Semiconductor film and method for manufacturing semiconductor film
By using an indium oxide semiconductor film doped with tin and hydrogen in thin film transistors and performing crystallization at high temperatures, the problem of lower mobility in TFT is solved, and the high mobility and stability are achieved. The stable film formation process and sputtering target are carried out.
Patent Information
- Application Number
- CN202380027706.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-01
- Filing Date
- 2023-02-21
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is difficult to balance between providing high mobility and stability for thin film transistors (TFTs), especially when heat treatment is performed at high temperatures.
The stability and mobility of the film are ensured by adding an appropriate amount of hydrogen to the sputtering target and crystallizing at high temperature. .
A semiconductor film with a small reduction in mobility when heat treatment is performed at high temperatures, taking into account high mobility and stable operation, and provides a stable film formation process and sputtering target.
Smart Images

Figure CN118946957A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a semiconductor film, and more particularly to a semiconductor film including solid-phase crystallized tin-doped indium oxide containing hydrogen atoms, a method for producing the semiconductor film, a sputtering target used for producing the semiconductor film, and a thin film transistor. Background Art
[0002] Tin-doped indium oxide (ITO) is used as a transparent electrode in display devices, touch panels, etc. It is also used as a component of semiconductor devices such as a semiconductor layer (sometimes also called a channel layer) of a thin film transistor (TFT) (for example, see Patent Documents 1 to 6).
[0003] Patent Document 1 discloses a TFT having a gate electrode, a gate insulating film, a source electrode, a drain electrode, and a semiconductor layer of an ITO film with low conductivity, wherein the carrier concentration of the semiconductor layer is 10 18 pcs.cm -3 Hereinafter, the semiconductor layer is set as a light-transmitting film.
[0004] Patent Document 2 discloses the use of a covalently bonded oxide other than a non-transition metal provided with dopant atoms in the semiconductor material of the channel region. In addition, it is taught that by setting the concentration of dopant atoms in the range of 0.001% to 0.3%, a conductivity sufficient for a semiconductor material used as a switching element can be obtained.
[0005] Patent document 3 discloses a TFT having a crystalline indium oxide semiconductor film, wherein the content of a metal element having a positive valence of tetravalent or higher is 10 atomic ppm or less relative to the metal element contained in the semiconductor film. It has been found that impurities in a semiconductor film composed of crystalline indium oxide, specifically metal elements having a positive valence of tetravalent or higher, affect the trap density of the semiconductor film, and the use of high-purity crystalline indium oxide is proposed.
[0006] Patent document 4 discloses a tin-containing In2O3 sintered body, which is an In2O3 sintered body containing tin as an added element, characterized in that tin is added so that the ratio of the number of tin atoms to the total number of atoms of all metal elements in the sintered body is 0.01 to 0.2%, thereby making the relative density greater than 98%.
[0007] Patent Document 5 discloses a method for forming a film of an oxide semiconductor, wherein the water content in a sputtering device is 3×10 -4 ~5×10 -2 Pa, a sputtering target composed of a metal oxide is DC sputtered to form a film-forming body, and the film-forming body is crystallized.
[0008] Patent document 6 discloses a stacked structure having an oxide semiconductor thin film layer and a TFT using the same for a channel layer, and discloses that the material constituting the oxide semiconductor thin film layer is a stacked structure consisting of indium oxide, Ga-doped indium oxide, Al-doped indium oxide, Zn-doped indium oxide and Sn-doped indium oxide.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Application Laid-Open No. 05-251705
[0012] Patent Document 2: Japanese Patent Publication No. 11-505377
[0013] Patent Document 3: International Publication No. 2010 / 047063
[0014] Patent Document 4: Japanese Patent Application Publication No. 2011-093730
[0015] Patent Document 5: Japanese Patent Application Publication No. 2011-222557
[0016] Patent Document 6: Japanese Patent Application Publication No. 2012-253315 Summary of the invention
[0017] It is known that a high-mobility oxide semiconductor film can be formed by forming a high-purity indium oxide film by sputtering in the presence of water or hydrogen and then crystallizing the film. However, sometimes the mobility is reduced due to heat treatment at a high temperature (for example, above 350°C) for stabilization of the TFT. Therefore, it is sometimes difficult to achieve both high mobility and stable operation in a TFT.
[0018] The present invention aims to provide a semiconductor film and a method for manufacturing the semiconductor film, which has a small decrease in mobility even when heat-treated at high temperature for stabilizing TFTs, and a sputtering target capable of stably forming a film when manufacturing the semiconductor film.
[0019] According to the present invention, the following semiconductor films and the like are provided.
[0020] 1. A semiconductor film comprising a solid phase crystallized product of indium oxide doped with tin and hydrogen.
[0021] 2. The semiconductor film according to 1, wherein the content ratio of tin atoms (Sn) in the solid phase crystallized product to the total of indium atoms (In) and tin atoms (Sn) [Sn / (In+Sn): molar ratio] is 0.000005 to 0.008,
[0022] The concentration of hydrogen atoms (H) measured by secondary ion mass spectrometry was 0.5×1020 ~50×10 20 atoms / cc.
[0023] 3. The semiconductor film according to 1 or 2, which has a conical cross section.
[0024] 4. A method for manufacturing a semiconductor film according to any one of 1 to 3, comprising:
[0025] A step of forming an amorphous film by sputtering a tin-doped indium oxide (ITO) sputtering target in a film-forming gas containing a gas supplying hydrogen atoms at a partial pressure of 0.5 to 12%;
[0026] The amorphous film is heated to be crystallized.
[0027] 5. The manufacturing method according to 4, further comprising: after the step of forming the amorphous film, a step of processing the etched cross section into a tapered shape in a photolithography step.
[0028] 6. A tin-doped indium oxide sputtering target, wherein the content ratio of tin atoms (Sn) to the total of indium atoms (In) and tin atoms (Sn) [Sn / (In+Sn): molar ratio] is 0.000005 to 0.008, and is used for forming an amorphous film of indium oxide doped with tin and hydrogen.
[0029] 7. A thin film transistor comprising the semiconductor film according to any one of 1 to 3.
