Method for sorting collophanite rich in calcium and magnesium silicate minerals
By crushing, ball milling and ultrafine grinding of silicon-calcareous phosphate blocking rocks, combining pickling dissociation and the use of silicone inhibitors, the problem of difficulty in dissociation of apatite and ganglite minerals has been solved, and the problem of difficulty in dissociation of apatite and ganglite minerals has been improved. Flotation sorting improves the grade and recovery of phosphorus concentrate.
Patent Information
- Application Number
- CN202411039713.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
It is difficult to dissociate apatite and ganglite minerals in silicon-calcareous phosphate block rocks, and the flotation and sorting characteristics are poor, making it difficult to develop and utilize.
Through crushing, ball milling, and ultrafine grinding, pickling and dissociation are carried out, and silicone inhibitors and collectors are added during the flotation process to improve the dissociation and flotation sorting of apatite and gangue minerals and flotation sorting. .
The grade and recovery rate of phosphorus concentrate are improved, and more efficient utilization of phosphorus ore resources is achieved.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of collophanite flotation, and in particular to a method for separating collophanite rich in calcium-magnesium silicate minerals. Background Art
[0002] Phosphorite can be divided into siliceous phosphorite, calcareous phosphorite and siliceous-calcareous phosphorite, among which siliceous-calcareous phosphorite has the highest relative reserves. Phosphorite mainly includes phosphorus-containing minerals and gangue minerals. Phosphorus-containing minerals are mainly carbon fluoroapatite (collophane); gangue minerals mainly include carbonate minerals such as dolomite and calcite, silicate minerals such as mica and clay minerals, siliceous materials such as quartz and chalcedony, and a small amount of iron-containing minerals and carbonaceous materials.
[0003] The mineral types of siliceous-calcium phosphate rock are complex and the content is high, mainly carbonate minerals such as dolomite and calcite, silicate minerals such as mica and clay minerals, and siliceous materials such as quartz and chalcedony. The magnesium oxide content is high, the phosphate minerals and the gangue minerals are closely coexisting, and the minerals are embedded in fine particles. It is the most difficult type of phosphate ore to be selected. With the increasing depletion of rich phosphate resources, the development of beneficiation technology for medium and low-grade difficult-to-select collophanites is imminent. At present, most of the difficult-to-select collophanites at home and abroad adopt the flotation method. The flotation processes used mainly include direct flotation or reverse flotation, direct and reverse flotation, reverse flotation and double reverse flotation, among which, (1) Positive flotation: Positive flotation is a process that suppresses gangue minerals under weakly alkaline conditions and directly selects phosphate ore. For example, under alkaline conditions, "S" series inhibitors are used to suppress gangue minerals, and anionic collectors are used to positively float phosphate minerals. However, the amount of products selected by positive flotation is large, bubbles are difficult to eliminate, and it is also seriously affected by temperature. Reverse flotation method: generally used for flotation of phosphate ore with high carbonate content, low silicate content and simple composition; (2) Direct-reverse flotation method: Direct-reverse flotation process is widely used for medium- and low-grade calcareous colloidal phosphate with high content of gangue minerals such as dolomite and quartz and complex components. Under alkaline conditions, water glass is used to inhibit siliceous minerals, and anionic collectors are used to positively float phosphate minerals and carbonate minerals containing calcium and magnesium to obtain positive flotation concentrate. Sulfuric acid or phosphoric acid is added to the positive flotation concentrate as a phosphate mineral inhibitor, and anionic collectors are used to float carbonate minerals under weakly acidic conditions. The product in the tank is phosphate concentrate. For example, Luo Huihua et al. used direct-reverse flotation when processing Dayukou difficult-to-select phosphate ore. The P2O5 grade of the Dayukou phosphate ore was 22.28%. After flotation, a concentrate with a P2O5 grade of 30.68% was obtained, and the concentrate recovery rate was 83.66%. However, the amount of reagents required for acid-base conversion was greatly increased. (3) Reverse flotation method: Use sulfuric acid or phosphoric acid to inhibit phosphate minerals, use anionic collectors to reverse float dolomite and other carbonate minerals under weak acidic conditions, then use lime or sodium carbonate as a pH adjuster, sodium silicate to inhibit siliceous minerals, and positively float phosphate minerals in an alkaline environment. It is suitable for sedimentary collophosphate ores with lower grade requirements. Generally, it can effectively remove gangue minerals to achieve the purpose of enriching phosphate ore; (4) Double reverse flotation method: Cationic collectors are used to reverse flotate siliceous-calcium phosphate ore to separate useful minerals and gangue minerals. Ge Yingyong et al. used cationic collector GE-609 to reverse flotation to remove silicon from a siliceous-calcium phosphate ore in Yichang. The P2O5 grade and recovery rate in the phosphate concentrate were 32.17% and 87.80%, respectively. However, the cationic foam was abundant and difficult to defoam, making it impossible to carry out industrial production.
