Efficient copper smelting slag beneficiation method
Through slow cooling method and multi-step process optimization, including crushing, grinding grading, flotation and dehydration, the problems of copper content in tailings and metal loss in copper smelting slag are solved, and more efficient copper recycling and resource utilization are achieved.
Patent Information
- Application Number
- CN202411243956.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-15
AI Technical Summary
In the existing copper sludge ore dressing methods, the copper content and metal loss of tailings are large, resulting in insufficient resource utilization and the differences in properties caused by differences in cooling methods and selection processes are difficult to effectively solve.
采用缓冷方式对炉渣进行冷却,包括空冷、间断水冷和连续水冷,确保来料性质稳定,并通过破碎、磨矿分级、浮选和脱水流程,结合特定的药剂使用和设备配置,实现更高效的铜回收。
It reduces the energy consumption of the selection process, improves the slag utilization rate, obtains good tailings copper-containing indicators, reduces metal loss, and saves economic costs.
Smart Images

Figure CN118950243A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nonferrous metallurgy, and in particular to a high-efficiency copper smelting slag beneficiation method. Background Art
[0002] The recovery of copper from smelting slag is increasingly valued by the copper metallurgical industry. The most commonly used and effective copper recovery process is the flotation process. However, copper smelting slag is a complex aggregate that is chemically bonded and physically adhered to iron, silicon, magnesium and other substances under high temperature conditions. Its properties depend not only on the raw material composition and operating conditions of pyrometallurgy, but also on the cooling method and cooling system of the slag. Currently, the common cooling methods are rapid cooling and slow cooling. The properties of slag under the two different cooling modes are quite different. The later selection process is adjusted according to the properties of the original ore to recover copper as much as possible and reduce metal loss.
[0003] After searching, the patent with application number CN201110430785.2 discloses a screening and flotation combined process beneficiation method for recovering copper from copper smelting converter slag. The method is to feed the converter slag into a ball mill after crushing, and then enter the screening and grading after grinding. After secondary screening, the +2mm screen-grade product is returned to the ball mill as return sand for re-grinding; the -2mm screen-under and +0.1mm screen-over products can be directly used as copper concentrate products; the -0.1mm screen-under products are pulped and added with flotation agents to enter flotation; after three roughing selections and one scavenging selection, the copper concentrate product is obtained; the method adopts the screening and flotation combined process to recover the coarse-grained copper in advance and effectively; it has a wide range of applications, is easy to operate, and has low cost.
[0004] However, combined with the differences in the final tailings copper content and recovery rate of various smelting industries, the main reasons are the differences in slag properties, crystal formation methods, separation processes and reagent systems. Therefore, an efficient copper smelting slag beneficiation method is proposed to reduce the copper content in the slag tailings, minimize metal loss, and maximize resource utilization. Summary of the invention
[0005] In order to solve the above problems existing in the prior art, the present invention provides a high-efficiency copper smelting slag beneficiation method.
[0006] The technical solution of the present invention is as follows:
[0007] An efficient copper smelting slag beneficiation method comprises the following five processes:
[0008] S1, cooling and ore matching, using slow cooling method to fully cool the slag, the slow cooling method includes air cooling, intermittent water cooling and continuous water cooling, the air cooling time is controlled to be 18 to 24 hours for mineral monomer dissociation; the intermittent water cooling time is controlled to be 10 to 12 hours to avoid slag cracking caused by rapid cooling; the continuous water cooling time is controlled to be more than 40 hours to fully cool the slag;
[0009] S2, crushing process, after the slag obtained in step S1 is classified and stacked according to its different components, ore blending is carried out, and then the slag is roughly crushed and transported to the intermediate ore bin;
[0010] S3, grinding and classification process, the slag in the intermediate ore bin in step S2 is conveyed to the semi-autogenous mill through a feeder and a belt for grinding, and then enters the linear vibrating screen for screening, the slag that does not pass the linear vibrating screen is returned to the semi-autogenous mill for re-grinding, and the slag that passes the linear vibrating screen is subjected to a first-stage classification and a controlled classification at a time, and the slag that passes both the first-stage classification and the controlled classification is combined with the ball mill discharge and then returned to the first-stage classification process by a slurry pump to repeat the operation;
[0011] S4, flotation process, the slurry transported to the flotation stirring tank in step S3 is stirred with chemicals, and then flows into the flotation machine for rough selection. The rough selection adopts rapid flotation. The tailings are scavenged four times to obtain the final tailings, which are pumped to the tailings thickener by the slurry pump. The four scavenged concentrates are combined into medium ore, and then pumped back to the control classification hydrocyclone for classification. The qualified slag concentrate obtained by flotation is transported to the next process for dehydration;
[0012] S5, dehydration process, the slag concentrate in step S4 is precipitated in a thickener, and when the concentration is greater than 40%, the slag concentrate is pumped to the feed pump pool of the vertical filter press in the concentrate filtration workshop by a slurry pump, and then fed into the filter press by the filter press feed pump; when the concentration is greater than 55%, the slag concentrate is pumped to the slurry distribution tank in the tailings filtration workshop by a slurry pump, and flows into the ceramic filter for filtration.