[0030] According to the present invention, a semiconductor film having a small decrease in mobility even when heat-treated at a high temperature for stabilizing a TFT and a method for manufacturing the same can be provided. In addition, a sputtering target capable of stably forming a film when manufacturing the semiconductor film can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 It is a schematic cross-sectional view of a TFT according to one embodiment of the present invention.
[0032] Figure 2 This is a SEM photograph of a cross section of the sputtering target produced in Example 1-1.
[0033] Figure 3 This is a schematic cross-sectional view of a TFT fabricated in an example.
[0034] Figure 4 This is the transfer curve of the TFT produced in Example 2-1.
[0035] Figure 5 This is a Vg-μ graph of the TFT produced in Example 2-1.
[0036] Figure 6This is the transfer curve of the TFT produced in Comparative Example 3-1.
[0037] Figure 7 This is a Vg-μ graph of the TFT produced in Comparative Example 3-1. DETAILED DESCRIPTION
[0038] In this specification and the like, the term "film" or "thin film" and the term "layer" can be used interchangeably according to circumstances.
[0039] In the sintered body and the oxide thin film in this specification and the like, the term "compound" and the term "crystalline phase" can be used interchangeably as the case may be.
[0040] In this specification, the "oxide sintered body" may be simply referred to as a "sintered body".
[0041] In this specification, a "sputtering target" may be simply referred to as a "target".
[0042] In this specification, etc., "electrical connection" includes connection via "some substance having an electrical function". Here, "some substance having an electrical function" is not particularly limited as long as it can transmit and receive electrical signals between the connected objects. For example, "some substance having an electrical function" includes electrodes, wiring, switching elements (transistors, etc.), resistors, inductors, capacitors, and other elements with various functions.
[0043] In this specification, the functions of the source and drain of a transistor may be interchanged when transistors of different polarities are used or when the direction of current changes during circuit operation. Therefore, in this specification, the terms source and drain may be used interchangeably.
[0044] In the present specification, "x to y" represents a numerical range of "x or more and y or less." The upper limit value and the lower limit value described in the numerical range can be arbitrarily combined.
[0045] Furthermore, an embodiment in which two or more of the embodiments of the present invention described below are combined is also an embodiment of the present invention.
[0046] 1. Semiconductor film
[0047] The semiconductor film according to the present embodiment includes a solid phase crystallized material of indium oxide doped with tin and hydrogen (hereinafter, indium oxide doped with tin and hydrogen may be abbreviated as H:ITO).
[0048] Here, solid phase crystallization refers to crystallizing an amorphous (non-crystalline) body in a solid phase by heating. On the other hand, gas phase crystallization refers to crystallization by, for example, film formation.
[0049] It is known that vapor-phase crystallized indium oxide and tin-doped indium oxide (ITO) cannot be etched without using a strong acid such as aqua regia. When etching with a strong acid, the source electrode, drain electrode, gate electrode, etc. constituting the TFT are sometimes damaged, so their use is restricted. In addition, damage to the interlayer insulating film, gate insulating film, etc. is also considered.
[0050] On the other hand, the amorphous film used in the solid phase crystallization can be etched even with weak acid organic acids such as oxalic acid, so there is no influence on the source electrode, drain electrode, gate electrode, etc. constituting the TFT, and thus the TFT can be manufactured stably.
[0051] In this aspect, for example, by crystallizing an amorphous film in a solid phase formed by sputtering by heating after etching, a semiconductor film including a solid phase crystallized product of H:ITO can be obtained.
[0052] Tin-and-hydrogen-doped indium oxide (H:ITO) means indium oxide doped with tin atoms and hydrogen atoms.
[0053] The doping and doping amount (content) of tin and hydrogen can be measured by elemental analysis such as secondary ion mass spectrometry (SIMS), high frequency inductively coupled mass spectrometry (ICP-MS), or the like.
[0054] The thickness of the semiconductor film of this embodiment is preferably 5nm to 150nm. If it is within this range, it is easy to obtain a homogeneous film, and the film formation time is appropriate, and the productivity is improved. In addition, the mobility is sometimes increased when used in TFT. It is preferably 10nm to 100nm, and more preferably 15nm to 80nm.
[0055] It is known that the addition of tin atoms to indium oxide has the effect of improving the sinterability (crystallinity) of a sintered body crystal. Similarly, it is believed that the crystallinity of an indium oxide film to which tin atoms are added is improved.
[0056] If the amount of tin atoms added is too small, a semiconductor film may not be able to withstand heating at, for example, 350° C. or higher. On the other hand, if too much tin atoms are added, a transparent conductive film may be formed and the film may not function as a semiconductor film.
[0057] From the above viewpoints, in the semiconductor film of the present embodiment, the content ratio of tin atoms (Sn) in the solid phase crystallized material to the total content ratio of indium atoms (In) and tin atoms (Sn) [Sn / (In+Sn): molar ratio] is preferably 0.000005 to 0.008. It is more preferably 0.00001 to 0.005, further preferably 0.00002 to 0.003, and particularly preferably 0.00002 to 0.001. The upper limit may be less than 0.001.
[0058] In addition, it is known that in ITO, tin (Sn 4+ ) dopant activation, Sn at the In site of In2O3 crystal 4+ For example, if all the added tin atoms are activated and each unit of tin dopant emits 2 electron carriers, even if the amount of SnO2 added as the raw material is 0.01% by mass, per 1 cm 3 The number of tin atoms is also 6.5×10 18 Therefore, the electron concentration is assumed to be 10 18 More than one, a transparent conductive film is expected to be formed.
[0059] However, surprisingly, it is considered that the tin dopant is not activated in the present embodiment, and as a result, a semiconductor film is formed.
[0060] In addition, the following possibility is considered: during the crystallization process, Sn 4+ Reduced by H dopant to Sn 2+ , even if the In site of In2O3 crystal is composed of Sn 2+ In order to operate as a semiconductor film without generating electron carriers even if substitution is performed, hydrogen doping becomes important.
[0061] Furthermore, it is well known that in the case of a crystalline indium oxide thin film, carriers are generated due to oxygen defects. It is also considered that the generation of carriers due to oxygen defects can be compensated by -OH groups, thereby suppressing the generation of carriers.
