Solid electrolyte layer and all-solid-state secondary battery
By using a solid electrolyte layer composed of the first phase and the second phase with a γ-Li3PO4 type and Li4SiO4 type crystal structure in an all-solid secondary battery, a high ion conductive grain boundary layer is formed, and the ion conduction of the existing electrolyte layer is solved. The problem of low rate achieves higher ion conductivity.
Patent Information
- Application Number
- CN202380027197.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-17
- Filing Date
- 2023-03-17
- Publication Date
- 2024-11-12
AI Technical Summary
The solid electrolyte layer in existing all-solid secondary batteries has low ion conductivity, making it difficult to meet higher ion conductivity requirements.
A solid electrolyte layer consisting of the first phase and the second phase with a γ-Li3PO4 type and a Li4SiO4 type crystal structure is used to improve the ion conductivity of the electrolyte layer by forming a high ion conductive grain boundary layer during the sintering process.
The ion conductivity of the solid electrolyte layer is significantly improved, the ion conductivity of the all-solid secondary battery is enhanced, and the problem of low conductivity is solved.
Smart Images

Figure CN118946936A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a solid electrolyte layer and an all-solid secondary battery.
[0002] This application claims priority based on Tokugan Application No. 2022-042604 filed in Japan on March 17, 2022, and the contents are incorporated herein by reference. Background Art
[0003] In recent years, the rapid development of electronic technology has achieved the miniaturization, lightness, thinness and multifunctionality of portable electronic devices. As a result, for batteries that become the power source of electronic devices, there is a strong desire for miniaturization, lightness, thinness and improved reliability. Therefore, all-solid secondary batteries using solid electrolytes as electrolytes have attracted much attention. In the past, as solid electrolytes for all-solid secondary batteries, sulfide solid electrolytes and oxide solid electrolytes were mainly used.
[0004] Sulfide-based solid electrolytes have excellent plasticity, so by pressing powder, an interface between the solid electrolyte and the active material can be formed. However, sulfide-based solid electrolytes have safety issues because they produce hydrogen sulfide when reacting with water.
[0005] On the other hand, oxide solid electrolytes do not produce hydrogen sulfide due to reaction with water and are safe. However, for oxide solid electrolytes, in order to obtain high ionic conductivity, it is necessary to densify them, and therefore, it is necessary to sinter at high temperatures. However, in the sintering for forming a dense solid electrolyte layer, sometimes the oxide solid electrolyte reacts with the active material, thereby generating a reaction layer with low ionic conductivity at the interface of the oxide solid electrolyte and the active material.
[0006] LSPO (Li2PO4) is known as an oxide-based solid electrolyte that is relatively stable with respect to the active material even when sintered at high temperature for densification. 3+x Si x P 1-x O4) (see Non-Patent Document 1). However, LSPO has an ion conductivity as low as 1×10 -6 S / cm platform (see Non-Patent Document 2).
[0007] Prior art literature
[0008] Non-patent literature
[0009] Non-patent document 1: Solid State Ionics 283 (2015) 109-114
[0010] Non-patent document 2: Ionics 7 (2001) 469-473 Summary of the invention
[0011] Problems to be solved by the invention
[0012] Conventionally, various solid electrolytes have been used in all-solid secondary batteries. However, in all-solid secondary batteries, further improvement in ion conductivity is required, and a solid electrolyte layer with further excellent ion conductivity is required.
[0013] The present invention has been developed in view of the above-mentioned problems, and an object of the present invention is to provide a solid electrolyte layer having high ion conductivity and an all-solid secondary battery including the solid electrolyte layer.
[0014] Technical solutions to solve problems
[0015] In order to solve the above problems, the following technical solutions are provided.
[0016] [1] One embodiment of the present invention provides a solid electrolyte layer comprising:
[0017] A first phase region comprising a first solid electrolyte containing Li, Si, P and O and having a γ-Li3PO4 type crystal structure; and
[0018] The second phase region includes a second solid electrolyte containing Li, Si, P and O, having a composition different from that of the first solid electrolyte, and having a Li4SiO4 type crystal structure.
[0019] [2] The solid electrolyte layer according to [1], wherein the ratio of the volume of the first phase region to the volume of the second phase region is preferably 0.1 to 9.
[0020] [3] The solid electrolyte layer according to any one of [1] or [2], wherein the ratio of the number of Si atoms contained in the first phase region to the number of P atoms is preferably 0.1 or more and less than 1.5.
[0021] [4] The solid electrolyte layer according to any one of [1] to [3], wherein the ratio of the number of Si atoms contained in the second phase region to the number of P atoms is preferably 1.5 to 9.
[0022] [5] One embodiment of the present invention provides an all-solid secondary battery comprising: a solid electrolyte layer as described in any one of [1] to [4]; and a positive electrode layer and a negative electrode layer sandwiching the solid electrolyte layer.
