Method for recovering barite from oil-based drilling cuttings through combination of roasting, flotation and strong magnetic separation
Through the combined process of roasting-flotation-strong magnetic separation, the problem of barite in oil-based drilling rock chips was solved, efficient separation and resource recycling were achieved, environmental pollution was reduced, and high-precision ore was obtained Grade and low tailings pollution effects.
Patent Information
- Application Number
- CN202411154996.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-15
AI Technical Summary
Oil-based drilling rock chips are generated during shale gas drilling and mining. If directly discharged or simply landfill, it will cause serious pollution, pose a threat to the environment and human health. The valuable components in it are such as petroleum hydrocarbon mineral oil and barcrystalline. The stone was not effectively recycled.
By using the combined process of roasting-flotation-strong magnetic separation, the sieving, roasting, multiple flotation and strong magnetic separation, the barite is gradually separated and recovered, and the influence of petroleum hydrocarbons is eliminated by roasting, and the barite is separated by flotation. , and remove black mica through strong magnetic separation to improve concentrate grade.
The efficient recycling of barite has been achieved, the content of concentrate barite has reached 91.30%, and the yield is 27.47%. The tailings pollutant indicator has been reduced to below the industry standard, and the resource recycling and harmless treatment have been achieved, which has reduced the Environmental pollution.
Smart Images

Figure CN118950239A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mineral processing, and in particular relates to a method for recovering barite from oil-based drilling cuttings by combined roasting-flotation-high-intensity magnetic separation. Background Art
[0002] Oil-based drilling cuttings are solid waste generated during the shale gas drilling process. Their basic components are petroleum hydrocarbon mineral oils, mud weighting agents (barytes), rock fragments brought out by drilling mud, and various chemical additives added to the drilling mud. These components constitute a complex multiphase system. The mineral oil, phenolic compounds and heavy metals contained in them, if directly discharged or simply landfilled, will cause serious pollution to the soil and groundwater, and have serious impacts on the ecological environment and human health. Therefore, oil-based drilling cuttings have been included in the national list of hazardous wastes.
[0003] In order to reduce the emission and treatment volume of oil-based drilling cuttings and transform them from hazardous waste into secondary resources, the valuable components such as petroleum hydrocarbon mineral oil and barite are fully recycled and utilized, and a small amount of waste is treated harmlessly, so as to achieve the purpose of resource recycling, reduce environmental pollution and avoid environmental risks. Summary of the invention
[0004] In order to solve the above problems, the present invention proposes a method for recovering barite from oil-based drilling cuttings by roasting-flotation-high-intensity magnetic separation.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for recovering barite from oil-based drilling cuttings by roasting-flotation-high-intensity magnetic separation comprises the following steps:
[0007] 1) Screening and discarding tailings: Put the oil-based drilling cuttings ash sample into a vibrating screen, use a 0.15mm aperture standard screen to screen out low-grade coarse tailings with a particle size greater than 0.15mm, and the samples with a particle size less than 0.15mm under the screen are used as raw materials for roasting;
[0008] 2) Calcination: Place the sample with a particle size less than 0.15 mm obtained after screening in a box-type resistance furnace for calcination. The calcined material can directly enter the roughing flotation machine for flotation;
[0009] 3) Primary flotation roughing: the roasted material is placed in a roughing flotation machine, mixed with water to form a slurry with a concentration of 20%, a pH adjuster is first added, then 2500 g / t of an inhibitor and 600 g / t of a collector are added, stirred and aerated, and concentrate 1 and tailings 1 are separated by primary flotation roughing;
[0010] 4) Secondary flotation roughing: put the tailings 1 into the roughing flotation machine, first add 1000g / t of inhibitor, then add 300g / t of collector, stir and aerate, and select the concentrate 2 and tailings 2 through secondary flotation roughing;
[0011] 5) Scavenging: put the tailings 2 into a scavenging flotation machine, first add 1000g / t of inhibitor, then add 200g / t of collector, stir and aerate, and scavenging to separate the middlings 1 and flotation tailings;
[0012] 6) Primary concentration: Concentrate 1 and concentrate 2 are combined and put into a concentration flotation machine, stirred, and concentrate 3 and middling 2 are separated through primary concentration. Middling 1 and middling 2 are returned to the roughing flotation machine after roasting, and are put into the roughing flotation machine together with the roasted materials for primary flotation and roughing;
[0013] 7) Secondary concentration: Put the concentrate 3 into the concentration flotation machine, stir it, and separate the concentrate 4 and the middling 3 through secondary concentration. After the middling 3 is returned to the secondary flotation roughing, it is put into the concentration flotation machine together with the concentrate 1 and concentrate 2 for primary concentration;
[0014] 8) Intensive magnetic separation: The concentrate 4 is placed in a wet-type high-intensity magnetic separator, the magnetic field strength is set, and the concentrate and the high-intensity magnetic tailings are separated by high-intensity magnetic separation.