[0062] On the other hand, In defects may also occur. + To compensate for the In in the crystal 3+ Possibility of defects. + The ionic radius of the ion is In 3+ Ionic radius of ions (6-coordinate In 3+ )for Therefore, it is also possible to consider the H with a smaller ionic radius. + The possibility that the In ions compensate for the In defects and maintain the stability of the crystal.
[0063] From the above viewpoints, the concentration of hydrogen atoms (H) contained in the semiconductor film is preferably 0.5×10 20 ~50×10 20 atoms / cc. If it is less than 0.5×10 20 atoms / cc, there is sometimes no effect of hydrogen addition. In addition, in order to make it less than 0.5×10 20atoms / cc, it is sometimes necessary to dehydrogenate the crystallized indium oxide film under high temperature and high vacuum, which reduces productivity. 20 atoms / cc, the amount of hydrogen due to physically adsorbed water may be included, resulting in a decrease in mobility or a decrease in driving stability of the TFT. More preferably, 1×10 20 ~30×10 20 atoms / cc, more preferably 1×10 20 ~20×10 20 atoms / cc, particularly preferably 1×10 20 ~10×10 20 atoms / cc.
[0064] In addition, the concentration of hydrogen atoms (H) contained in the semiconductor film is set to the hydrogen concentration (atoms / cc) measured by secondary ion mass spectrometry (SIMS). In addition, the concentration of hydrogen atoms (H) contained in the solid phase crystallized material is not constant in the depth direction of the film thickness but varies, and is shown as an average value.
[0065] In the semiconductor film of this embodiment, it is preferable that the etched cross section has a tapered shape, so that when forming a constituent film of a TFT such as an interlayer insulating film or a gate insulating film, it is easy to ensure insulation from other films.
[0066] The taper angle (the inner angle between the bottom and the side of the cross section) is 45° to 90°. If it is less than 45°, the width of the taper shape becomes wider, which is sometimes not suitable for the manufacture of TFTs with shorter channel widths. On the other hand, if it exceeds 90°, sometimes the coverage of the interlayer insulating film is insufficient and contacts with other layers, and the TFT does not work. The taper angle is preferably 50° to 85°, and more preferably 55° to 80°.
[0067] 2. Semiconductor film manufacturing method
[0068] The semiconductor film of the present invention can be manufactured, for example, by sputtering an ITO target in a film forming gas (sputtering gas) containing a gas supplying hydrogen atoms at a partial pressure of 0.5 to 12% to form an amorphous film, and then heating the amorphous film to crystallize it.
[0069] As the gas supplying hydrogen atoms, water (water vapor), hydrogen, etc. can be used. The gas supplying hydrogen atoms is preferably supplied to the sputtering device in a gaseous state. The concentration of the gas supplying hydrogen atoms during sputtering is adjusted according to the desired crystallization temperature.
[0070] For example, when the hydrogen atom supply gas is supplied at a partial pressure of less than 0.5% during sputtering, the film tends to crystallize at a low temperature, so a gas phase crystallized film may be obtained. As a result, sometimes crystallization occurs during heat treatment in the photolithography process and etching becomes impossible, or residue is generated and etching is poor, which hinders the manufacture of TFTs.
[0071] On the other hand, if the partial pressure of the hydrogen atom supply gas is increased, the crystallization temperature tends to increase. When the hydrogen atom supply gas is supplied at a partial pressure exceeding 15%, the crystallization temperature caused by heating becomes higher than the desired temperature, so that the amorphous film may not be crystallized, or even if it is crystallized, the crystallinity may be low. As a result, the mobility of the TFT may be reduced.
[0072] The supply amount of the hydrogen atom supply gas is preferably such that the partial pressure is 0.5 to 12%, more preferably 1 to 12%, further preferably 1 to 10%, and particularly preferably 2 to 8%.
[0073] An oxidizing gas may be mixed in the film-forming gas. As the oxidizing gas, oxygen, N2O, NO2, etc. can be used. Among them, oxygen is preferred.
[0074] When hydrogen is used as the hydrogen atom supply gas, it is preferably used together with oxygen. When sputtering is performed by supplying only hydrogen without supplying oxygen, In2O3 itself is reduced to generate oxygen defects, and thus a transparent conductive film may be formed.
[0075] When forming a semiconductor film, it is preferable to use oxygen and hydrogen, or water and hydrogen in combination.
[0076] When oxygen and hydrogen are used in combination, the amount of oxygen supplied during sputtering is adjusted according to the amount of hydrogen used in combination. As shown in the following formula, oxygen and hydrogen react to generate water.
[0077] H2+1 / 2O2→H2O
[0078] Therefore, the supply amount of hydrogen is preferably at least twice that of oxygen. This allows efficient hydrogen doping.
[0079] On the other hand, when water is used as the hydrogen atom supply gas, hydrogen doping can be performed using hydrogen atoms contained in water molecules, but hydrogen doping can be performed more efficiently by further supplying hydrogen.
[0080] The conditions for sputtering the ITO target in the film forming gas containing at least one of a gas supplying hydrogen atoms and an oxidizing gas are not particularly limited and can be appropriately adjusted according to the apparatus used, the composition of the target, the composition of the sputtering gas, and the like.
[0081] The film forming method is not particularly limited, and examples thereof include DC sputtering, AC sputtering, RF sputtering, ICP sputtering, reactive sputtering, etc. Among them, as DC sputtering, pulse DC sputtering can be preferably used.
[0082] In the case of pulsed DC sputtering, the pulse frequency is, for example, 1 KHz to 1 MHz, preferably 10 KHz to 500 KHz, and more preferably 30 KHz to 300 KHz. In addition, the driving time in the pulse (the actual ratio of sputtering drive, expressed as duty cycle (%)) is usually 30% to 95%, preferably 40% to 95%, and more preferably 50% to 90%.
[0083] If the duty ratio is below 30%, the sputtering speed may decrease, the sputtering time may become longer, and the productivity may decrease. If the duty ratio is above 95%, the sputtering speed may increase excessively, and the yellow flakes may increase during sputtering, and may sometimes adhere to the target as foreign matter and cause nodules.