[0023] Effects of the Invention
[0024] The solid electrolyte layer of the present invention has: a first phase region, which includes a first solid electrolyte, the first solid electrolyte contains Li, Si, P and O, and has a γ-Li3PO4 type crystal structure; and a second phase region, which includes a second solid electrolyte, the second solid electrolyte contains Li, Si, P and O, is composed of a composition different from that of the first solid electrolyte, and has a Li4SiO4 type crystal structure. Therefore, the solid electrolyte layer of the present invention has high ion conductivity.
[0025] Therefore, the all-solid secondary battery including the solid electrolyte layer of the present invention and the positive electrode layer and the negative electrode layer sandwiching the solid electrolyte layer has good ion conductivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic cross-sectional view showing the all-solid secondary battery according to the first embodiment.
[0027] Figure 2 Yes Figure 1 The schematic cross-sectional view showing an enlarged portion of the solid electrolyte layer 3 of the all-solid secondary battery 10 is shown. DETAILED DESCRIPTION
[0028] The present inventors have repeatedly conducted intensive studies focusing on the relationship between the crystal structure and ion conductivity in a solid electrolyte layer including an oxide-based solid electrolyte containing Li, Si, P, and O in order to solve the above-mentioned problems.
[0029] As a result, it was found that when the solid electrolyte layer has a first phase region and a second phase region, the ion conductivity is higher than that of the solid electrolyte layer composed of only the first phase region or only the second phase region, thereby conceiving the present invention. The first phase region includes a first solid electrolyte, which contains Li, Si, P and O and has a γ-Li3PO4 type crystal structure; the second phase region includes a second solid electrolyte, which contains Li, Si, P and O, is composed of a composition different from that of the first solid electrolyte, and has a Li4SiO4 type crystal structure.
[0030] In a solid electrolyte layer having the above-mentioned first phase region and the above-mentioned second phase region, the mechanism by which the ion conductivity becomes higher compared to a solid electrolyte layer composed only of the first phase region or only of the second phase region has not yet been determined, but it is estimated that this is because a grain boundary layer with high ion conductivity is generated at the interface between the first phase region and the second phase region with different crystal phases during the firing process in the manufacturing process of the all-solid secondary battery.
[0031] Hereinafter, the solid electrolyte layer and the all-solid secondary battery of the present embodiment will be described with reference to the accompanying drawings as appropriate. Figure 1 In the drawings used in the following description, in order to facilitate the understanding of the features of the present invention, the features are sometimes enlarged for convenience. Therefore, the dimensional ratios of the components are sometimes different from the actual ones. The materials, dimensions, etc. illustrated in the following description are examples, and the present invention is not limited to these, and can be appropriately changed and implemented within the scope of not changing its purpose.
[0032] [All-solid-state secondary battery]
[0033] Figure 1 1 is a schematic cross-sectional view of an all-solid secondary battery 10 according to the present embodiment. The all-solid secondary battery 10 has a stack 4, a first external terminal 5, and a second external terminal 6. The first external terminal 5 and the second external terminal 6 are formed of a conductive material. The first external terminal 5 and the second external terminal 6 are respectively connected to the opposite surfaces of the stack 4. The first external terminal 5 and the second external terminal 6 extend in a direction intersecting (orthogonal) with the stacking surface of the stack 4.
[0034] The laminate 4 includes a positive electrode layer 1, a negative electrode layer 2, and a solid electrolyte layer 3 sandwiched between the positive electrode layer 1 and the negative electrode layer 2. The laminate 4 is a sintered body formed by laminating the positive electrode layer 1 and the negative electrode layer 2 via the solid electrolyte layer 3 and sintering them. The number of layers of the positive electrode layer 1 and the negative electrode layer 2 contained in the laminate 4 may be one layer each, or may be two or more layers. Figure 1 As shown, the solid electrolyte layer 3 is not only between the positive electrode layer 1 and the negative electrode layer 2, but also between the positive electrode layer 1 and the second external terminal 6, and between the negative electrode layer 2 and the first external terminal 5. Figure 1 As shown, one end of the positive electrode layer 1 is connected to the first external terminal 5 , and one end of the negative electrode layer 2 is connected to the second external terminal 6 .
[0035] The all-solid secondary battery 10 is charged or discharged by transfer of ions between the positive electrode layer 1 and the negative electrode layer 2 via the solid electrolyte layer 3 .
[0036] [Solid electrolyte layer]
[0037] Solid electrolyte layer 3 is capable of moving ions by an electric field applied from the outside. The solid electrolyte forming solid electrolyte layer 3 is a substance (for example, particles) that is capable of moving ions by an electric field applied from the outside.
[0038] Figure 2 Yes Figure 1 FIG. 1 is a schematic cross-sectional view showing a part of the solid electrolyte layer 3 of the all-solid secondary battery 10 enlarged. Figure 2 As shown, the solid electrolyte layer 3 has a first phase region 31 and a second phase region 32 .
[0039] The first phase region 31 includes a first solid electrolyte, which contains Li, Si, P and O and has a γ-Li3PO4 type crystal structure. The first phase region 31 can also be composed of the first solid electrolyte. The second phase region 32 includes a second solid electrolyte, which contains Li, Si, P and O, is composed of a composition different from the above-mentioned first solid electrolyte, and has a Li4SiO4 type crystal structure. The second phase region 32 can also be composed of a second solid electrolyte. The solid electrolyte layer 3 is preferably composed only of the first phase region 31 and the second phase region 32.