[0015] Preferably, in the above-mentioned method for recovering barite from oil-based drilling cuttings by combined roasting-flotation-high-intensity magnetic separation, in step 2), the roasting conditions are: roasting temperature is 500° C., and roasting time is 60 min.
[0016] Preferably, in the above-mentioned method for recovering barite from oil-based drilling cuttings by combined roasting-flotation-high-intensity magnetic separation, in step 3), the pH adjuster is H2SO4, the amount of which is 5000g / t, and the pH value of the slurry is adjusted to 9.
[0017] Preferably, in the above-mentioned method for recovering barite from oil-based drilling cuttings by roasting-flotation-high-intensity magnetic separation, in step 3), the collector is: 400 g / t of sodium dodecyl sulfate and 200 g / t of sodium oleate.
[0018] Preferably, in the above-mentioned method for recovering barite from oil-based drilling cuttings by roasting-flotation-high-intensity magnetic separation, in step 4), the collector is: 200 g / t of sodium dodecyl sulfate and 100 g / t of sodium oleate.
[0019] Preferably, in the above-mentioned method for recovering barite from oil-based drilling cuttings by combined roasting-flotation-high-intensity magnetic separation, in step 5), the collector is: sodium dodecyl sulfate in an amount of 150 g / t and sodium oleate in an amount of 50 g / t.
[0020] Preferably, in the above-mentioned method for recovering barite from oil-based drilling cuttings by combined roasting-flotation-high-intensity magnetic separation, the inhibitor is water glass.
[0021] Preferably, in the above-mentioned method for recovering barite from oil-based drilling cuttings by combined roasting-flotation-high-intensity magnetic separation, in step 3), the stirring and aeration time is 4 minutes.
[0022] Preferably, in the above-mentioned method for recovering barite from oil-based drilling cuttings by combined roasting-flotation-high-intensity magnetic separation, in step 4) and step 5), the stirring and aeration time is 2 minutes.
[0023] Preferably, in the above-mentioned method for recovering barite from oil-based drilling cuttings by combined roasting-flotation-high-intensity magnetic separation, in step 6), the stirring time is 3 minutes.
[0024] Preferably, in the above-mentioned method for recovering barite from oil-based drilling cuttings by combined roasting-flotation-high-intensity magnetic separation, in step 7), the stirring time is 2 minutes.
[0025] Preferably, in the above-mentioned method for recovering barite from oil-based drilling cuttings by combined roasting-flotation-high-intensity magnetic separation, in step 8), the magnetic field strength is 160KA / m.
[0026] The beneficial effects of the present invention are:
[0027] 1. According to the properties of barite and sample raw materials, the present invention adopts a closed-circuit process of pre-screening and discarding tailings-roasting-flotation-strong magnetic separation. The pre-screening and discarding of tailings discards the low-grade coarse particles of +0.15 mm, which can not only realize the pre-enrichment of materials, but also reduce the amount of materials for roasting and flotation; the purpose of roasting is to eliminate the influence of petroleum hydrocarbon mineral oil on flotation; the materials after screening and roasting enter flotation, and after two roughing selections, one scavenging selection and two fine selections, the flotation concentrate is subjected to strong magnetic separation to remove biotite, and a concentrate with a barite content of 91.30% can be obtained, the concentrate yield is 27.47%, and the concentrate barite recovery rate is 71.39%.
[0028] 2. The present invention studies and determines the flotation process conditions for the roasted samples. By using sulfuric acid to adjust the pH value of the pulp to weak alkalinity, a small amount of inhibitor is used in combination, and a compound fatty acid agent is used as the collector, two roughing selections, one scavenging selection and two fine selections are carried out under this condition to obtain a barite concentrate with a relatively ideal grade.
