Preparation method of diversion absorption material
During the preparation process of the flow-drain absorbing material, hot melt adhesive and specific process parameters are used to form a fast flow-draining material layer structure, which solves the problems of slow down seepage speed and high return seepage amount of flow-draining material, and improves the product Yield and performance.
Patent Information
- Application Number
- CN202310549741.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-11-15
AI Technical Summary
The existing flow-guided absorbing materials have slow down in seepage, high in seepage after water absorption, and low yield during preparation, resulting in untimely water absorption and leakage, affecting production costs.
Combination is formed by spraying hot melt adhesive between the absorber layer and the fast-steering material layer and pressing at specific conveying speeds and pressures, combining specific layer structures and process parameters such as hot melt adhesive temperature, conveying speed and pressure to form a composite Materials ensure fast infiltration speed and low back seepage amount, while improving product yield.
The infiltration speed of the flow-guided absorbing material has been achieved, the back seepage amount after water absorption is low, and the product yield is no less than 96%, solving the problems of material performance and production efficiency in the prior art.
Smart Images

Figure CN118948531A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sanitary product materials, and in particular relates to a method for preparing a diversion absorption material. Background Art
[0002] Hygiene products materials with water absorption properties are widely used, for example, in baby diapers, sanitary napkins, etc. Existing sanitary products materials with water absorption properties can also be called diversion absorption materials, which are often composed of a multi-layer structure and have certain water absorption properties. However, the diversion absorption materials in the prior art often have the disadvantages of slow water infiltration speed and high re-infiltration after water absorption. This will cause untimely water absorption and water leakage. Moreover, the yield of this type of material in the prior art is not high during the preparation process, which is not conducive to reducing production costs.
[0003] Therefore, there is an urgent need to provide a new method for preparing a diversion absorbent material, so that the prepared diversion absorbent material has the characteristics of fast water infiltration speed and low re-infiltration after water absorption. Furthermore, it can also improve product yield and reduce production costs. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a method for preparing a diversion absorbent material. The diversion absorbent material prepared by the preparation method of the present invention has the advantages of fast water infiltration speed and low re-infiltration after water absorption, and the product prepared by the preparation method of the present invention has a high yield rate, which is not less than 96%.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0006] A method for preparing a diversion absorption material comprises the following steps:
[0007] (1) spraying hot melt adhesive onto the upper surface of the absorbent layer, then stacking a fast flow-guiding material layer on the absorbent layer, placing it in a first area for transmission, and then pressing it through a first pressing roller to obtain a composite intermediate;
[0008] (2) spraying hot melt adhesive on the lower surface of the skin-friendly layer and the upper surface of the waterproof layer, and then stacking the waterproof layer, the composite intermediate of step (1), and the skin-friendly layer in order from bottom to top, placing them in the second area for transmission, and then pressing them through a second pressing roller to obtain the diversion absorption material;
[0009] In step (1), the rapid flow-conducting material layer includes, from bottom to top, a lower layer, a connecting layer, and an upper layer;
[0010] The transmission speeds of the first area transmission and the second area transmission are both 50-500 m / min;
[0011] The pressure of the first pressing roller is 2-6 kgf / cm 2 The pressure of the second pressing roller is 2.5-6.5kgf / cm 2 ;
[0012] The temperature of the hot melt adhesive is 130-180°C.
[0013] The present invention coordinates various process parameters such as the transmission speed of the specific first area transmission, the transmission speed of the second area transmission, the pressure of the first pressing roller, the pressure of the second pressing roller, and the temperature of the hot melt adhesive, so that the prepared diversion absorption material has the advantages of fast water infiltration speed and low re-infiltration after water absorption, and the product yield prepared by the preparation method of the present invention is high, and the yield is not less than 96%. If the pressing pressure is too large, the layer structure is easily destroyed, resulting in a slow infiltration speed. If the pressing pressure is too small, the composite of each layer is not compact, which is manifested as low peeling force resulting in low yield and high re-infiltration. If the transmission speed is too fast, the production yield is too low, less than 90%, and it is not formed, offset, wrinkled, and cannot be cut, and the peeling force is too low. If the transmission speed is too slow, the local temperature and pressure are too high, which is also unfavorable to the infiltration speed and re-infiltration.