[0004] Therefore, siliceous-calcium phosphorite is a colloidal phosphate rich in calcium-magnesium silicate minerals. The symbiotic relationship between apatite and gangue minerals is complex and difficult to dissociate. At the same time, the interfacial properties of the gangue minerals (such as dolomite, olivine, anorthite, etc.) and apatite are slightly different. They all have calcium-magnesium active particles and similar floatability. They can be chemically adsorbed with fatty acid collectors and float up with apatite during positive flotation. The sorting selectivity is poor, which makes this type of ore difficult to develop and utilize at present. Summary of the invention
[0005] The purpose of the present invention is to overcome the above technical deficiencies, provide a method for separating collophanite rich in calcium magnesium silicate minerals, and solve the technical problems in the prior art that apatite and gangue minerals are difficult to dissociate and flotation separation is poor.
[0006] In order to achieve the above technical purpose, the technical solution provided by the present invention is: In a first aspect, the present invention provides a method for separating collophanite rich in calcium magnesium silicate minerals, comprising the following steps: S1, crushing, ball milling, ultrafine grinding and slurrying of collophanite ore rich in calcium magnesium silicate minerals to obtain slurry; S2, acid washing and dissociation of the slurry, adding a first collector to obtain a first slurrying material, and obtaining a reverse flotation concentrate through reverse flotation; and / or, S3, adding a forward flotation pH adjuster to the reverse flotation concentrate, adding an organosilicon inhibitor and a second collector to obtain a second slurrying material, and obtaining a forward flotation concentrate through forward flotation; the reverse flotation concentrate or the forward flotation concentrate is post-treated to obtain a phosphate concentrate.
[0007] Compared with the prior art, the beneficial effects of the present invention include: The method of the present invention crushes, ball-mills and ultrafinely grinds collophanite ore to obtain ultrafine powder, which is then slurried. The obtained slurry is acid-washed for dissociation, thereby solving the problem of difficult dissociation caused by the complex symbiotic relationship between minerals in silicon-calcium phosphorite phosphate ores, and making apatite and dolomite, olivine, calcium feldspar and the like be better dissociated. In addition, organic silicon inhibitors are added in the positive flotation to effectively improve the flotation separation performance. The method of the present invention can obtain phosphate concentrate with higher grade and recovery rate. DETAILED DESCRIPTION
[0008] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0009] Due to the complex symbiotic relationship between the minerals in silico-calcium phosphate rock phosphate ore, and the fact that the gangue minerals such as dolomite, olivine, and calcium feldspar have little difference in interface properties with apatite, they all have calcium and magnesium active particles that can react and adsorb with fatty acid collectors and float up with apatite during positive flotation, making it difficult to efficiently separate and utilize collophanite rich in calcium and magnesium silicate minerals.