[0029] 3. The various indicators of tailings pollutants obtained after treatment by the method of the present invention are far below the industry standard limit. The present invention not only realizes the full recycling of barite and achieves resource recycling, but also realizes the harmless treatment of a small amount of waste and reduces environmental pollution. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The present invention is a process flow chart of a method for recovering barite from oil-based drilling cuttings by combined roasting-flotation-high-intensity magnetic separation. DETAILED DESCRIPTION
[0031] Example 1 Sample component analysis
[0032] The sample is the ash residue after the oil-based drilling cuttings are heat-treated and the mineral oil is recovered. The sample is in the form of gray powder, which is mixed with coarse rock fragments and fine agglomerates. The sample has an unpleasant odor and poor wettability.
[0033] The samples were analyzed by X-ray powder diffraction and chemical multiple analysis (results as shown in Table 1). The content of barite (BaSO4) in the samples was 34.20%, and other mineral components were mainly quartz, plagioclase, calcite and a small amount of biotite. The results of sample screening analysis are shown in Table 2. The sample particle size is fine and uneven, and most of it is concentrated in -0.030mm (500 mesh). The -0.030mm particle size accounts for 54.07% of the total mass, and the +0.15mm (100 mesh) particle size accounts for 21.74% of the total mass. Barite mainly exists in the fine particle size, the -0.030mm particle size barite content is 44.50%, accounting for 72.10% of the total barite in the sample, while the +0.15mm particle size barite content is 6.19%, accounting for only 4.04% of the total barite.
[0034] Table 1 Results of multiple chemical analyses of samples (%)
[0035]
[0036] Table 2 Sample screening analysis results
[0037]
[0038] Example 2 Process Parameter Optimization
[0039] 1) Effect of roasting temperature and time on flotation
[0040] Petroleum hydrocarbons in the sample can be effectively removed by roasting. The most intuitive manifestation is that with the increase of roasting temperature, the color of the roasting product changes from gray to khaki. The raw material is highly hydrophobic before roasting, and strong friction stirring is required to fully wet it. The hydrophilicity of the material is significantly improved after roasting. At the same time, since the coarse particles are screened out, the roasted material can be directly put into the flotation machine for flotation test. However, the roasting temperature and time have a great influence on the roasting cost. At the same time, too high a temperature will change the composition of the sample and will also have a certain impact on flotation. Therefore, this experiment examines the influence of roasting temperature and time on flotation, and the results are shown in Table 3. The test results show that the sorting effect is better when the roasting temperature is 400℃ and 500℃. When the roasting temperature is 400℃, the barite concentrate content is 91.65%, and the barite recovery rate is 52.42%; when the roasting temperature is 500℃, the barite concentrate content is 94.10%, and the barite recovery rate is 41.38%. If the roasting time is too long or the temperature is too high, the barite content and recovery rate will decrease significantly. At the same time, considering that the drilling cuttings were previously heat treated at 500℃ to recover mineral oil, the ash roasted at 500℃ can obtain a higher barite content when flotating barite. Therefore, this test determines the roasting temperature to be 500℃ and the roasting time to be 60min.
[0041] Table 3 Effect of roasting temperature and time on flotation
[0042]
[0043]
[0044] 2) Effects of pH and pH adjusters on flotation
[0045] The sample has strong alkalinity and is mixed with water to form a slurry with a concentration of 20%, with a pH value of about 10. The pH value of the flotation medium will have a great influence on the surface properties of the target mineral and the adsorption of the flotation agent on the target mineral surface. This experiment examined the effects of pH value and pH adjuster on the flotation of barite, and the results are shown in Tables 4 and 5.
[0046] The results of the pH test (Table 4) show that without adding acid or alkali, the pH value of the pulp is about 10. Under this condition, the flotation effect is the worst, the concentrate yield and recovery rate are very low, and most of the barite cannot be recovered by flotation. Adding Na2CO3 to increase the pH value of the pulp, the flotation effect of barite is still not ideal. Adding H2SO4 to reduce the pH value of the pulp, the concentrate yield and recovery rate are significantly improved, and the concentrate recovery rate increases with the decrease of pH value. The BaSO4 content of the concentrate fluctuates slightly. When the pH is about 9, the concentrate recovery rate is the highest.
[0047] Table 4 Effect of pH value on flotation
[0048]
[0049]
[0050] Adding H2SO4 during flotation to reduce the pH value of the pulp is very beneficial to the recovery of barite, but it is generally believed that SO4 2- Ions have a certain inhibitory effect on barite. Therefore, this experiment used HCl instead of H2SO4 and examined the effect of HCl dosage on barite flotation. The results are shown in Table 5.