[0084] The sputtering film forming output relative to the target area is, for example, 1 W / cm 2 ~10W / cm 2 If less than 1w / cm 2 , sometimes the sputtering speed is reduced, the sputtering time is prolonged, and the productivity is reduced. In addition, the density of the obtained film is sometimes reduced. If 10W / cm 2 If the output is too high, a large amount of yellow flakes may be produced.
[0085] The film output is 8W / cm 2 In the case of about 1w / cm, by shortening the duty cycle, it is possible to adjust to suppress the generation of yellow flakes. 2 In the case of an output of about 200 Å, by extending the duty ratio, it is possible to adjust so that the sputtering rate is increased and the productivity is maintained high, or the generation of yellow flakes and nodules can be suppressed.
[0086] After forming an amorphous film by sputtering, the amorphous film is heated to be crystallized, thereby obtaining the semiconductor film of the present invention (film containing a solid phase crystallized product of H:ITO). In addition, the crystallization treatment by heating is sometimes called annealing.
[0087] The crystallization temperature is, for example, 200° C. to 500° C. If it is less than 200° C., crystallization may not occur. On the other hand, if it exceeds 500° C., the durability of the heating device may become a technical problem. It is preferably 250° C. to 450° C.
[0088] In the crystallization treatment, for example, by maintaining the temperature in a crystallization temperature range for a certain period of time or increasing the temperature at a temperature increase rate of 10° C. / min or less, an oxide semiconductor film with good crystallinity can be obtained.
[0089] The crystallization temperature changes depending on the amount of hydrogen atom supply gas supplied during film formation, and therefore the combination with film formation conditions becomes important.
[0090] When the crystallization temperature is maintained for a certain period of time, the holding time is preferably 5 to 60 minutes. If it is less than 5 minutes, crystallization may not start, and if it exceeds 60 minutes, the holding time is long, which becomes the main reason for reducing productivity. It is preferably 8 to 45 minutes, and more preferably 10 to 30 minutes.
[0091] In addition, it is also preferred to implement the heat treatment of crystallization in two stages. The crystal can be grown by the heat treatment in the first stage, and the crystal can be stabilized by the heat treatment in the second stage. The temperature can also be changed in each heat treatment. For example, the heat treatment in the first stage can be set to a low temperature and the heat treatment in the second stage can be set to a high temperature to crystallize, or the heat treatment in the first stage can be set to a high temperature and the heat treatment in the second stage can be set to a low temperature to crystallize, thereby stabilizing the crystal.
[0092] It is also possible to form a SiO2 film by N2 treatment or CVD treatment between the first stage of heat treatment and the second stage of heat treatment, and to set an interlayer insulating film, a gate insulating film, etc. In the formation process of the SiO2 film based on N2 treatment or CVD treatment, defects in the crystal structure are sometimes generated in the semiconductor film, or there are excess oxygen elements and hydrogen elements between crystal layers or between layers of other layers. By performing the heat treatment in two stages, the heat treatment in the second stage sometimes has an effect on stabilizing the semiconductor film.
[0093] The manufacturing method of this embodiment may include a step of processing the etched cross section into a tapered shape in a photolithography step after forming the amorphous film. Also, the amorphous film may be heated and crystallized (annealed) after being processed into the tapered shape.
[0094] Regarding the adjustment of the taper angle, if the adhesion between the resist and the amorphous film is improved, the taper angle tends to become larger. If the adhesion is reduced, the taper angle tends to become smaller. Therefore, the taper angle can be adjusted by controlling the adhesion.
[0095] Furthermore, if the temperature of the etching solution is increased, the taper angle tends to increase, and if the temperature is decreased, the taper angle tends to decrease. The above-mentioned adhesion between the resist and the amorphous film and the temperature of the etching solution can be combined for control.
[0096] When the semiconductor film formed by the above-mentioned manufacturing method is used in a TFT, the mobility does not decrease or decreases slightly even when exposed to high temperature. Therefore, even if high-temperature annealing is performed for stabilization of the TFT, the high mobility can be maintained, so that high mobility and stable operation can be achieved in the TFT.
[0097] The high-temperature annealing temperature for stabilizing the TFT may be 250° C. or higher, 300° C. or higher, or 350° C. or higher, and is usually 500° C. or lower.
[0098] 3. Sputtering target
[0099] The sputtering target according to one aspect of the present invention is a tin-doped indium oxide sputtering target for forming an amorphous film of indium oxide doped with tin and hydrogen, that is, an ITO target used in the production method of item 2 above.
[0100] From the same viewpoint as the semiconductor film of item 1 above, in the target of this embodiment, the content ratio of tin atoms (Sn) to the total of indium atoms (In) and tin atoms (Sn) [Sn / (In+Sn): molar ratio] is preferably 0.000005 to 0.008, more preferably 0.00002 to 0.005, further preferably 0.00003 to 0.005, and particularly preferably 0.00005 to 0.005.
[0101] By adding tin atoms, the tin atoms are solid-dissolved in indium oxide to generate carriers, thereby having an effect of reducing the resistance of the target.
[0102] In the target of this embodiment, the relative density is preferably 99.0% or more. This allows stable film formation. The relative density is more preferably 99.1% or more. In addition, relative density refers to the measured value relative to the theoretical density (7.18 g / cm 3 ) ratio (%).
[0103] In addition, the bulk (intrinsic) resistance value of the target is preferably 10 mΩcm or less. This allows stable film formation. The bulk resistance value is more preferably 5 mΩcm or less. In addition, the bulk resistance value is a value measured by the method described in the Examples.
[0104] The target manufacturing method of this scheme is not particularly limited, and a general method can be used. Specifically, when the content of tin atoms is more than 0.0001, it can be manufactured by the following method: indium oxide and tin oxide as raw materials are mixed and crushed, the mixed powder is formed, and then sintered to form an oxide sintered body, which is cut and ground as needed and fixed to a backing plate.