[0010] In view of the above defects, the present invention provides a method for separating collophanite rich in calcium-magnesium silicate minerals. The method solves the problem of difficult dissociation caused by the complex symbiotic relationship between the minerals in silicon-calcium phosphorite phosphate ores through ultrafine grinding dissociation and strong acid decomposition, so that apatite and dolomite, olivine, calcium feldspar and the like can be better dissociated; and organic silicon inhibitors are added to overcome the defect that the calcium-magnesium silicate gangue and collophanite have similar properties, and the flotation sorting property is improved; thereby obtaining a phosphate concentrate with higher grade and recovery rate.
[0011] In a first aspect, the present invention provides a method for separating collophanite rich in calcium magnesium silicate minerals, comprising the following steps: S1, crushing, ball milling, ultrafine grinding and slurry preparation of collophanite ore rich in calcium magnesium silicate minerals to obtain slurry; S2, acid-washing and dissociating the ore pulp, adding a first collector to obtain a first slurry material, and performing reverse flotation to obtain a reverse flotation concentrate; S3, adding a forward flotation pH adjuster to the reverse flotation concentrate, and then adding an organosilicon inhibitor and a second collector to obtain a second slurry material, and performing forward flotation to obtain a forward flotation concentrate; The reverse flotation concentrate or the direct flotation concentrate is post-processed to obtain phosphate concentrate.
[0012] Preferably, in step S1, the ultrafine grinding fineness is -0.037 mm and the content is 60% to 98%.
[0013] Preferably, in step S1, the concentration of the slurry is 35-40%.
[0014] Preferably, in step S2, the pickling dissociation is performed by adding acid solution to the ore pulp to adjust the pH value to 0.5-5; the acid solution is a sulfuric acid solution with a mass concentration of 20%, and the amount of the sulfuric acid solution is 10-100 kg / t of the original ore.
[0015] Preferably, in step S2, the pickling dissociation time is 5 to 30 minutes.
[0016] Preferably, in step S2, the first collector is an anionic collector MG-7.
[0017] Further preferably, in step S2, reverse flotation comprises the following steps: The first slurry material is subjected to reverse flotation roughing to obtain reverse flotation concentrate, wherein the dosage of the first collector is 2.5-3.5 kg / t of raw ore (collophane ore rich in calcium magnesium silicate minerals); or, The first slurry material is subjected to reverse flotation roughing to obtain a roughing concentrate and a foam tailing, and the roughing concentrate is added with a first collector for reverse flotation concentration to obtain a reverse flotation concentrate; wherein, the amount of the first collector in the reverse flotation roughing is 1.5-2.5 kg / t of original ore, and the amount of the first collector in the reverse flotation concentration is 0.4-0.6 kg / t of original ore.
[0018] Preferably, in step S2, the speed of reverse flotation is 800-1600 r / min, and the aeration volume is 0.06-0.12 m 3 / h.
[0019] Preferably, in step S3, the forward flotation pH adjuster includes sodium carbonate, and the forward flotation pH adjuster is added to the reverse flotation concentrate to adjust the pH value to 9.5-11.
[0020] Preferably, in step S3, the organosilicon inhibitor includes methyl silicate, and more preferably potassium methyl silicate or sodium methyl silicate, which have low surface tension and good inhibitory performance. The molecular weight of the organosilicon inhibitor ranges from 100 to 250.
[0021] Preferably, in step S3, the total dosage of the organosilicon inhibitor is 1-6 kg / t of raw ore; if the dosage of the organosilicon inhibitor is too high, the phosphate rock will also be suppressed and cannot be floated, and if the dosage is too low, the tailings will all float up, resulting in poor sorting performance.
[0022] Preferably, in step S3, the second collector is a fatty acid collector MG-3; the total dosage of the second collector is 1-3 kg / t of the original ore.
[0023] Preferably, in step S3, the direct flotation specifically includes the following steps: the second slurry material is subjected to roughing to obtain roughing tailings and roughing concentrate; the roughing tailings are added with a second collector for scavenging to obtain tailings in the first tank and foam middlings; the roughing concentrate is added with a positive flotation pH adjuster and an organosilicon inhibitor, and subjected to 1 to 2 rounds of positive flotation to obtain tailings in the second tank and a positive flotation concentrate.
