefore, the reaction evaluation of the test solution and the two reagents was achieved without contamination between the reaction solutions.

[0378] On the other hand, the contamination results of the microfluidic chips of Comparative Examples 2 to 4 were all unqualified ("×"). The reaction solution could not remain in the state near the outlet, and the reaction solution flowed back to the branching part 18 of the flow path. Therefore, contamination between the reaction solutions occurred, and the reaction evaluation between the test solution and the two reagents could not be carried out.

[0379] Among them, Comparative Examples 2, 3, and 4 are cases where the bonding or heating conditions in the heating furnace in Examples 10, 12, and 14 are respectively implemented at low temperatures. It can be considered that only the siloxane with a small polymerization number volatilizes in Comparative Examples 2 to 4, so that a sufficient hydrophobic effect is not obtained. Therefore, it can be considered that in the second embodiment, the higher the temperature of the sintering conditions of PDMS, the more preferred.

[0380] <Suppression of backflow of droplets>

[0381] In a microfluidic chip, the movement of droplets in the flow path is associated with the balance of the Laplace pressure of the liquid interface in the flow path. In the Laplace pressure, the surface energy of the solid surface, that is, the contact angle, which is the contact part with the liquid surface, is an important factor. Therefore, by suppressing the contact angle of the flow path surface, backflow can be prevented. In order to make the fluid flow smoothly, a material whose contact angle on the surface of the material is hydrophilic is usually used. In addition, in the case where the droplets are left in a specified place as disclosed in the present invention, a material whose contact angle on the surface of the material is hydrophobic is used. In the relationship between the droplets and the solid surface, the surface tension of the droplets has almost no effect on the solid surface with hydrophilicity. That is, the droplets are easy to adhere to the hydrophilic surface. On the other hand, the droplets are easy to act on the solid surface with hydrophobicity. That is, the droplets are difficult to adhere to the hydrophobic surface. If these properties are utilized, the droplets can be left on the hydrophilic surface. After in-depth research, the inventors found that by setting the contact angle of the hydrophobic area to more than 90 degrees and less than 130 degrees and setting the contact angle of the hydrophilic area to less than 90 degrees, the backflow of the droplets can be suppressed.

[0382] It should be noted that the microfluidic chip and the method for manufacturing the microfluidic chip of the present invention are not limited to the above-mentioned embodiments and examples, and various changes can be made within the scope of not impairing the characteristics of the invention.

[0383] Possibility of Industrial Application

[0384] The present invention can be preferably used as a microfluidic chip and a method for manufacturing a microfluidic chip that can prevent backflow of reaction solutions and contamination between reaction solutions in a microfluidic chip for research purposes, diagnosis, inspection, analysis, culture, etc., by setting hydrophobic areas and hydrophilic areas using materials that constitute the flow path.

[0385] In addition, since it is not necessary to provide a special process, the contact angle can be controlled in the process commonly performed in the production of a microchannel chip, such as UV irradiation and bonding, which also has the effect of improving the production efficiency.

[0386] Reference numerals

[0387] 1, 101: microfluidic chip, 2: input part, 3: flow path part, 3a: main flow path part, 3b, 3c: branch flow path part, 4, 5: output part, 10, 10a~10l: substrate, 11, 11a~11l: bottom material layer, 12, 12b~12l: partition wall layer, 13, 13b~13l: upper cover layer, 1213: cover material also serving as partition wall layer, 14, 14a~14l: layer containing silicone polymer, 15: reagent, 16: test solution, 18: branch part, 19: middle part, 211: silicon coating, 49: test solution, 50: reagent

Claims

1. A microfluidic chip, characterized in that: It has an input part for introducing a fluid, a flow path part through which the fluid flows, and an output part for discharging the fluid or a reagent fixing part for contacting the fluid with a reagent. The output part for discharging the fluid or the reagent fixing part for contacting the fluid with a reagent is collectively referred to as the "output part". The flow path portion has a region where the contact angle of the surface in contact with the fluid is greater than or equal to 90 degrees and less than or equal to 130 degrees, and this region is hereinafter referred to as a "hydrophobic region".

2. The microfluidic chip according to claim 1, characterized in that: The hydrophobic region is formed with a layer containing a silicone polymer.

3. The microfluidic chip according to claim 2, characterized in that: The flow path portion is surrounded by at least a base material layer, a partition wall layer and an upper cover layer on the substrate. The surface of at least one of the base layer, the partition wall layer, and the cap layer has the hydrophobic region.

4. The microfluidic chip according to claim 2, characterized in that: The surface of the flow path portion close to the output portion has a region close to the hydrophobic region and having a contact angle of less than 90 degrees with the surface in contact with the fluid. This region is hereinafter referred to as a "hydrophilic region".

5. The microfluidic chip according to claim 2, characterized in that: The flow path portion includes a main flow path portion communicating with the input portion and a plurality of branch flow paths branching from the main flow path portion toward the output portion.

6. The microfluidic chip according to claim 2, wherein: The siloxane polymer-containing layer contains at least any one of trimers to icosomers of the siloxane polymer.

7. The microfluidic chip according to claim 3, wherein: The upper cover layer is formed of PDMS.

8. The microfluidic chip according to claim 3, wherein: The upper cover layer is formed of any one of PET, PMMA, PC, COP, and glass.

9. The microfluidic chip according to claim 3, wherein: The base material layer and the partition wall layer are formed of a photosensitive resin.

10. The microfluidic chip according to claim 9, wherein: The photosensitive resin is photosensitivity to light with a wavelength of 190 nm to 400 nm.

11. A method for manufacturing a microfluidic chip, characterized in that: It contains: A first step of forming a base material layer on a substrate; A second step of forming a partition wall layer on the substrate and the base material layer; and a third step of bonding the upper cover layer to the partition wall layer, Wherein, a hydrophobic region is formed on the surface of at least one of the base material layer, the partition wall layer and the upper cover layer.

12. The method for manufacturing a microfluidic chip according to claim 11, characterized in that: A layer containing a silicone polymer is formed on the hydrophobic area.

13. The method for manufacturing a microfluidic chip according to claim 12, wherein: The upper cover layer is formed of PDMS, The third step is a step of heating the upper cover layer and the partition wall layer to bond them together.

14. The method for manufacturing a microfluidic chip according to claim 12, wherein: The base material layer is formed of a first photosensitive resin. The partition wall layer is formed of a second photosensitive resin, The first photosensitive resin or the second photosensitive resin contains polysiloxane or a silane coupling agent, The third step is a step of heating the upper cover layer and the partition wall layer to bond them together.

15. The method for manufacturing a microfluidic chip according to claim 12, wherein: The method further comprises, before the third step, a fourth step of placing a surface of any one of the substrate, the base material layer, the partition wall layer, and the cap layer in a low molecular weight siloxane atmosphere.

16. The method for manufacturing a microfluidic chip according to claim 15, wherein: In the fourth step, the low molecular weight siloxane atmosphere is formed by heating PDMS at 100° C. or higher for 5 minutes or more in a heating furnace.

17. The method for manufacturing a microfluidic chip according to claim 12, wherein: In the first step, the base material layer is formed into a pattern. The hydrophobic region is formed on one of the surface of the substrate where the primer layer is not formed and the surface of the primer layer, and the hydrophilic region is formed on the other surface.

18. The method for manufacturing a microfluidic chip according to claim 14, wherein: The first photosensitive resin and the second photosensitive resin are photosensitivity to light with a wavelength of 190 nm to 400 nm.