[0105] On the other hand, when the content of tin atoms is less than 0.0001, the relative density of the target is sometimes reduced, or the bulk resistance value is increased. However, by using a device such as a planetary ball mill that can perform high-energy mixing and crushing, the raw materials are made into fine sintering powder, and a high-density and low-resistance sintered body (target) can be manufactured.
[0106] The shape of the target can be selected from circular, rectangular, cylindrical, etc. according to the sputtering device.
[0107] The purity of indium oxide as a raw material is preferably 99.9% or more, more preferably 99.99% or more, and even more preferably 99.995% or more. By making the purity higher, scattering of carriers caused by impurities can be suppressed, and a high-performance semiconductor film can be produced.
[0108] The crystal grain size in the target (sintered body) is preferably 0.5 to 20 μm. If it is less than 0.5 μm, the crystal grains are too small, the strength of the sintered body is reduced, and sometimes cracks or microcracks occur. On the other hand, if the crystal grains are larger than 20 μm, the crystals sometimes grow abnormally and crack or microcracks occur inside the crystals. In a target with microcracks, a large amount of yellow flakes or nodules are sometimes produced. The removal of yellow flakes and nodules takes time, the actual sputtering time is shortened, and sometimes the productivity is reduced. The crystal grain size is more preferably 1 to 15 μm, and more preferably 1 to 10 μm.
[0109] 4. Thin Film Transistor
[0110] The TFT according to this embodiment includes the semiconductor film of the present invention described above. The semiconductor film of the present invention is preferably used as a semiconductor layer (channel layer) of the TFT.
[0111] Figure 1 It is a schematic cross-sectional view of a thin film transistor according to one embodiment of the present invention.
[0112] like Figure 1 As shown, the thin film transistor 100 includes a silicon wafer 20 , a gate insulating film 30 , a semiconductor film 40 , a source electrode 50 , a drain electrode 60 , and interlayer insulating films 70 , 70A.
[0113] The silicon wafer 20 is a gate electrode. The gate insulating film 30 is an insulating film that blocks conduction between the gate electrode and the semiconductor film 40 , and is provided on the silicon wafer 20 .
[0114] The semiconductor film 40 is a channel layer, and is provided on the gate insulating film 30. As the semiconductor film 40, the semiconductor film according to the present invention is used.
[0115] The source electrode 50 and the drain electrode 60 are conductive terminals for allowing a source current and a drain current to flow through the semiconductor film 40 , and are provided in contact with the vicinity of both ends of the semiconductor film 40 .
[0116] The interlayer insulating film 70 is an insulating film that blocks conduction between the source electrode 50 and the drain electrode 60 and the semiconductor film 40 except for the contact portions.
[0117] The interlayer insulating film 70A is an insulating film that blocks conduction in portions other than the contact portions between the source electrode 50 and the drain electrode 60 and the semiconductor film 40. The interlayer insulating film 70A is also an insulating film that blocks conduction between the source electrode 50 and the drain electrode 60. The interlayer insulating film 70A is also a channel layer protection layer.
[0118] The materials forming the drain electrode 60, the source electrode 50, and the gate electrode are not particularly limited, and any commonly used material can be selected. Figure 1 In the example given, a silicon wafer is used as a substrate and the silicon wafer also functions as an electrode, but the electrode material is not limited to silicon.
[0119] For example, transparent electrodes such as ITO, indium zinc oxide (IZO), ZnO and SnO2, metal electrodes such as Al, Ag, Cu, Cr, Ni, Mo, Au, Ti and Ta, or metal electrodes containing alloys thereof, and stacked electrodes can be used.
[0120] In addition, Figure 1 In the present invention, a gate electrode can also be formed on a substrate such as glass.
[0121] The material forming the interlayer insulating films 70 and 70A is not particularly limited, and any commonly used material can be selected. Specifically, for example, SiO2, SiNx, Al2O3, Ta2O5, TiO2, MgO, ZrO2, CeO2, K2O, Li2O, Na2O, Rb2O, Sc2O3, Y2O3, HfO2, CaHfO3, PbTiO3, BaTa2O6, SrTiO3, Sm2O3, AlN and other compounds can be used as the material forming the interlayer insulating films 70 and 70A.
[0122] The shape of the thin film transistor involved in this scheme is not particularly limited, and preferably a bottom-gate transistor, a top-gate transistor, a double-gate transistor, a dual-gate transistor, a back-channel etched transistor, or an etch-stop transistor.
[0123] Among transistor characteristics, the switch (On / Off) characteristic is a factor that determines the display performance of the display. When a thin film transistor is used as a switch for liquid crystal, the switch ratio (On / Off ratio) is preferably above 6 digits. In the case of OLED, since it is current driven, the on current is more important, but the switch ratio is also preferably above 6 digits.
[0124] In one embodiment, the on / off ratio of the TFT is preferably 1×10 6 above.
[0125] The on / off ratio is more preferably 1×10 6 ~1×10 12 , more preferably 1×10 7 ~10 11 , more preferably 10 8 ~10 10 If the switching ratio is 1×10 6 If the on / off ratio is 1×10 12 If the on / off ratio is 1×10 12 Below, the shutdown current can be 10 -11 A or less, when a thin film transistor is used for a transfer transistor or a reset transistor of a CMOS image sensor, it is possible to extend the image retention time or improve the sensitivity.
[0126] The method for measuring the on / off ratio is described in detail in the embodiments.
[0127] In addition, in one embodiment, the mobility of the TFT is preferably 5 cm 2 / Vs or more, more preferably 10cm 2 / Vs or above.
[0128] The method for measuring the linear mobility is described in detail in the Examples.
[0129] The threshold voltage (Vth) is preferably -3.0 to 3.0 V, more preferably -2.0 to 2.0 V, and further preferably -1.0 to 1.0 V. If the threshold voltage (Vth) is above -3.0 V, a TFT with high mobility can be obtained. If the threshold voltage (Vth) is below 3.0 V, a TFT with a small off current and a large on / off ratio can be obtained.
[0130] The method for measuring the threshold voltage (Vth) is described in detail in the examples.
[0131] The off current is preferably 1×10 -10 A or less, more preferably 1×10 -11 A or less, more preferably 1×10 -12 A or below.