[0014] Preferably, the conveying speeds of the first zone conveying and the second zone conveying are both 100-400 m / min.
[0015] Preferably, the pressure of the first pressing roller is 4-6kgf / cm 2 The second roller is pressed at a pressure of 4.5-6.5kgf / cm 2 ;
[0016] Preferably, the temperature of the hot melt adhesive is 150-180°C.
[0017] Preferably, the connecting layer comprises polyester, and the fineness of the polyester in the connecting layer is 5-120D and / or 1-72F. D and F are two indicators for defining the fineness of polyester.
[0018] Preferably, the upper layer and the lower layer are composed of polyester, and the fineness of the polyester in the upper layer and the lower layer is 10-150D and / or 1-324F.
[0019] The fast-absorbing material layer is a sandwich air layer fabric structure consisting of an upper layer, a connecting layer and a lower layer. The connecting line of the connecting layer can provide excellent support and elasticity; the polyester fiber fineness of the connecting layer is 10-72D and / or 1-72F, providing excellent support and resilience. The polyester fiber fineness of the upper and lower layers is 30-120D and / or 1-324F, forming a permeable mesh and toughness, rapid permeation, anti-deformation and no caking, dry and not stuffy.
[0020] Preferably, the skin-friendly layer is hot air non-woven fabric.
[0021] Preferably, the absorption layer is a conventional absorption core, including any one of dust-free paper or small white paper wrapped with fluff pulp and polymer absorbent resin, polymer absorbent resin paper, and fluff pulp mixed with polymer absorbent resin.
[0022] Preferably, the waterproof layer is polyethylene.
[0023] Preferably, the thickness of the diversion absorption material obtained by the preparation method is 0.3-5 mm, and the gram weight is 50-500 g / m 2 Further preferably, the thickness of the diversion absorption material obtained by the preparation method is 2-5mm, and the gram weight is 100-450g / m 2 .
[0024] Preferably, after step (2) is completed, step (3) is further included, and the content of step (3) is as follows:
[0025] The back of the waterproof layer of the diversion absorbent material obtained in step (2) is coated with adhesive, release paper is added, the outer garment is wrapped and folded into a target shape, and an easy-tear sticker is added to obtain an absorbent product. The absorbent product is a finished sanitary product and can be sold and used.
[0026] A diversion absorption material is prepared by the above preparation method.
[0027] Preferably, the water absorption ratio of the diversion absorption material obtained by the preparation method is 1-12 times, for example, 1-10 times.
[0028] Preferably, the surface of the skin-friendly layer of the diversion and absorption material has patterns of different colors, such as dot patterns of different colors.
[0029] A sanitary product material comprises the above-mentioned diversion absorption material.
[0030] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0031] The present invention coordinates various process parameters such as the transmission speed of the specific first area transmission, the transmission speed of the second area transmission, the pressure of the first pressing roller, the pressure of the second pressing roller, and the temperature of the hot melt adhesive, so that the prepared diversion absorption material has the advantages of fast water infiltration speed and low re-infiltration after water absorption, and the product yield prepared by the preparation method of the present invention is high, and the yield is not less than 96%. If the pressing pressure is too large, the layer structure is easily destroyed, resulting in a slow infiltration speed. If the pressing pressure is too small, the composite of each layer is not compact, which is manifested as low peeling force resulting in low yield and high re-infiltration. If the transmission speed is too fast, the production yield is too low, less than 90%, and the product is not formed, offset, wrinkled, and cannot be cut, and the peeling force is too low. If the transmission speed is too slow, the local temperature and pressure are too high, which is also unfavorable to the infiltration speed and re-infiltration. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a schematic diagram of the structure of the diversion absorption material prepared in Example 1 of the present invention;
[0033] Figure 2 This is a schematic structural diagram of a rapid flow-guiding material layer in a flow-guiding absorption material prepared in Example 1 of the present invention;
[0034] Figure 3 This is a schematic diagram of a structure with pores formed by interweaving multiple coils in the upper layer or the lower layer of the rapid flow-conducting material layer in Example 1 of the present invention. DETAILED DESCRIPTION
[0035] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0036] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.