[0040] In the solid electrolyte layer 3, a region other than the first phase region 31 and the second phase region 32 may be included within a range that does not impair the effect of the present invention. The region other than the first phase region 31 and the second phase region 32 may be, for example, a phase composed of a metal oxide having a composition and a crystal structure different from those of the first phase region 31 and the second phase region 32.
[0041] In the solid electrolyte layer 3, the first phase region 31 and the second phase region 32 may be uniformly distributed or unevenly distributed. In order to make the first phase region 31 and the second phase region 32 easily contact each other and increase the area of the interface between the first phase region 31 and the second phase region 32, it is preferred that they are distributed approximately uniformly. In addition, there is no particular limitation on the shape and size of the first phase region 31 and the second phase region 32. For example, Figure 2 As shown, it can also be in an amorphous granular form.
[0042] exist Figure 2 In the figure, reference numeral 33 indicates grain boundaries between the first phase region 31 and the second phase region 32, between the first phase regions 31, and between the second phase regions 32. The grain boundaries 33 between the first phase region 31 and the second phase region 32 in the grain boundaries 33 form grain boundary layers 33a having high ion conductivity.
[0043] Since the first phase region 31 of the first solid electrolyte having a γ-Li3PO4 type crystal structure and the second phase region 32 of the second solid electrolyte having a Li4SiO4 type crystal structure have different crystal phases, it is estimated that the grain boundary layer 33a is formed at the interface between the first phase region 31 and the second phase region 32. Therefore, in the case where the solid electrolyte layer has only one crystal phase, for example, in the case where the solid electrolyte layer is composed of only one of the first phase region 31 and the second phase region 32, a grain boundary layer with high ion conductivity is not formed. Therefore, compared with the solid electrolyte layer 3 of the present embodiment in which a plurality of crystal phases coexist, the ion conductivity of the solid electrolyte layer having only one crystal phase is small.
[0044] There is no particular limitation on the ratio of the volume of the first phase region 31 to the volume of the second phase region 32 contained in the solid electrolyte layer 3 (first phase region / second phase region), but it is preferably 0.1 to 9, more preferably 0.25 to 4, and further preferably 0.5 to 1.5. When the ratio of the volume of the first phase region 31 to the volume of the second phase region 32 is 0.1 to 9, the first phase region 31 and the second phase region 32 are easily in contact, so the area of the interface between the first phase region 31 and the second phase region 32 increases, and a large amount of grain boundary layers 33a with high ion conductivity are generated. Therefore, a solid electrolyte layer 3 with high ion conductivity is formed.
[0045] The first solid electrolyte may be composed only of Li, Si, P and O, or it may contain at least one element selected from Ti, Co, Ni and Mn within a range capable of maintaining a γ-Li3PO4 type crystal structure, depending on the characteristics required of the all-solid secondary battery 10.
[0046] In addition, the first phase region 31 not only contains the first solid electrolyte, but also may contain components such as sintering aids, active material materials forming the positive electrode layer 1 and / or the negative electrode layer 2 (at least one of the positive electrode layer 1 and the negative electrode layer 2) within the range that does not impair the effect of the present invention.
[0047] The ratio of the number of Si atoms contained in the first phase region 31 to the number of P atoms (Si / P) is preferably 0.1 or more and less than 1.5, and Si / P is further preferably 0.8 or more and 1.2 or less. If the ratio of the number of Si atoms contained in the first phase region 31 to the number of P atoms (Si / P) is 0.1 or more and less than 1.5, the first phase region 31 has a stable (strongly bonded and not easily damaged) γ-Li3PO4 type crystal structure, and therefore, a large number of grain boundary layers 33a with high ion conductivity are generated at the interface with the second phase region 32. Therefore, a solid electrolyte layer 3 with high ion conductivity can be formed.
[0048] The second solid electrolyte may be composed only of Li, Si, P and O, or it may contain at least one element selected from Ti, Co, Ni and Mn within a range capable of maintaining a Li4SiO4 type crystal structure, depending on the characteristics required of the all-solid secondary battery 10.
[0049] The second phase region 32 may contain not only the second solid electrolyte but also components derived from, for example, a sintering aid and active material forming the positive electrode layer 1 and / or the negative electrode layer 2 within a range not impairing the effects of the present invention.
[0050] The ratio of the number of Si atoms contained in the second phase region 32 to the number of P atoms (Si / P) is preferably 1.5 or more and 9 or less, and Si / P is further preferably 2 or more and 4 or less. If the ratio of the number of Si atoms contained in the second phase region 32 to the number of P atoms (Si / P) is 1.5 or more and 9 or less, the second phase region 32 has a stable Li4SiO4 type crystal structure, and therefore, a large number of grain boundary layers 33a with high ion conductivity are generated at the interface with the first phase region 31. Therefore, a solid electrolyte layer 3 with high ion conductivity is formed.