[0051] By comparing the dosage tests of HCl and H2SO4, it can be seen that the BaSO4 content of the HCl flotation concentrate is significantly higher than that of H2SO4, while the concentrate recovery rate is significantly lower than that of H2SO4. The reason may be that the Ca in the slurry 2+ About SO4 2- Ions can precipitate Ca in the slurry 2+ ions, thereby controlling the Ca 2+ Ion concentration and pH value, while the slurry remains weakly alkaline, SO4 2- Ions and Ca 2+ After ion precipitation, it did not inhibit barite. Although HCl can reduce the pH value of the slurry, it greatly increases the Ca 2+ Ion concentration, Ca 2+ Ions react with collectors and consume them, thus affecting the recovery of barite. Therefore, when using HCl, the amount of collector must be increased to improve the flotation recovery rate. After comprehensive consideration, the amount of pH adjuster H2SO4 is determined to be 5000g / t.
[0052] Table 5 Effect of hydrochloric acid dosage on flotation
[0053]
[0054] 3) Effect of inhibitors on flotation
[0055] The main function of the inhibitor is to increase the hydrophilicity of the gangue minerals, expand the floatability difference with the target minerals, or disperse the gangue slime to prevent the gangue slime from agglomerating with the target minerals, thereby improving the separation efficiency or the concentrate grade. This test selected water glass, a commonly used inhibitor in the barite flotation process, and the inhibitor dosage test results are shown in Table 6.
[0056] The test results show that the BaSO4 content of the concentrate changes slightly with the increase of inhibitor dosage, and the overall effect is not significant. The concentrate yield and recovery rate increase with the increase of inhibitor. When the inhibitor dosage is 2500g / t, the BaSO4 content of the concentrate is the highest, and when the inhibitor dosage is 5000g / t, the concentrate recovery rate is the highest. After comprehensive consideration, the inhibitor dosage is determined to be 2500g / t.
[0057] Table 6 Effect of inhibitors on flotation
[0058]
[0059] 4) Effect of collector on flotation
[0060] Barite collectors include fatty acids, alkyl sulfates, petroleum sulfonates, phosphonates, amines, aminoalkylphosphonic acids and combined collectors, among which fatty acids, alkyl sulfates and petroleum sulfonates are the most commonly used. According to the principle of synergy between agents, two or more collectors are often used in a certain proportion to improve the collection capacity and selectivity of the mixed agent, so as to obtain a better flotation effect than a single collector. This test selected three agents, namely, sodium petroleum sulfonate (SW), sodium oleate (LN) and sodium dodecyl sulfate (SSN), for flotation tests. The concentration of the collectors was 1%, and the test results are shown in Table 7.
[0061] Through the examination of three collectors, it was found that under the same dosage conditions, SW had the worst sorting effect on barite, and the BaSO4 content and recovery rate of the concentrate were lower than those of SSN and LN; compared with SSN and LN, SSN had better selectivity and higher BaSO4 content in the concentrate, while LN had stronger collection ability and higher recovery rate, but the BaSO4 content was slightly lower than that of SSN. After SSN and LN were mixed, their effect was better than the indicators of the two used alone, and with the increase of collector dosage, the concentrate yield and recovery rate increased. When the dosage of SSN and LN was 400g / t and 200g / t respectively, the concentrate recovery rate reached 84.54%. The recovery rate did not increase significantly with the continued increase of collectors. Therefore, the collector dosage was determined to be 400g / t for SSN and 200g / t for LN.
[0062] Table 7 Effect of collector type and dosage on flotation
[0063]
[0064] Example 3 Recovery of barite from oil-based drilling cuttings by roasting-flotation-high-intensity magnetic separation
[0065] The process flow of recovering barite from oil-based drilling cuttings by roasting-flotation-high-intensity magnetic separation is as follows: Figure 1 .
[0066] 1) Screening and discarding tailings: Put the oil-based drilling cuttings ash sample into the dry screening equipment RK / ZS-600*300 vibrating screen, and use a 0.15mm aperture (100 mesh) standard screen to screen out low-grade coarse tailings with a particle size greater than 0.15mm. The samples with a particle size less than 0.15mm under the screen are used as raw materials for roasting. Since the coarse-grained barite content in the sample is low, the coarse-grained cuttings can be removed by screening, which can not only achieve the pre-enrichment of the material, but also reduce the amount of material for roasting and flotation, and at the same time reduce the impact of coarse particles on flotation and the wear on the flotation machine.