[0037] The instantaneous absorption time (corresponding to the infiltration rate in Table 2 of the present invention), the re-infiltration amount and the yield rate of the diversion absorption material were tested.
[0038] in,
[0039] The test method for instantaneous absorption time is carried out in accordance with the requirements of the national standard GB / T 8939-2018. Specifically, place the absorption speed tester in a horizontal position, pour enough standard synthetic test solution into the liquid storage tank, start the instrument, click the rinse button, and rinse twice. Calibrate the liquid filling volume of the automatic liquid filling device according to the instrument manual. Remove the arc sample holder on the absorption speed tester and place it on a horizontal table. Take a sample, tear off the bottom release paper, and gently stick it on the arc test area of the arc sample holder. When sticking, the front end of the sample is on the left (L) side of the arc sample holder, and the rear end is on the right (R) side of the arc sample holder. The center line of the wing (perpendicular to the towel body) is aligned with the corresponding line of the liquid outlet on the base. Stick the wing on both sides of the arc sample holder, and then place the arc sample holder with the sample on the fixed position of the absorption speed tester. Enter the test interface of the absorption speed tester and set the sample thickness to ensure that the standard test module can fall freely to the sample surface. Click the test button, and the automatic liquid adding device will add (2.0±0.1)mL of standard synthetic test solution into the standard test module. The timer will start timing automatically until the liquid level disappears at the lowest point of the absorption zone. The sample is placed horizontally, and a test module is placed on the sample surface. A drain funnel is set above the module. Take 2mL of standard solution and quickly inject the standard solution into the drain funnel (all the liquid will be squeezed out within 3 seconds). The timer records the time it takes for the sample to completely absorb the standard solution. It should be noted that at least 3 valid data are measured for each sample, and the result is expressed as the arithmetic mean of the test values of the 3 samples, in seconds (s).
[0040] The test method of back-seepage volume is carried out in accordance with the requirements of the national standard GB / T 28004-2011. Specifically: rinse the funnel twice with the test solution and fix the funnel on the bracket. Place several layers of φ230mm filter paper of known mass on the horizontal operating table, unfold the sample in a natural state (the two ends of the straight strip sample need to be tilted so that the test area length is about 200mm) and place it on the filter paper. Accurately measure the test solution with a dosage unit and pour it into the funnel. The lower opening of the funnel should be facing the operator, and the vertical distance between the center point of the lower opening and the sample surface is 5mm to 10mm. Then quickly open the funnel valve to the maximum, so that the test solution can flow freely to the surface of the sample, and start timing at the same time (the solution should not overflow from both sides of the sample during the test). After 5 minutes, inject the same amount of test solution with the funnel again. After 10 minutes, quickly put several layers of φ110mm filter paper of known mass (until the top layer of filter paper has no liquid absorption) on the surface of the sample, and press the standard pressure block on the filter paper at the same time, and restart the timing. After 1 minute of pressure, remove the standard pressure block and weigh the mass of the filter paper on the surface of the sample with a balance. The back-infiltration amount of the sample is expressed as the mass difference before and after the test of the filter paper on the surface of the sample, and is calculated as follows: m = m1-m2; in the formula, m is the back-infiltration amount, in grams (g); m1 is the mass of the filter paper on the surface of the sample after absorbing liquid, in grams (g); m2 is the mass of the filter paper on the surface of the sample before absorbing liquid, in grams (g). Take the arithmetic mean of the test results of the three samples as the test result, accurate to 0.1g.
[0041] The test method for good products is based on statistics from 10,000 products produced on the production line, assisted by a visual stain inspection system. Products with wrinkles, offsets, curling, or incomplete separation of edges and slots in the guide and absorbent materials are considered defective products.
[0042] The D number refers to the mass in grams of a 9000m long fiber at the specified moisture regain; the F number refers to the number of microfibers in a fiber.
[0043] Example 1
[0044] A diversion absorption material, the structure from bottom to top is: a waterproof layer, an absorption layer, a rapid diversion material layer, and a skin-friendly layer;
[0045] The rapid flow-conducting material layer is composed of a lower layer, a connecting layer and an upper layer from bottom to top.