[0051] When the laminate 4 is a sintered body, the first solid electrolyte and the second solid electrolyte and the sintering aid may be used as the material of the solid electrolyte layer 3 for manufacturing reasons such as increased productivity and improved yield when forming the solid electrolyte layer 3. In this case, the solid electrolyte layer 3 may contain a sintering aid that is not removed and remains in the sintering step for manufacturing the laminate 4.
[0052] As the sintering aid, any known sintering aid can be used as long as it has a sinterability improving effect. Specifically, examples of the sintering aid include compounds containing lithium (Li), boron (B), zinc (Zn), bismuth (Bi), and the like.
[0053] [Positive electrode layer]
[0054] like Figure 1 As shown, the positive electrode layer 1 includes, for example, a positive electrode current collector 1A and a positive electrode active material layer 1B. Figure 1 As shown, the positive electrode active material layer 1B may be formed on both surfaces of the positive electrode current collector 1A, or may be formed on only one surface.
[0055] (Positive electrode collector)
[0056] The positive electrode current collector 1A has excellent electrical conductivity. The positive electrode current collector 1A is composed of, for example, a metal such as silver, palladium, gold, platinum, aluminum, copper, nickel, stainless steel, iron, or an alloy containing at least one of these metals. The positive electrode current collector 1A may also contain, for example, a positive electrode active material such as a lithium vanadium compound (LiV2O5, Li3V2(PO4)3, LiVOPO4).
[0057] (Positive Electrode Active Material Layer)
[0058] The positive electrode active material layer 1B contains a positive electrode active material. The positive electrode active material layer 1B may contain a conductive auxiliary agent and a solid electrolyte.
[0059] (Positive electrode active material)
[0060] The positive electrode active material is not particularly limited as long as it can reversibly release and absorb lithium ions, and remove and insert lithium ions. For example, a positive electrode active material used in a known lithium ion secondary battery can be used.
[0061] The positive electrode active material is preferably one or two or more selected from transition metal oxides and transition metal composite oxides, for example.
[0062] As the positive electrode active material, lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese spinel (LiMn2O4), and lithium nickel oxide (LiNiO2) can also be used. x Co y Mn z M a O2 (x+y+z+a=1, 0≤x≤1, 0≤y≤1, 0≤z≤1, 0≤a≤1, M represents one or more elements selected from Al, Mg, Nb, Ti, Cu, Zn, Cr) represented by a composite metal oxide, lithium titanate (Li4Ti5O 12 )wait.
[0063] As the positive electrode active material, a positive electrode active material that does not contain lithium can also be used. For the positive electrode active material that does not contain lithium, it can be used in the following manner: a negative electrode active material doped with metallic lithium and / or lithium ions (at least one of metallic lithium and lithium ions) is pre-configured in the negative electrode layer 2, and used from the start of discharge for the all-solid secondary battery 10. As the positive electrode active material that does not contain lithium, for example, metal oxides (MnO2, V2O5, etc.) can be cited.
[0064] (Conductive additive)
[0065] The conductive aid is not particularly limited as long as it is a material that improves the electron conductivity in the positive electrode active material layer 1B, and a known conductive aid can be used. For example, carbon materials such as graphite, carbon black, graphene, and carbon nanotubes, metals such as gold, platinum, silver, palladium, aluminum, copper, nickel, stainless steel, and iron, conductive oxides such as ITO (indium tin oxide), or mixtures thereof can be cited. The conductive aid can also be in various forms such as powders and fibers.
[0066] (Solid Electrolyte)
[0067] The solid electrolyte contained in the positive electrode active material layer 1B makes the ion conductivity in the positive electrode active material layer 1B good. As the solid electrolyte, one or a mixture of two or more known solid electrolytes can be used. As the solid electrolyte, the same solid electrolyte as the first solid electrolyte or the second solid electrolyte used in the above-mentioned solid electrolyte layer 3 can also be used.
[0068] [Negative electrode layer]
[0069] like Figure 1 As shown, the negative electrode layer 2 includes, for example, a negative electrode current collector 2A and a negative electrode active material layer 2B. Figure 1 As shown, the negative electrode active material layer 2B may be formed on both surfaces of the negative electrode current collector 2A, or may be formed on only one surface.
[0070] (Negative electrode current collector)
[0071] The structure of the negative electrode current collector 2A is the same as that of the positive electrode current collector 1A.
[0072] (Negative Electrode Active Material Layer)
[0073] The negative electrode active material layer 2B contains a negative electrode active material. The negative electrode active material layer 2B may contain a conductive auxiliary agent or a solid electrolyte.
[0074] (Negative electrode active material)
[0075] The negative electrode active material is a compound that can absorb and release ions. The negative electrode active material is a compound that exhibits a lower potential than the positive electrode active material. As the negative electrode active material, the same material as the positive electrode active material can be used. The negative electrode active material and the positive electrode active material used in the all-solid secondary battery 10 are determined in consideration of the potential of the negative electrode active material and the potential of the positive electrode active material.