[0013] Preferably, in the coarse crushing process in S2, a hydraulic breaker is used to crush large pieces of slag to less than 350 mm, and then the crushed slag is transported to the original ore bin for secondary crushing by an inclined lifting trolley, and the particle size of the crushed product is controlled to be between 0 mm and 200 mm.
[0014] Preferably, the feeder in S3 is an underseat feeder, and the semi-autogenous mill uses 120mm forged balls, the mill filling rate is controlled at 8% to 15%, the grinding concentration is controlled at 75% to 85%, and the grinding fineness (-200 mesh) is controlled at more than 35%.
[0015] Preferably, the linear vibration screening in S3 uses a round hole screen with a mesh size of 8 mm to 10 mm, and the mesh is in the shape of an inverted trapezoid with small holes at the top and large holes at the bottom.
[0016] Preferably, the filling rate of the ball mill in S3 is controlled at 30% to 50%, the slurry concentration of the ball mill is controlled at 75% to 80%, the discharge fineness is controlled (-200 mesh) at more than 60%, a hydrocyclone is used for classification in one stage, and the classification pressure is controlled at 0.2 MPa to 0.3 MPa. The overflow of the hydrocyclone for one stage of classification is then pumped to the hydrocyclone for controlling the classification through a slurry pump, and the control classification pressure is controlled at 0.25 MPa to 0.35 MPa; the sand settling of the two stages of hydrocyclones is returned to the ball mill to form a closed-circuit grinding.
[0017] Preferably, the reagent in S4 uses DNTY-001 as a collector, 2# oil as a foaming agent, sodium hydroxide as a pH adjuster, sodium sulfide as an activator, and water glass as a dispersant, wherein DNTY-001, 2# oil, sodium sulfide, and water glass are added to five points, namely, roughing selection 1, roughing selection 2, scavenging selection 1, scavenging selection 2, and scavenging selection 3, in a certain amount, and sodium hydroxide is added to the return water pool.
[0018] Preferably, 2# oil is added as a stock solution, and DNTY-001, sodium sulfide, water glass, and sodium hydroxide need to be prepared into solutions with a concentration of 5% to 10% before being added.
[0019] Preferably, the extrusion pressure of the filter press in S5 is controlled at 0.65 MPa to 0.75 MPa, the wind drying pressure is controlled at 0.4 MPa to 0.5 MPa, and the filter cake thickness in the filter press is controlled at 20 mm to 30 mm.
[0020] Preferably, the filtration vacuum of the ceramic filter in S5 is controlled at 0.06 MPa to 0.08 MPa.
