Preparation method of methanol synthesis catalyst with highly dispersed graphite

By adding graphite and ethanol to the co-precipitation process of the catalyst, the problem of low dispersion uniformity of graphite is solved, the performance of the catalyst and methanol synthesis efficiency are improved, the defect of graphite failure at high temperature is avoided, and the efficient production of catalysts is achieved .

CN118950002APending Publication Date: 2024-11-15ANHUI CONCH IND TECHNOLOGY RESEARCH INSTITUTE CO LTD

Patent Information

Application Number
CN202410996681.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The graphite dispersion uniformity in existing methanol synthesis catalysts is low, resulting in poor catalytic performance and graphite fails to burn at high temperatures, affecting the performance and structure of the catalyst.

Method used

Add graphite and ethanol to the aqueous solution of copper, zinc and aluminum salts, and disperse graphite naturally and uniformly in the catalyst precursor through co-precipitation reaction, avoid mechanical mixing, improve the dispersion and thermal conductivity of graphite, and promote the separation of catalyst particles and Increased surface area.

Benefits of technology

The highly uniform dispersion of graphite in the catalyst is achieved, the catalytic performance and methanol spatiotemporal yield are improved, side reactions and hot spots are reduced, and the service life of the catalyst is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950002A_ABST
    Figure CN118950002A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a methanol synthesis catalyst with highly dispersed graphite, which comprises the following steps: adding graphite and ethanol into an aqueous solution of copper salt, zinc salt and aluminum salt, and uniformly mixing to obtain a solution A; adding graphite and ethanol into an aqueous solution of alkali, and uniformly mixing to obtain a solution B; mixing the solution A and the solution B, carrying out a co-precipitation reaction, and aging a co-precipitation reaction product; and filtering the aged co-precipitation reaction product to obtain a precipitate, washing, drying, roasting, and carrying out compression molding to obtain the catalyst. The graphite is successfully dispersed and added in the coprecipitation process, so that the influence of harmful impurities in the graphite on the performance of the catalyst is avoided, and the methanol production catalytic performance of the catalyst is effectively improved. The copper-based catalyst particles in the prepared catalyst are small, no agglomeration phenomenon exists, and the catalyst has the high methanol space time yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a catalyst, in particular to a method for preparing a methanol synthesis catalyst with highly dispersed graphite. Background Art

[0002] The widely used methanol synthesis catalyst is a copper-based catalyst prepared by coprecipitation. Although the prior art attempts to introduce various components into it to improve performance, it will also bring unknown adverse factors. Therefore, it is generally recognized that the effective components are CuO, ZnO and Al2O3. The prior art continuously optimizes the formula and production process around the above components and develops catalysts with their own characteristics. In addition to the above components, graphite is usually added to the catalyst by mechanical mixing after roasting and before molding to play a lubricating and demolding role. This graphite addition method has the following disadvantages: First, as a natural mineral, graphite contains impurities such as CaO, MgO, and P2O5, which will degrade the catalyst performance to a certain extent. Second, if the mechanical mixing time is too short, the mixing is uneven, and if it is too long, the energy consumption increases and the catalyst structure may be destroyed. Third, mechanical mixing can only disperse graphite to a certain extent, and it is not necessary to disperse graphite highly evenly for demolding. It only needs to be coated on the surface of the catalyst particles after sintering. Therefore, the graphite dispersion uniformity in the existing catalyst is low, and it will not have a significant impact on the performance of the catalyst. Fourth, since the purpose of adding graphite is to lubricate and demold, graphite is added after the catalyst is sintered and does not participate in the co-precipitation step of the catalyst. It will not affect the microscopic particle structure of the catalyst, and thus will not affect the catalytic performance of the catalyst. Moreover, since graphite will burn at high temperatures, the subsequent high-temperature sintering step may cause the graphite to burn and fail. Fifth, graphite has poor dispersibility in aqueous solution and tends to float on the surface of the aqueous solution, while the co-precipitation reaction occurs inside the aqueous solution. Therefore, it is difficult to evenly disperse graphite in the catalyst through an aqueous solution-based co-precipitation step. Summary of the invention

[0003] Purpose of the invention: The purpose of the present invention is to provide a method for preparing a methanol synthesis catalyst, and to solve the problem of how to apply graphite to the coprecipitation step to prepare a methanol synthesis catalyst.