[0076] (Conductive additive)
[0077] The conductive additive improves the electron conductivity of the negative electrode active material layer 2B. The conductive additive may be the same material as that of the positive electrode active material layer 1B.
[0078] (Solid Electrolyte)
[0079] The solid electrolyte contained in the negative electrode active material layer 2B makes the ion conduction in the negative electrode active material layer 2B good. As the solid electrolyte, one or a mixture of two or more known solid electrolytes can be used. As the solid electrolyte, the same solid electrolyte as the first solid electrolyte or the second solid electrolyte used in the above-mentioned solid electrolyte layer 3 can also be used.
[0080] [Method for manufacturing all-solid-state secondary battery]
[0081] Next, a method for manufacturing the all-solid secondary battery 10 of the present embodiment will be described.
[0082] First, the laminate 4 is produced. The laminate 4 can be produced, for example, by a simultaneous firing method or a sequential firing method, preferably by a simultaneous firing method. The simultaneous firing method is a method of producing the laminate 4 by stacking the materials forming each layer and then firing them all at once. The sequential firing method is a method of firing each layer each time it is formed. The simultaneous firing method can produce the laminate 4 by fewer operating steps than the sequential firing method. In addition, the laminate 4 produced by the simultaneous firing method is denser than the laminate 4 produced by the sequential firing method. Below, the case where the laminate 4 is produced by the simultaneous firing method is taken as an example to explain the method for producing the laminate 4.
[0083] First, the materials constituting the positive electrode collector 1A, the positive electrode active material layer 1B, the solid electrolyte layer 3, the negative electrode active material layer 2B, and the negative electrode collector 2A are paste-formed to prepare a paste corresponding to the material of each layer.
[0084] The paste of the solid electrolyte layer 3 is obtained, for example, by paste-forming a solid electrolyte material obtained by mixing particles consisting of a first solid electrolyte, particles consisting of a second solid electrolyte, and a sintering aid as required at a predetermined volume ratio.
[0085] There is no particular limitation on the method of making the various materials used to make the laminate 4 into a paste. For example, a method of mixing the powders of various materials into a carrier to obtain a paste can be adopted. Here, the carrier is a general term for a medium in a liquid phase. The carrier of this embodiment includes a solvent, a bonding material (adhesive), and a plasticizer.
[0086] Next, a green sheet is prepared. The green sheet is obtained by applying the paste prepared according to the respective materials on a substrate such as a PET (polyethylene terephthalate) film, drying as required, and then peeling off the substrate. There is no particular limitation on the method for applying the paste, and for example, a known method such as screen printing, coating, transfer, and a doctor blade method can be used.
[0087] Next, the green sheets made of the respective materials are stacked in the desired order and number of layers to produce a laminated sheet. When stacking the green sheets, alignment and cutting are performed as required. For example, in the case of manufacturing a parallel type or a series-parallel type battery, it is preferred to stack the green sheets by aligning them so that the end face of the positive electrode collector 1A and the end face of the negative electrode collector 2A do not coincide.
[0088] The green sheets that become the laminated sheets may be the positive electrode units and negative electrode units that have been manufactured in advance.
[0089] As the production order of the positive electrode unit, specifically, first, a paste for the solid electrolyte layer 3 is applied on a substrate such as a PET film by a doctor blade method and dried to form a sheet-like solid electrolyte layer 3. Next, a paste for the positive electrode active material layer 1B is printed on the solid electrolyte layer 3 by screen printing and dried to form the positive electrode active material layer 1B. Next, a paste for the positive electrode collector 1A is printed on the positive electrode active material layer 1B by screen printing and dried to form the positive electrode collector 1A. Next, a paste for the positive electrode active material layer 1B is printed on the positive electrode collector 1A by screen printing and dried to form the positive electrode active material layer 1B. Then, the positive electrode unit is obtained by peeling off the PET film. The positive electrode unit is a raw sheet in which the solid electrolyte layer 3, the positive electrode active material layer 1B, the positive electrode collector 1A, and the positive electrode active material layer 1B are stacked in sequence.
[0090] A negative electrode unit is produced in the same order. The negative electrode unit is a green sheet in which the solid electrolyte layer 3, the negative electrode active material layer 2B, the negative electrode collector 2A, and the negative electrode active material layer 2B are stacked in this order.
[0091] Next, the positive electrode unit and the negative electrode unit are stacked. At this time, the solid electrolyte layer 3 of the positive electrode unit and the negative electrode active material layer 2B of the negative electrode unit are stacked face to face. Alternatively, the positive electrode active material layer 1B of the positive electrode unit and the solid electrolyte layer 3 of the negative electrode unit are stacked face to face. Thus, a laminated sheet is obtained in which the positive electrode active material layer 1B, the positive electrode collector 1A, the positive electrode active material layer 1B, the solid electrolyte layer 3, the negative electrode active material layer 2B, the negative electrode collector 2A, the negative electrode active material layer 2B, and the solid electrolyte layer 3 are stacked in sequence. In addition, when the positive electrode unit and the negative electrode unit are stacked, the positive electrode collector 1A of the positive electrode unit and the negative electrode collector 2A of the negative electrode unit are stacked alternately.