[0021] The present invention has the following beneficial effects: the present invention adopts a slow cooling method including air cooling, intermittent water cooling and continuous water cooling through cooling ore, which can better ensure the stability of the incoming material properties entering the subsequent process, and can better reduce the energy consumption in the selection process, and then through the coarse crushing process to ensure that the crushed material can have a higher utilization rate when entering the next process, and after crushing, the grinding and grading process is carried out, which can more accurately screen and grind slag materials of different levels, improve the utilization rate of slag, and facilitate flotation and dehydration. The overall process can achieve good tailings copper content indicators while reducing energy consumption, increasing processing volume, and saving economic costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 For the present invention; DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] See also Figure 1 , an efficient copper smelting slag beneficiation method, including the following five processes:
[0025] S1, cooling and ore matching, using slow cooling method to fully cool the slag, the slow cooling method includes air cooling, intermittent water cooling and continuous water cooling, the air cooling time is controlled to be 18 to 24 hours for mineral monomer dissociation; the intermittent water cooling time is controlled to be 10 to 12 hours to avoid slag cracking caused by rapid cooling; the continuous water cooling time is controlled to be more than 40 hours to fully cool the slag;
[0026] S2, crushing process, after the slag obtained in step S1 is classified and stacked according to its different components, ore blending is carried out, and then the slag is roughly crushed and transported to the intermediate ore bin;
[0027] S3, grinding and classification process, the slag in the intermediate ore bin in step S2 is conveyed to the semi-autogenous mill through a feeder and a belt for grinding, and then enters the linear vibrating screen for screening, the slag that does not pass the linear vibrating screen is returned to the semi-autogenous mill for re-grinding, and the slag that passes the linear vibrating screen is subjected to a first-stage classification and a controlled classification at a time, and the slag that passes both the first-stage classification and the controlled classification is combined with the ball mill discharge and then returned to the first-stage classification process by a slurry pump to repeat the operation;
[0028] S4, flotation process, the slurry transported to the flotation stirring tank in step S3 is stirred with chemicals, and then flows into the flotation machine for rough selection. The rough selection adopts rapid flotation. The tailings are scavenged four times to obtain the final tailings, which are pumped to the tailings thickener by the slurry pump. The four scavenged concentrates are combined into medium ore, and then pumped back to the control classification hydrocyclone for classification. The qualified slag concentrate obtained by flotation is transported to the next process for dehydration;
[0029] S5, dehydration process, the slag concentrate in step S4 is precipitated in a thickener, and when the concentration is greater than 40%, the slag concentrate is pumped to the feed pump pool of the vertical filter press in the concentrate filtration workshop by a slurry pump, and then fed into the filter press by the filter press feed pump; when the concentration is greater than 55%, the slag concentrate is pumped to the slurry distribution tank in the tailings filtration workshop by a slurry pump, and flows into the ceramic filter for filtration.
[0030] Furthermore, in the coarse crushing process of S2, a hydraulic breaker is used to crush large pieces of slag to less than 350 mm, and then the crushed slag is transported to the original ore bin for secondary crushing by an inclined lifting car, and the particle size of the crushed product is controlled to be between 0 and 200 mm.
[0031] Furthermore, the feeder in S3 adopts an underseat feeder, and the semi-autogenous mill uses 120mm forged balls, the mill filling rate is controlled at 8% to 15%, the grinding concentration is controlled at 75% to 85%, and the grinding fineness (-200 mesh) is controlled at more than 35%.
[0032] Furthermore, the linear vibration screening in S3 uses a round hole screen with a mesh size of 8 mm to 10 mm, and the mesh is in the shape of an inverted trapezoid with small holes on the top and large holes on the bottom.
[0033] Furthermore, the filling rate of the ball mill in S3 is controlled at 30% to 50%, the slurry concentration of the ball mill is controlled at 75% to 80%, the discharge fineness is controlled (-200 mesh) at more than 60%, a hydrocyclone is used for classification in the first stage, and the classification pressure is controlled at 0.2 MPa to 0.3 MPa. The overflow of the hydrocyclone of the first stage classification is then pumped to the hydrocyclone for controlling the classification through a slurry pump, and the control classification pressure is controlled at 0.25 MPa to 0.35 MPa; the sand settling of the two stages of hydrocyclones is returned to the ball mill to form a closed-circuit grinding.