[0004] Technical solution: The method for preparing a methanol synthesis catalyst according to the present invention comprises the following steps:

[0005] (1) adding graphite and ethanol to an aqueous solution of copper salt, zinc salt and aluminum salt, and mixing them to obtain liquid A;

[0006] (2) adding graphite and ethanol to an alkaline aqueous solution and mixing well to obtain liquid B;

[0007] (3) mixing solution A and solution B to perform a coprecipitation reaction, and aging the coprecipitation reaction product;

[0008] (4) The aged coprecipitation reaction product is filtered to obtain the precipitate, which is then washed, dried, calcined, and pressed into a catalyst.

[0009] The present invention utilizes an appropriate amount of ethanol to promote the graphite to be uniformly dispersed in an aqueous solution of copper salt, zinc salt and aluminum salt and an aqueous solution of alkali, and the graphite is naturally and uniformly dispersed in the catalyst precursor precipitation during the coprecipitation reaction without mechanical dispersion. The graphite highly uniformly dispersed in the catalyst precursor can separate the catalyst particles formed by the coprecipitation, prevent the catalyst particles from agglomerating, increase the specific surface area, and thus improve the catalytic performance. In addition, the graphite also has good thermal conductivity. The graphite highly dispersed in the catalyst can quickly transfer the reaction heat generated by the methanol synthesis reaction, prevent the catalyst from generating hot spots, and reduce the occurrence of side reactions and the sintering of the catalyst.

[0010] Preferably, in step (1), the mass ratio of graphite to ethanol is 0.8-3.1:80-120; and in step (2), the mass ratio of graphite to ethanol is 0.265-2.65:80-120.

[0011] The right amount of ethanol can not only promote the dispersion of graphite in aqueous solution, but also promote the high dispersion of graphite in the catalyst through coprecipitation reaction. However, too much ethanol will hinder the coprecipitation reaction, resulting in a low yield of catalyst precursor. Too little ethanol cannot fully promote the dispersion of graphite. Therefore, the catalyst performance can be effectively improved by finding a suitable ratio of graphite to ethanol.

[0012] Preferably, in step (1), the molar ratio of Cu:Zn:Al in the aqueous solution of copper salt, zinc salt and aluminum salt is 0.48-10:0.6-4:1, and the amount of graphite added is 1-10% of the total weight of copper salt, zinc salt and aluminum salt.

[0013] Preferably, in step (1), the copper salt includes at least one of copper nitrate, copper acetate and copper acetylacetonate; the zinc salt includes at least one of zinc nitrate, zinc acetate and zinc acetylacetonate; and the aluminum salt includes at least one of aluminum nitrate, aluminum acetate and aluminum acetylacetonate.

[0014] Preferably, in step (2), the base comprises one or more of sodium carbonate, potassium carbonate, ammonium carbonate, sodium bicarbonate, potassium bicarbonate, ammonium bicarbonate, sodium hydroxide, potassium hydroxide, and aqueous ammonia.

[0015] Preferably, in step (2), the amount of graphite added is 1-10% by weight of the alkali.

[0016] Preferably, in step (3), the conditions of the coprecipitation reaction are that the pH of the coprecipitation process or the end point is controlled between 6.0-7.5, the temperature is controlled between 60-90° C., and the aging time is 0-2 h.

[0017] Preferably, in step (4), the drying temperature is 70-180° C., and the calcination method is calcination at 300-350° C. for 1-5 h in an inert atmosphere or in a flowing air atmosphere.

[0018] The inert atmosphere in the above calcination method creates an oxygen-free environment, mainly to prevent the graphite from burning out during the calcination process. The flowing air atmosphere is mainly to prevent the catalyst from being overheated locally and causing the graphite to burn, and to promote uniform heat distribution.

[0019] Preferably, the inert atmosphere is formed by filling N2, Ar, He, or CO2 gas, and the air velocity of the flowing air atmosphere is not less than 300 liters per liter of catalyst per hour.