[0024] Further preferably, in the roughing step, the amount of the organosilicon inhibitor is 1-5 kg / t of raw ore, and the amount of the second collector is 0.5-1.4 kg / t of raw ore; in the scavenging step, the amount of the second collector is 0.8-1.6 kg / t of raw ore; in each positive flotation and concentrating step, the amount of the positive flotation pH adjuster is 0.3-0.8 kg / t of raw ore, and the amount of the organosilicon inhibitor is 0.4-1.0 kg / t of raw ore. The roughing and two concentrating steps of the positive flotation process of the present invention require the addition of sodium carbonate and organosilicon inhibitors.
[0025] Preferably, in step S3, the temperature of the positive flotation is 20-60°C, the rotation speed is 1000-2000 r / min, and the aeration volume is 0.06-0.12 m 3 / h.
[0026] The invention aims at the technical problem that collophanite rich in calcium and magnesium silicate minerals is difficult to be efficiently separated and utilized. During the ore grinding, a ball mill and an ultra-vertical stirring mill are used for fine grinding, sulfuric acid is added for acid washing and dissociation in the reverse flotation roughing, after the sulfuric acid is added, the reverse flotation can inhibit the floating of fluoroapatite, thereby improving the reverse flotation concentrate yield and recovery rate; and after the dolomite and olivine react with the sulfuric acid, there is no calcium and magnesium active particles, and during the direct flotation, they cannot be adsorbed by a fatty acid collector and float with apatite, thereby reducing the impurities in the direct flotation concentrate.
[0027] The invention uses collophanite rich in calcium magnesium silicate minerals as raw ore, and uses sulfuric acid, anion collector, sodium carbonate, organosilicon inhibitor, and fatty acid collector as treatment agents. It is easy to industrialize on site and has good industrial application prospects. The invention effectively solves the problems of complex mineral symbiosis and interference of dolomite on desiliconization flotation, and realizes efficient sorting and utilization of calcium magnesium silicate collophanite containing phosphate resources.
[0028] The present invention is further described in detail below through specific examples and comparative examples. In the collophanite ore rich in calcium magnesium silicate minerals used in each embodiment and comparative example, the grade of P2O5 is 17.517%, the content of SiO2 is as high as 31.159%, and the grade of MgO is 4.778%; Anionic collector MG-7 and fatty acid collector MG-3 were purchased from Wuhan Wojuesheng Mining Technology Co., Ltd. The mass concentration of sulfuric acid solution is 20%.
[0029] Example 1 A method for separating collophanite rich in calcium magnesium silicate minerals, wherein the calcium magnesium silicate collophanite is subjected to reverse flotation, wherein the reverse flotation includes a roughing step, specifically comprising the following steps: S1. The collophanite ore rich in calcium magnesium silicate minerals is crushed, ball milled and ground with an ultrafine vertical stirred mill to separate the constituent mineral monomers. The grinding fineness is -0.037mm and the content is 84.01%. Water is added to adjust the slurry to obtain a slurry with a concentration of 40%; S2, reverse flotation: the slurry flows into the flotation stirring tank of the mechanical agitator flotation machine, and the adjusting agent sulfuric acid solution and the anion collector MG-7 are added thereto respectively. The amount of sulfuric acid solution added is 15 kg / t of the original ore, the pH is adjusted to 3.5, the reaction time of pickling dissociation is 10min, and the amount of anion collector MG-7 added is 3.0kg / t of the original ore. The slurry is adjusted to obtain the first slurry material; the first slurry material enters the reverse flotation system for reverse flotation, the reverse flotation speed is 1200r / min, and the aeration volume is 0.08-0.09m 3 / h, the flotation temperature is room temperature, the obtained foam product is the flotation tailings of carbonate gangue minerals, which is discharged and piled up; the product in the tank is the reverse flotation concentrate, which is dried to obtain the finished phosphate concentrate.