[0034] Furthermore, the reagent in S4 uses DNTY-001 as a collector, 2# oil as a foaming agent, sodium hydroxide as a pH adjuster, sodium sulfide as an activator, and water glass as a dispersant, among which DNTY-001, 2# oil, sodium sulfide, and water glass are added to five points, namely, roughing selection 1, roughing selection 2, scavenging selection 1, scavenging selection 2, and scavenging selection 3, in a certain amount, and sodium hydroxide is added to the return water pool.
[0035] Furthermore, 2# oil is added as a stock solution, and DNTY-001, sodium sulfide, water glass, and sodium hydroxide need to be prepared into solutions with a concentration of 5% to 10% before being added.
[0036] Furthermore, the extrusion pressure of the filter press in S5 is controlled at 0.65 MPa to 0.75 MPa, the wind drying pressure is controlled at 0.4 MPa to 0.5 MPa, and the filter cake thickness in the filter press is controlled at 20 mm to 30 mm.
[0037] Furthermore, the filtration vacuum of the ceramic filter in S5 is controlled at 0.06 MPa to 0.08 MPa.
[0038] Working principle of the present invention:
[0039] In the present invention, firstly, cooling and ore blending are carried out, and the slag is fully cooled by slow cooling. Slow cooling is helpful for the "growth" of copper sulfide and metallic copper crystal particles in the slag. Different cooling times are selected according to the copper content and iron content in the smelting element analysis results. A 12m3 casting slag bag or welding slag bag is used for cooling the slag bag; slow cooling methods include air cooling, intermittent water cooling and continuous water cooling. The air cooling time is controlled at 18 to 24 hours for the dissociation of mineral monomers; the intermittent water cooling time is controlled at 10 to 12 hours to avoid the slag from cracking due to rapid cooling and causing slag blasting; the continuous water cooling time is controlled at more than 40 hours to fully cool the slag and avoid the appearance of red core slag during slag pouring. The slag can be fully broken after slag pouring. The slag is classified and stacked according to different components, and ore blending is carried out before coarse crushing to ensure that the incoming materials entering the grinding and flotation system are stable. Sufficient preparatory work before selection can reduce energy consumption during the selection process;
[0040] Then, the crushing process is carried out. The coarse crushing process adopts the inclined lifting trolley loading method for the first time. Compared with the traditional loading method, the inclined lifting trolley loading can realize the raw ore matching and increase the cooling time of the slag after the bag is inverted. Compared with the belt loading, the inclined lifting trolley loading can have a higher operation rate, because the slag still has residual heat after the slow cooling, which will increase the belt loss. The large slag is crushed to less than 350mm by a mobile hydraulic crusher in the slag yard. The loader sends the slag in the slag slow cooling field to the inclined lifting trolley, and the material is transported to the raw ore bin by the inclined lifting trolley. The bottom of the bin is transported to the jaw crusher for crushing by a bar vibrating feeder. The particle size of the crushed product is 0mm to 200mm, and it is sent to the intermediate ore bin for storage by a belt conveyor.
[0041] Next, the grinding and grading process is carried out. The vibrating feeder under the middle ore bin feeds the slag into the belt conveyor and transports it to the semi-autogenous mill for grinding. The semi-autogenous mill uses 120mm forged balls, the mill filling rate is controlled at 8% to 15%, the grinding concentration is controlled at 75% to 85%, and the grinding fineness (-200 mesh) is controlled at more than 35%. The semi-autogenous mill discharges into the linear vibrating screen for screening. The vibrating screen has a round hole size of 8mm to 10mm. The screen holes are in the shape of an inverted trapezoid with small top and large bottom, which is conducive to screening without clogging the screen holes; the products on the screen are returned to the semi-autogenous mill through the belt conveyor for re-grinding, and the return sand ratio is controlled at 10% to 20%; the products under the screen (particle size less than 10mm) and the discharge from the ball mill are combined and pumped to a first-stage grading hydrocyclone for grading by a slurry pump. The ball mill filling rate is controlled at 30% to 35%, the ball mill grinding concentration is controlled at 75% to 80%, and the discharge is The fineness (-200 mesh) is controlled at more than 60%, and the classification pressure of the first-stage cyclone is controlled at 0.2mpa to 0.3mpa; the overflow of the first-stage hydrocyclone is pumped to the control classification hydrocyclone through a slurry pump, and the control classification pressure is controlled at 0.25mpa to 0.35mpa; the sand settling of the two-stage hydrocyclones is returned to the ball mill to form a closed-circuit grinding, and the overflow of the control classification hydrocyclone flows by gravity to the slurry stirring tank before the roughing, and the roughing concentration is controlled at 35 to 45%, and the fineness is controlled at more than 80%.