[0020] Preferably, in step (4), the washing method is to use deionized water to wash the precipitate until the metal cations or ammonium ions are completely removed, such as sodium ions, potassium ions, magnesium ions, calcium ions, etc. The washing process helps to remove components in the graphite that are harmful to the catalyst.

[0021] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:

[0022] The present invention successfully disperses and adds graphite during the coprecipitation process, avoids the influence of harmful impurities in the graphite on the catalyst performance, and effectively improves the catalyst's methanol production catalytic performance. The copper-based catalyst particles in the catalyst prepared by the present invention are small, have no agglomeration phenomenon, and have a high methanol space-time yield. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is the SEM image of the catalyst prepared in Example 1. DETAILED DESCRIPTION

[0024] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0025] Example 1: A method for preparing a methanol synthesis catalyst is as follows:

[0026] Weigh 0.15 mol of copper nitrate trihydrate, 0.09 mol of zinc acetate dihydrate, and 0.025 mol of aluminum nitrate nonahydrate, add 150 g of deionized water and stir to dissolve, then add 3.1 g of graphite with a particle size of less than 50 microns and 100 g of ethanol, and mix thoroughly to obtain salt solution A.

[0027] Weigh 0.25 mol of sodium carbonate, 0.56 g of graphite, and 100 g of ethanol, add 200 g of deionized water, stir to dissolve, and obtain alkaline solution B.

[0028] Heat the alkaline solution B to 70°C, add the salt solution A to the alkaline solution B while stirring, and maintain the reaction temperature at 70°C. When the pH drops to 6.5, stop adding the salt solution A, and maintain aging at 70°C for 1 hour.

[0029] The aged product was filtered and the filter cake was washed with deionized water until no Na + The filter cake was dried at 110°C for 12 hours, and then calcined at 330°C for 3 hours under flowing air, with the air velocity of the air flow not less than 300 liters per liter of catalyst per hour. Finally, it was molded into a cylinder with a diameter of 5 mm and a height of 5 mm to obtain catalyst sample 1, as shown in FIG. Figure 1 shown.

[0030] Example 2: A method for preparing a methanol synthesis catalyst is as follows:

[0031] Weigh 0.012 mol of copper nitrate trihydrate, 0.015 mol of zinc acetate dihydrate, and 0.025 mol of aluminum nitrate nonahydrate, add 150 g of deionized water and stir to dissolve, then add 1.5 g of graphite with a particle size of less than 75 microns and 80 g of ethanol, and mix thoroughly to obtain salt solution A.

[0032] Weigh 0.1 mol of sodium carbonate, 1.06 g of graphite, and 80 g of ethanol, add 200 g of deionized water, stir and dissolve to obtain alkaline solution B.

[0033] Heat the alkaline solution B to 70° C., add the salt solution A to the alkaline solution B while stirring, and maintain the reaction temperature at 70° C. When the pH drops to 6.5, stop adding the salt solution A, and maintain aging at 70° C. for 0.5 hour.

[0034] The aged product was filtered and the filter cake was washed with deionized water until no Na + The filter cake was dried at 100°C for 8 hours and then calcined at 330°C for 3 hours in a nitrogen atmosphere. Finally, it was molded into a cylinder with a diameter of 5 mm and a height of 5 mm to obtain catalyst sample 2.

[0035] Example 3: A method for preparing a methanol synthesis catalyst is as follows:

[0036] Weigh 0.25 mol of copper acetate monohydrate, 0.1 mol of zinc acetate dihydrate, and 0.025 mol of aluminum nitrate nonahydrate, add 150 g of deionized water and stir to dissolve, then add 0.881 g of graphite with a particle size of less than 50 microns and 120 g of ethanol, and mix thoroughly to obtain salt solution A.

[0037] Weigh 0.75 mol of sodium carbonate, 0.32 g of graphite, and 120 g of ethanol, add 200 g of deionized water, stir to dissolve, and obtain alkaline solution B.

[0038] Heat the alkaline solution B to 80° C., add the salt solution A to the alkaline solution B while stirring, and maintain the reaction temperature at 80° C. When the pH drops to 7.0, stop adding the salt solution A, and maintain aging at 80° C. for 1.5 hours.