[0132] If the closing current is 1×10 -10 A or less, it is possible to drive an organic EL with a large contrast. In addition, when used for a transfer transistor or a reset transistor of a CMOS image sensor, it is possible to extend the image retention time or improve the sensitivity.
[0133] The method for measuring the off current is described in detail in the examples.
[0134] The TFT according to this embodiment can be suitably used in electronic devices such as solar cells, liquid crystal elements, display elements such as organic electroluminescent elements and inorganic electroluminescent elements, power semiconductor elements, and touch panels.
[0135] Example
[0136] Hereinafter, the present invention will be described in detail based on examples, but the present invention is not limited to the examples.
[0137] [Manufacturing of sputtering target]
[0138] Example 1-1
[0139] 0.01 mass % tin oxide (manufactured by Kojun Chemical) was added to 99.99 mass % indium oxide (manufactured by Kojun Chemical) and mixed and pulverized using a planetary ball mill (Pulverisette 5, manufactured by Fritsch, Germany). Zirconia beads were used as pulverizing media, the rotation speed was set to 220 rpm, and the treatment was performed for 4 hours.
[0140] The obtained powder is pressed and formed by granulation, stamping and CIP (cold isostatic pressing). The formed body is fired at 1450°C for 28 hours to obtain an oxide sintered body. After cooling to room temperature in the furnace, it is ground and polished. The ground oxide sintered body is joined to a backing plate to manufacture a sputtering target with a diameter of 4 inches and a thickness of 5 mm. In Example 1-1, the sputtering target has no cracks or breakages, and can be manufactured well.
[0141] Examples 1-2 to 1-5
[0142] As shown in Table 1, a sputtering target was produced in the same manner as in Example 1-1 except that the content of indium oxide and tin oxide was changed. In the example, the sputtering target was not cracked or broken, and was produced satisfactorily.
[0143] Comparative Examples 1-1 to 1-3
[0144] As shown in Table 1, a sputtering target was produced in the same manner as in Example 1-1 except that the blending of indium oxide and tin oxide was changed and a ball mill was used for mixing and pulverizing the raw materials. In the ball mill, the raw materials and zirconium oxide balls were placed in a plastic container and rotated using a rotating roller for 24 hours.
[0145] The raw material composition, the atomic (molar) ratio calculated from the composition, and the number of particles per cm 3 The number of tin atoms, relative density, and bulk resistance are shown in Table 1. The atomic ratio is the value of (In or Sn) / (In+Sn).
[0146] Furthermore, using CS200 manufactured by ULVAC, in an argon atmosphere containing 6% water (partial pressure), a sputtering pressure of 0.5 Pa and a DC power of 400 W (target having a diameter of 4 inches), the presence or absence of abnormal discharge during sputtering was observed for 2 hours.
[0147] The results are shown in Table 1.
[0148] [Table 1]
[0149]
[0150] With a density of 7.18 g / cm 3 The formula weight of indium oxide is 277.64 per 1cm 3 In any of the embodiments and comparative examples, per 1 cm 3 The number of tin atoms is 1×10 18 Therefore, the electron concentration is considered to be 10 18 Since the target has more than 100 nanometers, it is expected that the film formed by using the target will be a conductive film. However, in the examples described later, a semiconductor film was obtained.
[0151] Relative density is measured value × 100 / theoretical density (7.18g / cm 3 ).
[0152] The bulk resistance (mΩcm) was measured using a resistivity meter LORESTA (manufactured by Mitsubishi Chemical Corporation, LORESTA AX MCP-T370) according to the four-probe method (JIS R 1637). The measurement locations were the center of the sputtering target and the midpoint between the four corners and the center, a total of five locations, and the average value of the five locations was taken as the bulk resistance.
[0153] As can be seen from Table 1, the sputtering target produced using the planetary ball mill had a relative density of 99% or more, abnormal discharge was not observed during sputtering, and stable film formation was possible.
[0154] Figure 2 This is a SEM photograph of a cross section of the sputtering target (oxide sintered body) prepared in Example 1-1. Figure 2 , the average crystal grain size is 3.1μm.
[0155] [Semiconductor film, TFT production]
[0156] Examples 2-1 to 2-5
[0157] Using the sputtering target produced in Example 1-1, semiconductor films (evaluation samples) and semiconductor layers of TFTs were produced according to the film formation conditions shown in Table 2 (film formation atmosphere gas partial pressure ratios).
[0158] (A) Semiconductor film (sample for evaluation)
[0159] (1) Formation of oxide film
[0160] On a glass substrate (“ABC-G” manufactured by Nippon Electric Glass Co., Ltd.), an oxide film (film thickness: 40 nm) was formed under the film formation conditions shown in Table 2.
[0161] The sputtering conditions other than those described in Table 2 are as follows.
[0162] Ultimate pressure: 5×10 -5 Pa
[0163] Sputtering pressure: 0.5Pa
[0164] Sputtering method: DC magnetron sputtering
[0165] Sputtering power (W / cm 2 ):5.33(400W)
[0166] Duty cycle: 100%
[0167] Distance between T (target) and S (substrate): 70 mm
[0168] Substrate temperature: room temperature
[0169] The obtained oxide film was analyzed using an inductively coupled plasma emission spectrometer (ICP-AES, manufactured by Shimadzu Corporation), and it was confirmed that the atomic ratio of metal atoms in the oxide film was the same as the atomic ratio of metal atoms in the sputtering target used to manufacture the film.
[0170] (2) Crystallization treatment (annealing A)
[0171] The substrate with the oxide film was heat-treated under the conditions shown in Table 2. In Table 2, "-" for the heating rate means that the substrate was put into a furnace set at the heating temperature.
[0172] The film after the treatment was subjected to Hall effect measurement and evaluation of the crystallinity (crystalline or amorphous (amorphous)) of the film.
[0173] (3) Reduction treatment (annealing B)
[0174] The substrate after the crystallization treatment in (2) was placed in a furnace under nitrogen flow, heated from room temperature to 250°C over 3 minutes, and maintained at 250°C for 5 minutes. It was then cooled to below 100°C and taken out of the furnace.
[0175] Hall effect measurements were performed on the treated films.