[0046] Figure 1 This is a schematic diagram of the structure of the diversion absorption material prepared in Example 1 of the present invention; Figure 1 100 represents the waterproof layer, 200 represents the absorption layer, 300 represents the fast diversion material layer, and 400 represents the skin-friendly layer.
[0047] Figure 2This is a schematic structural diagram of a rapid flow-guiding material layer in a flow-guiding absorption material prepared in Example 1 of the present invention; Figure 2 In the figure, 310 indicates a lower layer, 320 indicates a connection layer, and 330 indicates an upper layer.
[0048] Figure 3 This is a schematic diagram of a structure with pores formed by interweaving multiple coils in the upper layer or the lower layer of the rapid flow-conducting material layer in Example 1 of the present invention.
[0049] A method for preparing a diversion absorption material comprises the following steps:
[0050] (1) spraying hot melt adhesive onto the upper surface of the absorbent layer, then stacking a fast flow-guiding material layer on the absorbent layer, placing it in a first area for transmission, and then pressing it through a first pressing roller to obtain a composite intermediate;
[0051] (2) spraying hot melt adhesive on the lower surface of the skin-friendly layer and the upper surface of the waterproof layer, and then stacking the waterproof layer, the composite intermediate of step (1), and the skin-friendly layer in order from bottom to top, placing them in the second area for transmission, and then pressing them through a second pressing roller to obtain a diversion absorption material;
[0052] The transmission speed of the first area transmission and the second area transmission is 50m / min;
[0053] The first pressing roller applies a pressing pressure of 2 kgf / cm 2 The second roller is pressed at a pressure of 2.5 kgf / cm 2 ;
[0054] The temperature of the hot melt adhesive is 130°C.
[0055] In step (1), the rapid flow-guiding material layers are, from bottom to top, a lower layer, a connecting layer, and an upper layer;
[0056] The connecting layer is composed of polyester, and the fineness of the polyester in the connecting layer is 75D, 36F.
[0057] The upper layer and the lower layer are composed of polyester, and the fineness of the polyester in the upper layer and the lower layer is 150D, 36F.
[0058] The skin-friendly layer is hot air non-woven fabric.
[0059] The absorption layer is a conventional absorption core, which is a small white paper wrapped fluff pulp and Sumitomo 60N high molecular water-absorbent resin (weight 88gsm).
[0060] The waterproof layer is polyethylene.
[0061] The thickness of the diversion absorption material obtained by the preparation method is 2 mm.
[0062] The manufacturing method of the upper layer or the lower layer of the rapid diversion material layer is as follows:
[0063] It is made of coils interwoven vertically and horizontally, in which the upper and lower layers are looped in the horizontal weft direction and interwoven layer by layer to form a plane with continuous pores, thereby forming the upper and lower layers;
[0064] The process of coil interweaving is as follows:
[0065] 1. At the beginning, the loop is in the needle hook. When the needle starts to rise, the loop opens the needle tongue and slides into the needle bar.
[0066] 2. The knitting needle continues to rise until the loop is completely separated from the needle latch;
[0067] 3. When the knitting needle rises to a certain level and starts to move downward, the yarn is fed into the hook;
[0068] 4. As the knitting needle continues to move downward, the old coil rises relatively and closes the needle tongue, pulling the fed yarn into an arc. Finally, because the needle tongue is closed, the needle hook slides out of the old coil and passes the introduced yarn through the old coil to form a new coil, thus completing the criss-crossing interweaving of the coils.
[0069] The only difference between Examples 2-9 and Comparative Examples 1-4 and Example 1 is that the hot melt adhesive temperature, the conveying speed of the first area conveying and the second area conveying, the pressing pressure of the first pressing roller, and the pressing pressure of the second pressing roller are changed. The specific process parameters are shown in Table 1.
[0070] Table 1
[0071]
[0072]
[0073] The performance parameters of the water infiltration rate, re-infiltration amount and yield rate of the diversion and absorption materials prepared in the above-mentioned Examples 1-9 and Comparative Examples 1-4 are shown in Table 2.