[0092] Next, the laminated sheets are pressed together to improve the adhesion of each layer to form a laminated substrate. Pressing can be performed by, for example, a molding machine, a warm isostatic press (WIP), a cold isostatic press (CIP), an isostatic press, etc. Pressing is preferably performed while heating. The heating temperature during pressurization can be, for example, 40 to 95°C.
[0093] Next, the laminated substrate obtained after the pressurization is cut using a cutting device to obtain a laminated body. Then, the obtained laminated body is subjected to a binder removal and sintering step. Thus, a laminated body 4 composed of a sintered body is obtained.
[0094] The debinding and firing process can be performed by placing the laminate on a ceramic table, for example. The debinding and firing process is, for example, a process of heating to 550° C. to 1100° C. in an air atmosphere. The heating time (firing time) can be, for example, 0.1 hour to 6 hours. The heating temperature and firing time in the debinding and firing process can be appropriately determined according to the composition of each layer constituting the laminate 4, etc.
[0095] When the heating temperature in the debinding and sintering process is 550°C or higher, a grain boundary layer 33a with high ion conductivity is easily formed at the grain boundary 33 between the first phase region 31 and the second phase region 32 of the solid electrolyte layer 3, and a solid electrolyte layer 3 with high ion conductivity is formed. When the heating temperature in the debinding and sintering process is 1100°C or lower, the coarsening of the particles constituting the first phase region 31 and the second phase region 32 is suppressed, and the amount of the grain boundary layer 33a increases. As a result, a solid electrolyte layer 3 having the first phase region 31 and the second phase region 32 and high ion conductivity is formed. The heating temperature in the debinding and sintering process is preferably 600°C to 1000°C.
[0096] The sintered laminate 4 (sintered body) can also be placed in a cylindrical container together with abrasive materials such as aluminum oxide and ground by a drum grinding method. Thus, the chamfering of the corners of the laminate 4 can be performed. The grinding of the laminate 4 can also be performed using a sandblasting method. The sandblasting method can only reduce a specific portion of the surface of the laminate 4, so it is preferred.
[0097] Next, first external terminals 5 and second external terminals 6 are formed on mutually opposing side surfaces of the produced laminated body 4. The first external terminals 5 and second external terminals 6 can be formed by sputtering, dipping, screen printing, spraying, or the like.
[0098] By going through the above steps, the all-solid secondary battery 10 can be manufactured.
[0099] The all-solid secondary battery 10 of the present embodiment has a solid electrolyte layer 3, which has: a first phase region 31, which includes a first solid electrolyte, the first solid electrolyte contains Li, Si, P and O, and has a γ-Li3PO4 type crystal structure; and a second phase region 32, which includes a second solid electrolyte, the second solid electrolyte contains Li, Si, P and O, is composed of a composition different from the above-mentioned first solid electrolyte, and has a Li4SiO4 type crystal structure. Therefore, the solid electrolyte layer 3 of the all-solid secondary battery 10 of the present embodiment has high ion conductivity. In the all-solid secondary battery 10 of the present embodiment, the principle of forming the solid electrolyte layer 3 with high ion conductivity has not yet been determined, but it is estimated that it is because in the firing process in the manufacturing process of the all-solid secondary battery 10, a grain boundary layer 33a with high ion conductivity is generated at the interface of the first phase region 31 and the second phase region 32 with different crystal phases.
[0100] Although the embodiments of the present invention have been described in detail with reference to the drawings, each structure in each embodiment and their combination are merely examples, and addition, omission, replacement, and other changes to the structure are possible without departing from the spirit of the present invention.
[0101] Example
[0102] Example 1
[0103] Li2CO3, SiO2 and Li3PO4 were prepared as starting materials. Li2CO3, SiO2 and Li3PO4 were weighed in a molar ratio of 2:1:1 and wet mixed for 16 hours using a ball mill with water as a dispersion medium. The obtained mixture was calcined at 1200°C for 2 hours to obtain Li 3.5 Si 0.5 P 0.5 The obtained particles were subjected to X-ray diffraction measurement using CuKα rays using an X-ray diffraction device (X'pert PRO manufactured by PANlytical) to confirm that they had a γ-Li3PO4 type crystal structure. The above steps gave particles composed of the first solid electrolyte of Example 1.
[0104] Li2CO3, SiO2 and Li3PO4 were prepared as starting materials. Li2CO3, SiO2 and Li3PO4 were weighed in a molar ratio of 6:3:1 and wet mixed for 16 hours using a ball mill with water as a dispersion medium. The obtained mixture was calcined at 1200°C for 2 hours to obtain Li 3.75 Si 0.75 P 0.25The obtained particles were subjected to X-ray diffraction measurement using CuKα rays using an X-ray diffractometer (X'pert PRO manufactured by PANlytical) to confirm that they had a Li4SiO4 type crystal structure. The above steps gave particles composed of the second solid electrolyte of Example 1.