[0176] (4) Stabilization treatment (annealing C)
[0177] After the above (3), the heating treatment was performed again at the temperature and time shown in Table 2 in the atmosphere.
[0178] For the treated films, the Hall effect and the concentration of hydrogen atoms (H) measured by secondary ion mass spectrometry were measured.
[0179] (B) Fabrication of TFT
[0180] Production Figure 3 TFT shown.
[0181] (1) Formation of oxide (amorphous) film
[0182] A silicon wafer 20 (gate electrode) with a SiO2 thermal oxide film (gate insulating film 30) was used as a substrate. On the SiO2 thermal oxide film, sputtering was performed through a metal mask using the sputtering target manufactured in Example 1-1 under the same film forming conditions as in (A)(1) above, thereby forming a 40 nm thick amorphous film 40.
[0183] (2) Formation of source and drain electrodes
[0184] Next, sputtering is performed using a titanium metal target through a metal mask having a contact hole shape for forming the source electrode 50 and the drain electrode 60 , thereby forming titanium electrodes to be the source electrode 50 and the drain electrode 60 , thereby manufacturing a TFT.
[0185] (3) Crystallization treatment (annealing A)
[0186] The TFT obtained in the above (2) was subjected to a heat treatment under the same conditions (Table 2) as those for the above (A) semiconductor film (evaluation sample).
[0187] (4) Reduction treatment (annealing B)
[0188] The TFT after the crystallization treatment in (3) was subjected to heat treatment under the same conditions (Table 2) as the semiconductor film (evaluation sample) in (A). That is, it was placed in a furnace under a nitrogen flow, heated from room temperature to 250°C in 3 minutes, and maintained at 250°C for 5 minutes. It was then allowed to cool to below 100°C and then taken out of the furnace.
[0189] (5) Stabilization treatment (annealing C)
[0190] After the above (4), the heat treatment was performed again under the same conditions (Table 2) as those for the above (A) semiconductor film (evaluation sample).
[0191] [Characteristics evaluation]
[0192] The following evaluations were performed on the evaluation samples and TFTs. The results are shown in Table 2. In the table, “X.XXE+YY” means “X.XX×10+YY For example, "1E-12" is "1×10 -12 ”.
[0193] (Hall Effect Measurement)
[0194] Evaluation was performed on each evaluation sample after the above annealing A, B and C. Metal indium (In) was soldered to the four corners of the substrate with the film in a size of about 2 mm×2 mm or less to prepare a sample for measuring the Hall effect.
[0195] The sample for Hall effect measurement was set in a Hall effect-resistivity measuring device (Resi Test 8300, manufactured by Toyo Technica Corporation), and the Hall effect was evaluated at room temperature to determine the carrier concentration and mobility.
[0196] (Crystallinity of the film)
[0197] The evaluation samples before and after the annealing A were evaluated. The crystallinity of the oxide film was evaluated by X-ray diffraction (XRD) measurement. The case where no peak was observed in the XRD measurement was judged as "amorphous", and the case where a peak was observed in the XRD measurement was judged as "crystalline". In addition, when a wide fine pattern was observed instead of a clear peak, it was set as "microcrystal".
[0198] In addition, the substance indicated as "crystal" was confirmed to be a crystalline substance having a bixbyite structure by evaluating an X-ray diffraction spectrum obtained by XRD measurement.
[0199] (Etching Characteristics)
[0200] The evaluation samples before annealing A were evaluated. The etching characteristics of the oxide film were evaluated by the taper angle. Specifically, a resist film patterned into lines and spaces of 1 mm was formed by a photolithography process on a substrate formed with an oxide film. A 4% oxalic acid aqueous solution was used to make the etching time 1.5 times the appropriate etching time, and the cross-section of the etched surface was observed by SEM to measure the etching angle.
[0201] (Hydrogen Atom Concentration)
[0202] The evaluation samples after the annealing C were evaluated using a quadrupole secondary ion mass spectrometer (D-SIMS manufactured by ULVAC-PHI) with a Cs ion source of 1 kV, a primary ion current of 100 nA, and a chamber vacuum of 5×10 -10 The measurement was performed under the measurement conditions of 10 torr. In order to eliminate the influence of the semiconductor film interface, the secondary ion intensity of H at each depth obtained by the quadrupole secondary ion mass spectrometer was integrated with the film thickness, the intensity was standardized using an In-O film with a known hydrogen concentration and film thickness, the hydrogen concentration was quantified, and the average value of the obtained values was taken as the hydrogen atomic concentration.
[0203] (TFT Characteristic Evaluation)
[0204] The linear mobility, threshold voltage (Vth), on / off ratio, and off current of the TFTs after the annealing A and the annealing C were evaluated.
[0205] The linear mobility is obtained from the transfer characteristics when a drain voltage of 0.1 V is applied. Specifically, a transfer characteristic Id-Vg graph is prepared, the transconductance (Gm) at each Vg is calculated, and the mobility is derived from the equation in the linear region. In addition, Gm is given by It means that Vg is applied within -15 to 25 V, and the maximum mobility within this range is defined as the linear mobility. The above Id is the current between the source and drain electrodes, and Vg is the gate voltage when the voltage Vd is applied between the source and drain electrodes.
[0206] The threshold voltage (Vth) is calculated from the transfer characteristic diagram with Id=10- 9 Vg is defined under A.
[0207] The on / off ratio is calculated by the ratio [on current value / off current value], where the value of Id at Vg=-10V is the off current value and the value of Id at Vg=20V is the on current value.
[0208] (Characteristics evaluation of high-speed response TFT)
[0209] The TFT after the above annealing C was evaluated.
[0210] The field effect mobility μ in the linear region is obtained from the transfer characteristics when a drain voltage of 0.1 V is applied. Specifically, a transfer characteristic Id-Vg graph is prepared, the transconductance (Gm) at each Vg is calculated, and the field effect mobility is derived from the equation in the linear region. Gm is given by Vg is applied from -15V to 20V, and the maximum mobility in this range is defined as field effect mobility. Id is the current between the source and drain electrodes, and Vg is the gate voltage when the voltage Vd is applied between the source and drain electrodes.