[0067] 2) Calcination: Place the sample with a particle size less than 0.15 mm after screening into a box-type resistance furnace of the calcination equipment at a calcination temperature of 500°C for 60 minutes. The calcined material can be directly fed into the roughing flotation machine for flotation. The purpose of calcination pretreatment is to volatilize or oxidize organic oils such as petroleum hydrocarbons in the sample to reduce or eliminate the impact on flotation.
[0068] 3) Primary flotation roughing: the roasted material is placed in a roughing flotation machine and mixed with water to form a slurry with a concentration of 20% (pH value is 10), 5000 g / t of pH adjuster H2SO4 is first added to adjust the pH value of the slurry to 9, and then 2500 g / t of water glass and collector are added, the amount of collector is SSN 400 g / t and LN is 200 g / t, stirred and aerated for 4 minutes, and concentrate 1 and tailings 1 are selected through primary flotation roughing.
[0069] 4) Secondary flotation roughing: put tailings 1 into the roughing flotation machine, first add 1000g / t of water glass, then add collector, the amount of collector is SSN 200g / t and LN is 100g / t, stir and aerate for 2 minutes, and select concentrate 2 and tailings 2 through secondary flotation roughing.
[0070] 5) Scavenging: put the tailings 2 into a scavenging flotation machine, first add 1000g / t of water glass, then add collectors, the amount of collectors is SSN 150g / t and LN is 50g / t, stir and aerate for 2 minutes, and scavenging to separate the middling ore 1 and flotation tailings.
[0071] 6) Primary concentration: Concentrate 1 and concentrate 2 are combined and put into the concentration flotation machine, stirred for 3 minutes, and concentrate 3 and middling 2 are separated through primary concentration. Middling 1 and middling 2 are returned to the roasting machine after the roasting is completed, and put into the roughing flotation machine together with the roasted materials for primary flotation and roughing.
[0072] 7) Secondary concentration: Put the concentrate 3 into the concentration flotation machine, stir for 2 minutes, and select the concentrate 4 and the middling 3 through secondary concentration. After the middling 3 is returned to the secondary flotation roughing, it is put into the concentration flotation machine together with the concentrate 1 and concentrate 2 for primary concentration. The middling ore is generally returned to the sorting operation with similar grade to achieve full recovery of valuable minerals.
[0073] 8) Strong magnetic separation: Put the concentrate 4 into a 50*70 wet strong magnetic separator, the magnetic field strength is 160KA / m, and the concentrate and strong magnetic tailings are separated by strong magnetic separation. There is a small amount of biotite in the barite flotation concentrate. Biotite has a certain hydrophobicity and is easy to enter the concentrate with the flotation foam, which affects the grade of the concentrate. The sample contains a very small amount of magnetic iron (mFe content 0.40%). Therefore, the flotation concentrate is subjected to strong magnetic separation to remove biotite and improve the grade of the concentrate.
[0074] The products and their indicators of the oil-based drilling cuttings ash samples separated by the above process are shown in Tables 8 and 9. The recovery of barite from oil-based drilling cuttings adopts a screening-roasting-flotation-strong magnetic separation combined process, through which relatively ideal technical indicators are obtained, with a concentrate barite content of 91.30%, a concentrate yield of 27.47%, and a barite recovery rate of 71.39%.
[0075] Table 8 Ore dressing indexes of roasting-flotation-high intensity magnetic separation process
[0076] Product Name Yield (%) <![CDATA[BaSO4 content (%)]]> <![CDATA[Recovery rate of BaSO4(%)]]> Concentrate 27.47 91.30 71.39 Strong magnetic tailings 3.54 25.64 2.58 Flotation tailings 47.25 16.50 22.19 Coarse tailings 21.74 6.19 3.84 raw material 100.00 35.13 100.00
[0077] Table 9 Barite concentrate quality analysis
[0078] Element <![CDATA[BaSO4]]> <![CDATA[SiO2]]> <![CDATA[Fe2O3]]> <![CDATA[Al2O3]]> CaO MgO content(%) 91.30 2.26 0.32 1.67 1.09 0.18
[0079] The analysis of tailings pollutants (coarse-grained tailings, flotation tailings and strong magnetic tailings) is tested in accordance with the requirements of the "Standard for the Utilization and Disposal of Residual Solid Phase after Comprehensive Utilization of Oily Sludge in Natural Gas Exploitation" (DB51 / T 2850-2021). The specific analysis items and analysis results are shown in Table 10. It can be seen from Table 10 that the various indicators of tailings pollutants are far below the standard limits.