[0105] 5 volume % of the particles consisting of the first solid electrolyte and 95 volume % of the particles consisting of the second solid electrolyte are weighed, wet mixed using a ball mill with water as a dispersion medium, and then dried to obtain a mixed powder of the first solid electrolyte and the second solid electrolyte.
[0106] Next, the obtained mixed powder was formed into a disk shape, placed on a ceramic table, and fired by heating at 900° C. for 0.5 hours in an air atmosphere to obtain a solid electrolyte layer of Example 1 composed of a fired body.
[0107] Embodiment 2 to Embodiment 7
[0108] Solid electrolyte layers of Examples 2 to 7 consisting of sintered bodies were obtained in the same manner as in Example 1, except that the ratio of particles consisting of the first solid electrolyte and particles consisting of the second solid electrolyte used as the material of the solid electrolyte layer was changed so that the total was 100 volume %.
[0109] Embodiments 8 to 11
[0110] The same method as in Example 1 was used except that the molar ratio of Li2CO3, SiO2 and Li3PO4 used as the material of the particles constituting the first solid electrolyte was changed to obtain a solid electrolyte composed of Li 3.55 Si 0.55 P 0.45 O4、Li 3.33 Si 0.33 P 0.67 O4、Li 3.09 Si 0.09 P 0.91 O4、Li 3.05 Si 0.05 P 0.95 The obtained particles were subjected to X-ray diffraction measurement using CuKα rays using an X-ray diffraction device (X'pert PRO manufactured by PANlytical) to confirm that they had a γ-Li3PO4 type crystal structure. The particles composed of the first solid electrolyte of Examples 8 to 11 were obtained through the above steps.
[0111] Then, the same procedure as in Example 4 was carried out except that the particles composed of the first solid electrolyte of Examples 8 to 11 were used, thereby obtaining solid electrolyte layers of Examples 8 to 11 composed of sintered bodies.
[0112] Embodiments 12 to 15
[0113] The same method as in Example 1 was used except that the molar ratio of Li2CO3, SiO2 and Li3PO4 used as the material of the particles constituting the second solid electrolyte was changed to obtain a solid electrolyte composed of Li 3.67 Si 0.67 P 0.33 O4、Li 3.83 Si 0.83 P 0.17 O4、Li 3.91 Si 0.91 P 0.09 O4、Li 3.95 Si 0.95 P 0.05 The obtained particles were subjected to X-ray diffraction measurement using CuKα rays using an X-ray diffractometer (X'pert PRO manufactured by PANlytical) to confirm that they had a Li4SiO4 type crystal structure. The particles composed of the second solid electrolyte of Examples 12 to 15 were obtained through the above steps.
[0114] Then, the same procedure as in Example 4 was carried out except that the particles composed of the second solid electrolyte of Examples 12 to 15 were used, thereby obtaining solid electrolyte layers of Examples 12 to 15 composed of sintered bodies.
[0115] Comparative Example 1
[0116] A solid electrolyte layer of Comparative Example 1 consisting of a sintered body was obtained in the same manner as in Example 1 except that 100% by volume of particles consisting of the first solid electrolyte were used and particles consisting of the second solid electrolyte were not used.
[0117] Comparative Example 2
[0118] A solid electrolyte layer of Comparative Example 2 consisting of a sintered body was obtained in the same manner as in Example 1 except that 100% by volume of particles consisting of the second solid electrolyte were used instead of the particles consisting of the first solid electrolyte.
[0119] For the solid electrolyte layers of Examples 1 to 15, Comparative Examples 1 and 2 thus obtained, the composition of the first solid electrolyte (first phase region 31), the ratio of the number of Si atoms contained in the first phase region 31 to the number of P atoms (Si / P in the first phase region), the composition of the second solid electrolyte (second phase region 32), and the ratio of the number of Si atoms contained in the second phase region 32 to the number of P atoms (Si / P in the second phase region) are shown in Table 1. In Table 1, the first phase region 31 is described as region A, and the second phase region 32 is described as region B. In addition, 100% by volume is described as 1.
[0120] In addition, the composition of the first phase region 31 in the solid electrolyte layer of Examples 1 to 15, Comparative Examples 1 and 2 can be regarded as the same as the first solid electrolyte used as the material of the first phase region 31. In addition, the crystal structure of the first solid electrolyte in the first phase region 31 can be regarded as the same as the first solid electrolyte used as the material of the first phase region 31.
[0121] Similarly, the composition of the second phase region 32 in the solid electrolyte layer of Examples 1 to 15, Comparative Examples 1, and 2 can be regarded as the same as the second solid electrolyte used as the material of the second phase region 32. In addition, the crystal structure of the second solid electrolyte in the second phase region 32 can be regarded as the same as the second solid electrolyte used as the material of the second phase region 32.
[0122]
[0123] In addition, for the solid electrolyte layers of Examples 1 to 15, Comparative Examples 1 and 2, the volume ratio (volume %) of the first phase region 31 in the solid electrolyte layer 3, the volume ratio (volume %) of the second phase region 32 in the solid electrolyte layer 3, and the ratio of the volume of the first phase region 31 to the volume of the second phase region 32 (first phase region / second phase region) were obtained by the method shown below. The results are shown in Table 1.