[0211] The field effect mobility at Vg=Vth(threshold voltage)+5(V) was obtained from the Vg-μ graph obtained by the field effect mobility method in the linear region. The average field effect mobility from Vg=Vth(V) to Vth+20(V) was obtained from the following formula.
[0212] [Number 1]
[0213] Average migration rate = ∫ Vth Vth+20 μdVg / 20
[0214] The field effect mobility of Vg = Vth + 5 (V) is 10 cm 2 A TFT having an average field effect mobility from Vg=Vth(V) to Vth+20(V) of at least 50% of the maximum field effect mobility in this range can be called a high-speed response TFT.
[0215] [Table 2]
[0216]
[0217] Examples 3-1 to 3-3
[0218] A semiconductor film (evaluation sample) and a semiconductor layer of a TFT were produced and evaluated in the same manner as in Example 2-1 except that the sputtering target produced in Example 1-2 was used and the film formation conditions shown in Table 3 were used.
[0219] [Table 3]
[0220]
[0221] Examples 4-1 to 4-3
[0222] Except that the sputtering target manufactured in Example 1-3 was used and the film forming conditions shown in Table 4 were set, a semiconductor film (evaluation sample) and a semiconductor layer of a TFT were manufactured and evaluated in the same manner as in Example 2-1. In addition, in Example 4-3, a pulsed DC sputtering method was used with a pulse frequency of 100 kHz and a duty cycle of 50%. The results are shown in Table 4.
[0223] [Table 4]
[0224]
[0225] * Example 4-3: Pulsed DC sputtering
[0226] Examples 5-1 to 5-3
[0227] Except that the sputtering target manufactured in Example 1-4 was used and the film forming conditions shown in Table 5 were set, a semiconductor film (evaluation sample) and a semiconductor layer of a TFT were manufactured and evaluated in the same manner as in Example 2-1. In addition, in Example 5-3, a pulsed DC sputtering method was used, the pulse frequency was set to 100 kHz, and the duty ratio was set to 50%. The results are shown in Table 5.
[0228] [Table 5]
[0229]
[0230] * Example 5-3: Pulsed DC sputtering
[0231] Examples 6-1 to 6-3
[0232] A semiconductor film (evaluation sample) and a semiconductor layer of a TFT were produced and evaluated in the same manner as in Example 2-1 except that the sputtering target produced in Example 1-5 was used and the film formation conditions shown in Table 6 were used.
[0233] [Table 6]
[0234]
[0235] Comparative Examples 2-1 to 2-3
[0236] A semiconductor film (evaluation sample) and a semiconductor layer of a TFT were produced and evaluated in the same manner as in Example 2-1 except that the sputtering target produced in Comparative Example 1-1 was used and the film formation conditions shown in Table 7 were used.
[0237] As in Comparative Example 2-1, when a target of high-purity indium oxide was used, the linear mobility of the TFT characteristics after annealing A at 300° C. was 30 cm 2 / V·, but after annealing at 350°C as a stabilization treatment (annealing C), the linear mobility decreased to 10 cm 2 / V·s.
[0238] [Table 7]
[0239]
[0240] Comparative Examples 3-1 to 3-4
[0241] A semiconductor film (evaluation sample) and a semiconductor layer of a TFT were produced and evaluated in the same manner as in Example 2-1 except that the sputtering target produced in Example 1-1 was used and the film formation conditions shown in Table 8 were used.
[0242] [Table 8]
[0243]
[0244] Figure 4 This is the transfer curve of the TFT produced in Example 2-1. Figure 5 This is a Vg-μ graph of the TFT produced in Example 2-1. Figure 6 This is the transfer curve of the TFT produced in Comparative Example 3-1. Figure 7 This is a Vg-μ graph of the TFT produced in Comparative Example 3-1.
[0245] Depend on Figure 4 and Figure 5It can be seen that the TFT formed with a semiconductor film by setting the partial pressure of water in the sputtering gas to 6% shows good performance. Figure 6 and Figure 7 It is found that when the film is formed in the absence of a hydrogen atom supply gas as in the comparative example, even if sputtering is performed in the presence of oxygen, the characteristics of the obtained TFT are inferior.
[0246] Although several embodiments and / or examples of the present invention described above have been described in detail, it is easy for those skilled in the art to add more changes to these exemplified embodiments and / or examples without departing from the novel teachings and effects of the present invention in substance. Therefore, these more changes are also included in the scope of the present invention.
[0247] The entire contents of all documents described in this specification and the applications on which the Paris Convention priority claim of the present application is based are cited herein.
Claims
1. A semiconductor film, It is characterized in that A solid phase crystallized material comprising indium oxide doped with tin and hydrogen.
2. The semiconductor film according to claim 1, It is characterized in that The content ratio of tin atoms (Sn) in the solid phase crystallized material to the total of indium atoms (In) and tin atoms (Sn) [Sn / (In+Sn): molar ratio] is 0.000005 to 0.008, The concentration of hydrogen atoms (H) measured by secondary ion mass spectrometry was 0.5×10 20 ~50×10 20 atoms / cc.
3. The semiconductor film according to claim 1 or 2, It is characterized in that The cross section is a tapered shape.
4. A method for manufacturing a semiconductor film according to any one of claims 1 to 3, It is characterized in that have: A step of forming an amorphous film by sputtering a tin-doped indium oxide (ITO) sputtering target in a film-forming gas containing a gas supplying hydrogen atoms at a partial pressure of 0.5 to 12%; The amorphous film is heated to be crystallized.
5. The manufacturing method according to claim 4, It is characterized in that The method comprises the step of processing the etched cross section into a tapered shape in a photolithography step after the step of forming the amorphous film.
6. A tin-doped indium oxide sputtering target, It is characterized in that The content ratio of tin atoms (Sn) to the total of indium atoms (In) and tin atoms (Sn) [Sn / (In+Sn): molar ratio] is 0.000005 to 0.008, and is used to form an amorphous film of indium oxide doped with tin and hydrogen.
7. A thin film transistor, It is characterized in that A semiconductor film comprising the semiconductor film according to any one of claims 1 to 3.