[0042] Then, the flotation process is carried out. The slurry transported to the flotation stirring tank in the grinding and grading process is stirred with chemicals, and then flows into the flotation machine for rough selection. The rough selection adopts rapid flotation. The tailings are scavenged four times to obtain the final tailings, which are pumped to the tailings thickener by the slurry pump. The four-time scavenging concentrates are combined into medium ore, and then pumped back to the controlled grading hydrocyclone for grading. The slag concentrate obtained by flotation is transported to the next process for dehydration. Among them, the reagents selected in the flotation process are DNTY-001 as the collector and 2# oil as the starting material. Foaming agent, sodium hydroxide as pH adjuster, sodium sulfide as activator, water glass as dispersant, among which, DNTY-001, 2# oil, sodium sulfide and water glass are added to the five points of rough selection 1, rough selection 2, scavenging selection 1, scavenging selection 2 and scavenging selection 3 according to a certain amount, and sodium hydroxide is added to the return water pool; among which, 2# oil is added as the original solution, DNTY-001, sodium sulfide, water glass and sodium hydroxide need to be prepared into a solution with a concentration of 5% to 10% before adding, and the preparation work system of the agent is to prepare once a day.
[0043] Finally, the dehydration process is carried out, and the slag concentrate obtained after flotation is precipitated in the thickener. When the precipitation reaches a concentration greater than 40%, the slag concentrate is pumped to the feed pump pool of the vertical filter press in the concentrate filtration workshop by a slurry pump, and then fed into the filter press by the filter press feed pump. Among them, the extrusion pressure of the filter press is controlled at 0.65 MPa to 0.75 MPa, the wind drying pressure is controlled at 0.4 MPa to 0.5 MPa, the filter cake thickness in the filter press is controlled at 20 mm to 30 mm, and the filter cake is unloaded to the concentrate belt. Conveyor, unloaded to the concentrate stack through the belt head and plow type discharger, the filtrate flows by gravity to the concentrate thickener, and the moisture content of the slag concentrate is controlled below 10%; when the precipitation reaches a concentration greater than 55%, the slag slurry pump is used to pump it to the slurry distribution tank in the tailings filtration workshop, and flows by gravity into the ceramic filter for filtration, among which the filtration vacuum of the ceramic filter is controlled at 0.06mpa to 0.08mpa, the filter cake is unloaded to the belt conveyor, and transferred to the tailings stack by the belt conveyor, and the moisture content of the slag tailings is controlled below 12%.
[0044] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. An efficient copper smelting slag beneficiation method, characterized in that: It includes the following five processes: S1, cooling and ore matching, using slow cooling method to fully cool the slag, the slow cooling method includes air cooling, intermittent water cooling and continuous water cooling, the air cooling time is controlled to be 18 to 24 hours for mineral monomer dissociation; the intermittent water cooling time is controlled to be 10 to 12 hours to avoid slag cracking caused by rapid cooling; the continuous water cooling time is controlled to be more than 40 hours to fully cool the slag; S2, crushing process, after the slag obtained in step S1 is classified and stacked according to its different components, ore blending is carried out, and then the slag is roughly crushed and transported to the intermediate ore bin; S3, grinding and classification process, the slag in the intermediate ore bin in step S2 is conveyed to the semi-autogenous mill through a feeder and a belt for grinding, and then enters the linear vibrating screen for screening, the slag that does not pass the linear vibrating screen is returned to the semi-autogenous mill for re-grinding, and the slag that passes the linear vibrating screen is subjected to a first-stage classification and a controlled classification at a time, and the slag that passes both the first-stage classification and the controlled classification is combined with the ball mill discharge and then returned to the first-stage classification process by a slurry pump to repeat the operation; S4, flotation process, the slurry transported to the flotation stirring tank in step S3 is stirred with chemicals, and then flows into the flotation machine for rough selection. The rough selection adopts rapid flotation. The tailings are scavenged four times to obtain the final tailings, which are pumped to the tailings thickener by the slurry pump. The four scavenged concentrates are combined into medium ore, and then pumped back to the control classification hydrocyclone for classification. The qualified slag concentrate obtained by flotation is transported to the next process for dehydration; S5, dehydration process, the slag concentrate in step S4 is precipitated in a thickener, and when the concentration is greater than 40%, the slag concentrate is pumped to the feed pump pool of the vertical filter press in the concentrate filtration workshop by a slurry pump, and then fed into the filter press by the filter press feed pump; when the concentration is greater than 55%, the slag concentrate is pumped to the slurry distribution tank in the tailings filtration workshop by a slurry pump, and flows into the ceramic filter for filtration.