[0039] The aged product was filtered and the filter cake was washed with deionized water until no Na + The filter cake was dried at 180°C for 3 hours, and then calcined at 330°C for 3 hours in a helium atmosphere. Finally, it was molded into a cylinder with a diameter of 5 mm and a height of 5 mm to obtain catalyst sample 3.

[0040] Example 4: A method for preparing a methanol synthesis catalyst is as follows:

[0041] Weigh 0.012 mol of copper acetate monohydrate, 0.1 mol of zinc acetylacetonate monohydrate, and 0.025 mol of aluminum acetylacetonate, add 150 g of deionized water and stir to dissolve, then add 1.5 g of graphite and 120 g of ethanol, and mix thoroughly to obtain salt solution A.

[0042] Weigh 0.2 mol of sodium bicarbonate, 0.265 g of graphite with a particle size of less than 50 microns, and 100 g of ethanol, add 200 g of deionized water, stir and dissolve, and obtain alkaline solution B.

[0043] Heat the alkaline solution B to 60° C., add the salt solution A to the alkaline solution B while stirring, and maintain the reaction temperature at 60° C. When the pH drops to 6.0, stop adding the salt solution A, and maintain aging at 60° C. for 2 hours.

[0044] The aged product was filtered and the filter cake was washed with deionized water until no Na + The filter cake was dried at 70°C for 12 hours and then calcined at 300°C for 5 hours in an argon atmosphere. Finally, it was molded into a cylinder with a diameter of 5 mm and a height of 5 mm to obtain catalyst sample 4.

[0045] Example 5: A method for preparing a methanol synthesis catalyst is as follows:

[0046] Weigh 0.25 mol of copper acetylacetonate, 0.015 mol of zinc nitrate hexahydrate, and 0.025 mol of aluminum acetate, add 150 g of deionized water and stir to dissolve, then add 3.1 g of graphite with a particle size of less than 50 microns and 100 g of ethanol, and mix thoroughly to obtain salt solution A.

[0047] Weigh 0.5 mol of potassium carbonate, 0.56 g of graphite, and 80 g of ethanol, add 200 g of deionized water, stir and dissolve to obtain alkaline solution B.

[0048] Heat the alkaline solution B to 90° C., add the salt solution A to the alkaline solution B while stirring, and maintain the reaction temperature at 90° C. When the pH drops to 7.5, stop adding the salt solution A, and maintain aging at 90° C. for 0.1 hour.

[0049] The aged product was filtered and the filter cake was washed with deionized water until no K was detected. + The filter cake was dried at 150°C for 10 hours and then calcined at 350°C for 1 hour in a carbon dioxide atmosphere. Finally, it was molded into a cylinder with a diameter of 5 mm and a height of 5 mm to obtain catalyst sample 5.

[0050] Embodiment 6: The rest is the same as Embodiment 1, except that:

[0051] Sodium carbonate was replaced by ammonium carbonate to obtain catalyst sample 6.

[0052] Embodiment 7: The rest is the same as Embodiment 1, except that:

[0053] Sodium carbonate was replaced by ammonium bicarbonate to obtain catalyst sample 7.

[0054] Embodiment 8: The rest is the same as Embodiment 2, except that:

[0055] Sodium carbonate was replaced by sodium hydroxide to obtain catalyst sample 8.

[0056] Embodiment 9: The rest is the same as Embodiment 2, except that:

[0057] Sodium carbonate was replaced by potassium hydroxide to obtain catalyst sample 9.

[0058] Embodiment 10: The rest is the same as Embodiment 1, except that:

[0059] Different catalyst samples were prepared with the weight of ethanol in salt solution A as a variable.

[0060] Comparative Example 1: The rest is the same as Example 1, except that:

[0061] The catalyst was prepared without adding graphite and ethanol during the preparation of salt solution A and alkaline solution B.

[0062] Comparative Example 2: The rest is the same as Example 1, except that:

[0063] No graphite and ethanol were added during the preparation of salt solution A and alkaline solution B. 3.66 g of graphite was mixed with the calcined product by mechanical stirring for 2 h to prepare a catalyst.

[0064] Comparative Example 3: The rest is the same as Example 1, except that:

[0065] When preparing salt solution A and alkaline solution B, only graphite is added without adding ethanol.