[0074] Table 2
[0075] Infiltration rate (s) Re-seepage amount (g) Yield rate (%) Example 1 3.4 1.3 96 Example 2 2.5 1.8 97 Example 3 1.8 2.6 96 Example 4 3.8 0.9 98 Example 5 2.7 1.2 96 Example 6 1.9 2.4 97 Example 7 4.8 0.7 99 Example 8 3.3 1 98 Example 9 2.3 2.1 95 Comparative Example 1 10.9 1.2 96 Comparative Example 2 1.7 4.2 85 Comparative Example 3 11.3 3.8 95 Comparative Example 4 12.1 4.1 95
[0076] It can be seen from Table 2 that the process parameters such as the hot melt adhesive temperature, the transmission speed of the first area transmission and the second area transmission, the pressing pressure of the first pressing roller, and the pressing pressure of the second pressing roller have a significant impact on the water infiltration rate, re-infiltration amount, and yield rate performance of the diversion absorbent material. Only within the specific process parameter range of the present invention can the water infiltration rate, re-infiltration amount, and yield rate performance of the prepared diversion absorbent material meet the requirements at the same time.
[0077] Example 10
[0078] Compared with Example 1, the only difference of Example 10 is that the upper and lower layers of the fast diversion material layer are composed of polyester, and the fineness of the polyester in the upper and lower layers is 200D and 324F. The infiltration speed and re-infiltration amount of the diversion absorption material prepared in Example 10 are 5.2s and 2.3g respectively.
Claims
1. A method for preparing a diversion absorption material, characterized in that: The following steps are involved: (1) spraying hot melt adhesive onto the upper surface of the absorbent layer, then stacking a fast flow-guiding material layer on the absorbent layer, placing it in a first area for transmission, and then pressing it through a first pressing roller to obtain a composite intermediate; (2) spraying hot melt adhesive on the lower surface of the skin-friendly layer and the upper surface of the waterproof layer, and then stacking the waterproof layer, the composite intermediate of step (1), and the skin-friendly layer in order from bottom to top, placing them in the second area for transmission, and then pressing them through a second pressing roller to obtain the diversion absorption material; In step (1), the rapid flow-conducting material layer includes, from bottom to top, a lower layer, a connecting layer, and an upper layer; The transmission speeds of the first area transmission and the second area transmission are both 50-500 m / min; The pressure of the first pressing roller is 2-6 kgf / cm 2 The pressure of the second pressing roller is 2.5-6.5kgf / cm 2 ; The temperature of the hot melt adhesive is 130-180°C.
2. The preparation method according to claim 1, characterized in that: The conveying speeds of the first area conveying and the second area conveying are both 100-400 m / min.
3. The preparation method according to claim 1, characterized in that: The pressure of the first pressing roller is 4-6 kgf / cm 2 The second roller is pressed at a pressure of 4.5-6.5kgf / cm 2 .
4. The preparation method according to claim 1, characterized in that: The temperature of the hot melt adhesive is 150-180°C.
5. The preparation method according to claim 1, characterized in that: The connecting layer is composed of polyester, and the fineness of the polyester in the connecting layer is 5-120D and / or 1-72F.
6. The preparation method according to claim 1, characterized in that: The upper layer and the lower layer are composed of polyester, and the fineness of the polyester in the upper layer and the lower layer is 10-150D and / or 1-324F.
7. The preparation method according to claim 1, characterized in that: The diversion absorption material prepared by the preparation method has a thickness of 0.3-5 mm and a gram weight of 50-500 g / m 2 .
8. The preparation method according to any one of claims 1 to 7, characterized in that: After step (2) is completed, step (3) is also included. The content of step (3) is as follows: The back of the waterproof layer of the diversion absorbent material obtained in step (2) is coated with adhesive, release paper is added, the outer garment is wrapped and folded, and an easy-tear sticker is added to obtain an absorbent product.
9. A diversion absorption material, characterized in that: Prepared by the above preparation method.
10. A sanitary product material, characterized in that: The invention comprises the diversion and absorption material as claimed in claim 9.