2. The high-efficiency copper smelting slag beneficiation method according to claim 1, characterized in that: In the coarse crushing process of S2, a hydraulic breaker is used to crush large pieces of slag to less than 350 mm, and then the crushed slag is transported to the original ore bin for secondary crushing by an inclined lifting car, and the particle size of the crushed product is controlled to be between 0 mm and 200 mm.
3. The high-efficiency copper smelting slag beneficiation method according to claim 1, characterized in that: The feeder in S3 is an underseat feeder, and the semi-autogenous mill uses 120mm forged balls. The mill filling rate is controlled at 8% to 15%, the grinding concentration is controlled at 75% to 85%, and the grinding fineness (-200 mesh) is controlled at more than 35%.
4. The high-efficiency copper smelting slag beneficiation method according to claim 1, characterized in that: The linear vibration screening in S3 uses a round hole screen with a mesh size of 8 mm to 10 mm, and the mesh is in an inverted trapezoidal shape with small top and large bottom.
5. The high-efficiency copper smelting slag beneficiation method according to claim 1, characterized in that: The filling rate of the ball mill in S3 is controlled at 30% to 50%, the slurry concentration of the ball mill is controlled at 75% to 80%, the discharge fineness (-200 mesh) is controlled at more than 60%, the first stage classification is carried out by a hydrocyclone, the classification pressure is controlled at 0.2 MPa to 0.3 MPa, the overflow of the hydrocyclone of the first stage classification is pumped to the hydrocyclone for controlling the classification through a slurry pump, and the control classification pressure is controlled at 0.25 MPa to 0.35 MPa; the sand settling of the two stages of hydrocyclones is returned to the ball mill to form a closed-circuit grinding.
6. The high-efficiency copper smelting slag beneficiation method according to claim 1, characterized in that: The reagent in S4 uses DNTY-001 as a collector, 2# oil as a foaming agent, sodium hydroxide as a pH adjuster, sodium sulfide as an activator, and water glass as a dispersant, wherein DNTY-001, 2# oil, sodium sulfide, and water glass are added to five points, namely, roughing selection 1, roughing selection 2, scavenging selection 1, scavenging selection 2, and scavenging selection 3, according to certain amounts, and sodium hydroxide is added to the return water tank.
7. The high-efficiency copper smelting slag beneficiation method according to claim 6, characterized in that: The 2# oil is added as a stock solution, and DNTY-001, sodium sulfide, water glass and sodium hydroxide need to be prepared into solutions with a concentration of 5% to 10% before being added.
8. The high-efficiency copper smelting slag beneficiation method according to claim 1, characterized in that: The extrusion pressure of the filter press in S5 is controlled at 0.65 MPa to 0.75 MPa, the wind drying pressure is controlled at 0.4 MPa to 0.5 MPa, and the filter cake thickness in the filter press is controlled at 20 mm to 30 mm.
9. The high-efficiency copper smelting slag beneficiation method according to claim 1, characterized in that: The filtration vacuum of the ceramic filter in S5 is controlled at 0.06 MPa to 0.08 MPa.
Citation Information
Cited By
Method for improving copper slag beneficiation and grinding classification efficiency and reducing ball consumption
CN120001496A