[0066] Comparative Example 4: The rest is the same as Example 1, except that:

[0067] Ethanol was replaced with isopropanol.

[0068] Comparative Example 5: The rest is the same as Example 1, except that:

[0069] Ethanol was replaced with 1,4-butanediol.

[0070] Comparative Example 6: The rest is the same as Example 1, except that:

[0071] The ethanol was replaced with glycerol.

[0072] The samples prepared in Test Examples 1-10 and Comparative Examples 1-7 were:

[0073] 1. Catalytic performance test: The catalyst was tested for activity using a fixed bed high pressure microreactor, and the product composition was analyzed by gas chromatograph to calculate the selectivity of the reaction and the space-time yield of methanol. The three catalyst samples of the embodiment and the comparative example were crushed, passed through a 40-80 mesh sieve, and then 0.1 g was weighed and mixed with 0.4 g of quartz sand and loaded into a fixed bed reactor. Before the activity test, the catalyst was subjected to in-situ temperature reduction in an atmosphere of 20% H2-80% Ar by volume, and reduced at 250°C for 1 hour.

[0074] Reaction conditions for methanol synthesis: reaction pressure 2.0 MPa, reaction temperature 220°C, space velocity 24000 h -1 ;

[0075] The volume composition of the raw gas is: CO2=24%, Ar=4%, and the rest is H2.

[0076] 2. Filtration time test: During the filtration and washing process, after a stable filter cake is formed, the time it takes for 500 mL of washing water to pass through the filter cake is tested and recorded as the filtration time.

[0077] 3. Catalyst resistance test: Use a multimeter to test the resistance values ​​of different particles in the cylindrical catalyst.

[0078] The test results are as follows:

[0079] Table 1 Performance test results of catalysts prepared by different methods and raw materials

[0080]

[0081] By comparing the filtration time of sample 1, comparative example 1 and comparative example 2, it can be seen that adding graphite during the precipitation process can play the role of a filtration structure aid, increase the filtration speed, reduce the filtration time, and improve the catalyst production efficiency.

[0082] Copper oxide, zinc oxide, aluminum oxide and other oxides in the catalyst are not conductors, so the conductivity in the catalyst is mainly contributed by graphite. Comparing the resistance values ​​of sample 1, comparative example 1 and comparative example 2, it can be seen that the resistance value of sample 1 is small and the resistance values ​​of different particles are close, indicating that the graphite in the catalyst prepared by the present invention has the characteristics of uniform and highly dispersed. However, the graphite in the catalyst prepared by mechanical mixing is unevenly distributed, and the resistance values ​​of different particles are quite different.

[0083] In addition to being conductive, graphite also has good thermal conductivity, which can quickly transfer the heat of reaction generated by methanol synthesis, prevent the catalyst from generating hot spots, and reduce the occurrence of side reactions and catalyst sintering. In addition, adding graphite during the precipitation process can separate copper-based catalyst particles and prevent the particles from agglomerating and growing, thus achieving a higher methanol space-time yield.

[0084] Comparative Example 3 shows that without the help of ethanol, graphite is difficult to disperse into the co-precipitation product during the co-precipitation process, resulting in a significant increase in the resistance value of the catalyst, and due to the lack of the help of graphite, the catalytic performance of the catalyst product also decreased.

[0085] Comparative Examples 4-6 show that although other alcohols can theoretically solve the problem of poor graphite dispersibility and promote the dispersion of graphite in aqueous solution, these alcohols may affect the coprecipitation reaction system, resulting in uneven coprecipitation products or agglomeration, and ultimately leading to a decrease in catalyst performance.

[0086] Since graphite is added during the precipitation process, the washing process after precipitation helps to remove catalyst-harmful components such as MgO, CaO, and P2O5 in the graphite. Therefore, the methanol selectivity of sample 1 is higher, which can reduce the waste of raw materials and the cost of subsequent separation and purification.