[0124] The solid electrolyte layer 3 was cut to expose the cross section, and a cross section polisher (CP) was used to obtain a smooth cross section. The cross section was then observed using a scanning electron microscope (SEM) at 5000 times magnification to obtain secondary electron composition images of 10 viewing fields.
[0125] For the particles with bright contrast and dark contrast in the secondary electron composition images of the obtained 10 fields of view, composition analysis was performed by energy dispersive X-ray analysis (EDS) to distinguish the first phase region 31 and the second phase region 32. Then, each secondary electron composition image was converted into a black and white image and binarized, and the number of pixels of the portion corresponding to the first phase region 31 and the portion corresponding to the second phase region 32 in each field of view were measured and added up respectively.
[0126] Then, the volume ratio of the first phase region 31 and the second phase region 32 is calculated for each viewing field using the following formula, and the average value of 10 viewing fields is defined as the volume ratio (volume %) of each region.
[0127] Volume ratio (volume %) of the first phase region 31 (or the second phase region 32) = (number of pixels of the first phase region 31 (or the second phase region 32) in the field of view / number of pixels of the entire field of view) × 100
[0128] In addition, the volume ratio of the first phase region 31 to the volume ratio of the second phase region 32 is calculated using the obtained volume ratios of the respective regions, and is set as (first phase region /
[0129] second phase region).
[0130] (Determination of ionic conductivity)
[0131] The mixed powder produced in the manufacturing process of the solid electrolyte layer of Examples 1 to 15, the particles composed of the first solid electrolyte produced in the manufacturing process of the solid electrolyte layer of Comparative Example 1, and the particles composed of the second solid electrolyte produced in the manufacturing process of the solid electrolyte layer of Comparative Example 2 were respectively formed into a disk shape to obtain a molded body. The obtained molded body was heated at 900° C. for 1 hour in an air atmosphere, thereby calcining to obtain a solid electrolyte layer for measuring ion conductivity.
[0132] Electrodes were connected to both surfaces of the obtained solid electrolyte layer, and the ion conductivity was measured using an impedance analyzer (manufactured by Solartron, Model SI1260) under the conditions of an amplitude of 50 mV and a frequency of 0.5 Hz to 1 MHz.
[0133] As shown in Table 1, compared with the solid electrolyte layers of Comparative Examples 1 and 2, the solid electrolyte layers of Examples 1 to 15 have higher ion conductivity.
[0134] In particular, compared with the solid electrolyte layers of Example 1 and Example 7, the solid electrolyte layers of Examples 2 to 6 and Examples 8 to 15, in which the ratio of the volume of the first phase region to the volume of the second phase region (first phase region / second phase region) is greater than 0.1 and less than 9, have higher ion conductivity.
[0135] In addition, compared with Example 11 in which the Si / P in the first phase region is less than 0.1 and the volume ratio of region A and region B is the same as that of Example 4, the ion conductivity of Example 4 in which the ratio of the number of Si atoms contained in the first phase region to the number of P atoms (Si / P in the first phase region) is 1 is higher.
[0136] In addition, compared with Examples 14 and 15 in which the Si / P in the second phase region exceeds 9 and the volume ratio of Region A and Region B is the same as that of Example 4, the ion conductivity of Example 4 in which the ratio of the number of Si atoms contained in the second phase region to the number of P atoms (Si / P in the second phase region) is 3 is higher.
[0137] Description of Reference Numerals
[0138] 1 positive electrode layer; 1A positive electrode current collector;
[0139] 1B positive electrode active material layer; 2 negative electrode layer;
[0140] 2A negative electrode current collector; 2B negative electrode active material layer;
[0141] 3 solid electrolyte layer; 4 laminate;
[0142] 5 first external terminal; 6 second external terminal;
[0143] 10 All-solid secondary battery; 31 First phase region;
[0144] 32 second phase region; 33 grain boundary;
[0145] 33a Grain boundary layer.
Claims
1. A solid electrolyte layer, wherein: have: a first phase region comprising a first solid electrolyte containing Li, Si, P and O and having a γ-Li3PO4 type crystal structure; and The second phase region includes a second solid electrolyte, which contains Li, Si, P and O, has a composition different from that of the first solid electrolyte, and has a Li4SiO4 type crystal structure.
2. The solid electrolyte layer according to claim 1, wherein The ratio of the volume of the first phase region to the volume of the second phase region is 0.1 to 9.
3. The solid electrolyte layer according to claim 1 or 2, wherein: A ratio of the number of Si atoms contained in the first phase region to the number of P atoms is greater than or equal to 0.1 and less than 1.
5.
4. The solid electrolyte layer according to any one of claims 1 to 3, wherein The ratio of the number of Si atoms contained in the second phase region to the number of P atoms is 1.5 to 9.
5. An all-solid secondary battery, wherein: have: The solid electrolyte layer according to any one of claims 1 to 4; and The positive electrode layer and the negative electrode layer sandwich the solid electrolyte layer.