[0080] Table 10 Analysis results of pollutants in barite beneficiation tailings
[0081]
[0082]
Claims
1. A method for recovering barite from oil-based drilling cuttings by roasting-flotation-high-intensity magnetic separation, characterized in that: The steps include: 1) Screening and discarding tailings: Put the oil-based drilling cuttings ash sample into a vibrating screen, use a 0.15mm aperture standard screen to screen out low-grade coarse tailings with a particle size greater than 0.15mm, and the samples with a particle size less than 0.15mm under the screen are used as raw materials for roasting; 2) Calcination: Place the sample with a particle size less than 0.15 mm obtained after screening in a box-type resistance furnace for calcination. The calcined material can directly enter the roughing flotation machine for flotation; 3) Primary flotation roughing: the roasted material is placed in a roughing flotation machine, mixed with water to form a slurry with a concentration of 20%, a pH adjuster is first added, then 2500 g / t of an inhibitor and 600 g / t of a collector are added, stirred and aerated, and concentrate 1 and tailings 1 are separated by primary flotation roughing; 4) Secondary flotation roughing: put the tailings 1 into the roughing flotation machine, first add 1000g / t of inhibitor, then add 300g / t of collector, stir and aerate, and select the concentrate 2 and tailings 2 through secondary flotation roughing; 5) Scavenging: put the tailings 2 into a scavenging flotation machine, first add 1000g / t of inhibitor, then add 200g / t of collector, stir and aerate, and scavenging to separate the middlings 1 and flotation tailings; 6) Primary concentration: Concentrate 1 and concentrate 2 are combined and put into a concentration flotation machine, stirred, and concentrate 3 and middling 2 are separated through primary concentration. Middling 1 and middling 2 are returned to the roughing flotation machine after roasting, and are put into the roughing flotation machine together with the roasted materials for primary flotation and roughing; 7) Secondary concentration: Put the concentrate 3 into the concentration flotation machine, stir it, and separate the concentrate 4 and the middling 3 through secondary concentration. After the middling 3 is returned to the secondary flotation roughing, it is put into the concentration flotation machine together with the concentrate 1 and concentrate 2 for primary concentration; 8) Intensive magnetic separation: The concentrate 4 is placed in a wet-type high-intensity magnetic separator, the magnetic field strength is set, and the concentrate and the high-intensity magnetic tailings are separated by high-intensity magnetic separation.
2. A method for recovering barite from oil-based drilling cuttings by roasting-flotation-high-intensity magnetic separation according to claim 1, characterized in that: In step 2), the calcination conditions are: calcination temperature is 500° C., and calcination time is 60 min.
3. A method for recovering barite from oil-based drilling cuttings by roasting-flotation-high-intensity magnetic separation according to claim 1, characterized in that: In step 3), the pH adjuster is H2SO4, the dosage is 5000g / t, and the pH value of the slurry is adjusted to 9.
4. A method for recovering barite from oil-based drilling cuttings by roasting-flotation-high-intensity magnetic separation according to claim 1, characterized in that: In step 3), the collector is: 400 g / t of sodium dodecyl sulfate and 200 g / t of sodium oleate.
5. A method for recovering barite from oil-based drilling cuttings by roasting-flotation-high-intensity magnetic separation according to claim 1, characterized in that: In step 4), the collector is: 200 g / t of sodium dodecyl sulfate and 100 g / t of sodium oleate.
6. A method for recovering barite from oil-based drilling cuttings by roasting-flotation-high-intensity magnetic separation according to claim 1, characterized in that: In step 5), the collector is: sodium dodecyl sulfate in an amount of 150 g / t and sodium oleate in an amount of 50 g / t.
7. A method for recovering barite from oil-based drilling cuttings by roasting-flotation-high-intensity magnetic separation according to claim 1, characterized in that: The inhibitor is water glass.
8. A method for recovering barite from oil-based drilling cuttings by roasting-flotation-high-intensity magnetic separation according to claim 1, characterized in that: In step 3), the stirring and aerating time is 4 minutes; in step 4) and step 5), the stirring and aerating time is 2 minutes.
9. A method for recovering barite from oil-based drilling cuttings by roasting-flotation-high-intensity magnetic separation according to claim 1, characterized in that: In step 6), the stirring time is 3 min; in step 7), the stirring time is 2 min.
10. The method for recovering barite from oil-based drilling cuttings by roasting-flotation-high-intensity magnetic separation according to claim 1, characterized in that: In step 8), the magnetic field strength is 160KA / m.
Citation Information
Cited By
Beneficiation method for efficiently recovering barite from heat treatment drilling waste
CN119588506A