[0030] Comparative Example 1 Compared with Example 1, the only difference is that the amount of sulfuric acid solution added is adjusted to 3 kg / t of raw ore; the other steps and conditions are the same as those in Example 1.
[0031] Example 2 A method for separating collophanite rich in calcium magnesium silicate minerals, which performs reverse flotation and direct flotation on the calcium magnesium silicate collophanite, specifically comprising the following steps: S1. The collophanite ore rich in calcium magnesium silicate minerals is crushed, ball milled and ground with an ultrafine vertical stirred mill to separate the constituent mineral monomers. The grinding fineness is -0.037mm and the content is 84.01%. Water is added to adjust the slurry to obtain a slurry with a concentration of 40%; S2, reverse flotation (one roughing + one concentrating): the slurry flows into the flotation stirring tank of the mechanical agitator flotation machine, and the adjusting agent sulfuric acid solution and the anion collector MG-7 are added thereto respectively. The amount of sulfuric acid solution added is 15 kg / t of the original ore, the pH is adjusted to 3.5, the reaction time of pickling dissociation is 10min, and the amount of anion collector MG-7 added is 2.5kg / t of the original ore. The slurry is adjusted to obtain the first slurry material; the first slurry material enters the reverse flotation system for reverse flotation, the reverse flotation speed is 1200r / min, and the aeration volume is 0.08-0.09m 3 / h, flotation temperature is room temperature, the obtained foam product is carbonate gangue mineral flotation tailings, which are discharged and piled up; the product in the tank is roughing concentrate, and the roughing concentrate is further added with anion collector MG-7 0.5kg / t original ore for reverse flotation. The foam product is tailings, and the product in the tank is reverse flotation concentrate.
[0032] S3, positive flotation (one roughing + one sweeping + two cleaning): S31, the reverse flotation concentrate is added to the flotation tank, and then 9.25kg / t of sodium carbonate, a pH adjuster, is added thereto to adjust the pH value to 10.25, and then 4kg / t of sodium methyl silicate, an organosilicon inhibitor, and 1.0kg / t of fatty acid collector MG-3 are added to adjust the slurry to obtain the second slurry material; the second slurry material enters the positive flotation system for positive flotation roughing, and the positive flotation system adopts a mechanical stirring flotation machine, the positive flotation speed is 1500r / min, and the inflation volume is 0.08-0.09m 3 / h, flotation temperature 50℃; S32, the product in the tank of direct flotation roughing is roughing tailings. Collector MG-3 1.2kg / t of raw ore is added to the roughing tailings to continue scavenging. The product in the scavenging tank is tailings discharged and piled up, and the foam product is middlings, which are collected after filtration; S33. The foam product of the roughing of direct flotation is the roughing concentrate. The roughing concentrate is subjected to two rounds of cleaning. 0.5kg / t of sodium carbonate and 0.67kg / t of sodium methyl silicate are added each time. The final product in the tank is the direct flotation tailings, and the foam product is the direct flotation concentrate. The direct flotation concentrate is concentrated, filtered and dried to obtain the finished phosphate concentrate.
[0033] Comparative Example 2 The difference from Example 2 is that the process sequence of steps S3 and S2 is exchanged, and the relevant raw materials need to be adaptively adjusted; the difference is that: S2, positive flotation (one roughing + one sweeping + two cleaning): S21, the slurry flows into the flotation stirring tank of the mechanical stirring flotation machine, and 1kg / t sodium carbonate as pH adjuster is added to adjust the pH value to 10.25, and then 4kg / t of organosilicon inhibitor and 0.8kg / t of fatty acid collector MG-3 are added to adjust the slurry. The adjusted slurry enters the positive flotation system for flotation. The positive flotation system adopts a mechanical stirring flotation machine with an impeller speed of 1500r / min and an aeration volume of 0.08-0.09m 3 / h, flotation temperature 50℃; S22, the product in the tank of direct flotation roughing is roughing tailings. Collector MG-3 1.2kg / t of raw ore is added to the roughing tailings to continue scavenging. The product in the scavenging tank is tailings discharged and piled up, and the foam product is middling ore; S23. The foam product of the direct flotation roughing is the roughing concentrate. The roughing concentrate is subjected to two rounds of cleaning. Each time, 0.5kg / t of sodium carbonate and 0.67kg / t of sodium methyl silicate are added respectively. The final product in the tank is the direct flotation tailings and the foam product is the direct flotation concentrate.