[0087] The test results of Example 10 are as follows:

[0088] Table 2 Effect of the weight ratio of graphite to ethanol on catalyst performance

[0089]

[0090] It can be seen from the results in Table 2 that when the amount of ethanol added is too little or too much, the graphite cannot be evenly distributed in the catalyst. Only in the range of 3.1:80-120 can the graphite be evenly dispersed and the effect of ethanol on the coprecipitation reaction be minimized, thereby effectively improving the catalytic production performance of the catalyst.

Claims

1. A method for preparing a methanol synthesis catalyst, characterized in that: The steps include: (1) adding graphite and ethanol to an aqueous solution of copper salt, zinc salt and aluminum salt, and mixing them to obtain liquid A; (2) adding graphite and ethanol to an alkaline aqueous solution and mixing well to obtain liquid B; (3) mixing solution A and solution B to perform a coprecipitation reaction, and aging the coprecipitation reaction product; (4) The aged coprecipitation reaction product is filtered to obtain the precipitate, which is then washed, dried, calcined, and pressed into a catalyst.

2. The method for preparing the methanol synthesis catalyst according to claim 1, characterized in that: In step (1), the mass ratio of graphite to ethanol is 0.8-3.1:80-120; in step (2), the mass ratio of graphite to ethanol is 0.265-2.65:80-120.

3. The method for preparing the methanol synthesis catalyst according to claim 1, characterized in that: In step (1), the molar ratio of Cu:Zn:Al in the aqueous solution of copper salt, zinc salt and aluminum salt is 0.48-10:0.6-4:1, and the added amount of graphite is 1-10% of the total weight of copper salt, zinc salt and aluminum salt.

4. The method for preparing the methanol synthesis catalyst according to claim 1, characterized in that: In step (1), the copper salt includes at least one of copper nitrate, copper acetate, and copper acetylacetonate; the zinc salt includes at least one of zinc nitrate, zinc acetate, and zinc acetylacetonate; and the aluminum salt includes at least one of aluminum nitrate, aluminum acetate, and aluminum acetylacetonate.

5. The method for preparing the methanol synthesis catalyst according to claim 1, characterized in that: In step (2), the base includes one or more of sodium carbonate, potassium carbonate, ammonium carbonate, sodium bicarbonate, potassium bicarbonate, ammonium bicarbonate, sodium hydroxide, potassium hydroxide, and aqueous ammonia.

6. The method for preparing the methanol synthesis catalyst according to claim 1, characterized in that: In step (2), the amount of graphite added is 1-10% of the weight of the alkali.

7. The method for preparing the methanol synthesis catalyst according to claim 1, characterized in that: In step (3), the conditions of the coprecipitation reaction are that the pH of the coprecipitation process or the end point is controlled between 6.0-7.5, the temperature is controlled between 60-90° C., and the aging time is 0-2 h.

8. The method for preparing the methanol synthesis catalyst according to claim 1, characterized in that: In step (4), the drying temperature is 70-180° C., and the calcination method is calcination at 300-350° C. for 1-5 h in an inert atmosphere or in a flowing air atmosphere.

9. The method for preparing the methanol synthesis catalyst according to claim 8, characterized in that: The inert atmosphere is formed by filling N2, Ar, He, and CO2 gases, and the air velocity of the flowing air atmosphere is not less than 300 liters per liter of catalyst per hour.

10. The method for preparing a methanol synthesis catalyst according to claim 1, characterized in that: In step (4), the washing method is to use deionized water to wash the precipitate until the metal cations or ammonium ions are completely removed.

Citation Information

Patent Citations

  • Method for preparing high-performance methanol synthesis catalyst through high-temperature roasting

    CN111036216A

  • Preparation method of high-stability methanol synthesis catalyst

    CN112221509A

  • Preparation method of high-activity methanol synthesis catalyst

    CN112237916A

  • N-doped graphite modified methanol synthesis catalyst and preparation method thereof

    CN116943698A

  • Modified catalyst for producing methanol by catalytic hydrogenation of carbon dioxide and method for preparing same

    WO2012151776A1

Cited By

  • Copper-zinc-aluminum-alkylated graphite carbon combined catalyst as well as preparation method and application thereof

    CN121042002A

  • Methanol synthesis catalyst and preparation method thereof

    CN122209397A

  • Graphite modified catalyst for preparing methanol from mixed gas and preparation method of graphite modified catalyst

    CN122625213A