[0034] S3, reverse flotation (one roughing + one concentrating): the positive flotation concentrate is added to the flotation tank, and then the adjusting agent sulfuric acid solution and anion collector MG-7 are added thereto respectively. The amount of sulfuric acid solution added is 12.5 kg / t of raw ore, the pH is adjusted to 3.5, the reaction time of pickling dissociation is 10min, the amount of anion collector MG-7 added is 2.5kg / t of raw ore, and the slurry is adjusted. After slurry adjustment, the material enters the reverse flotation system for reverse flotation of carbonate gangue minerals. The reverse flotation speed is 1200r / min, and the aeration volume is 0.08-0.09m 3 / h, flotation temperature is room temperature, the obtained foam product is carbonate gangue mineral flotation tailings, which are discharged and piled up; the product in the tank is roughing concentrate, and the roughing concentrate is further added with anion collector MG-7 0.5kg / t original ore for reverse flotation selection. The foam product is tailings, and the product in the tank is reverse flotation concentrate, which is dried to obtain finished phosphate concentrate.
[0035] Comparative Example 3 The difference from Example 2 is that the organosilicon inhibitor sodium methyl silicate is replaced by sodium silicate, and the other steps and conditions are the same as those of Example 3.
[0036] Comparative Example 4 The difference from Example 2 is that the grinding fineness is adjusted to -200 mesh accounting for 84%, and the other steps and conditions are the same as those of Example 3.
[0037] The phosphate concentrate obtained in the above examples and comparative examples was tested by ammonium phosphomolybdate volumetric method, and the results are shown in Table 1 below.
[0038] Table 1 Test results of phosphate concentrate obtained in Examples and Comparative Examples
[0039] As can be seen from Table 1, the amount of sulfuric acid solution used in Comparative Example 1 is insufficient relative to that in Example 1, resulting in a decrease in the yield and recovery rate of the phosphate concentrate.
[0040] Comparative Example 2 changes the process sequence relative to Example 2, with forward flotation first and then reverse flotation. Sulfuric acid cannot fully inhibit the flotation of fluoroapatite to increase the yield and recovery rate of phosphate concentrate, and dolomite, olivine, etc. still have calcium and magnesium active particles, resulting in more impurities in the obtained phosphate concentrate and lower P2O5 grade.
[0041] Comparative Example 3 changed the type of organosilicon inhibitor relative to Example 2, resulting in a decrease in the grade of phosphate concentrate and a decrease in the recovery rate.
[0042] Comparative Example 4 did not fully refine the ore, resulting in the inability to effectively dissociate apatite from dolomite, olivine, anorthite, etc. during pickling dissociation, thereby affecting the grade and recovery rate of the phosphate concentrate.
[0043] Comparative Example 5 Compared with Example 1, the only difference is that the sulfuric acid solution is replaced by hydrochloric acid solution and phosphoric acid solution; the other steps and conditions are the same as those in Example 1.
[0044] The results showed that hydrochloric acid, phosphoric acid, sulfuric acid, etc. can all be used as inhibitors, but hydrochloric acid has a poor inhibitory effect, and phosphoric acid has a high cost. Sulfuric acid can extract part of the phosphate rock into phosphoric acid, and sulfuric acid reacts with dolomite to form calcium sulfate, which increases the dissociation degree of gangue minerals and enables dolomite to be better floated and separated, overcoming the defects of dolomite and quartz that are difficult to remove.
[0045] The present invention provides a method for separating collophanite rich in calcium magnesium silicate minerals, wherein the collophanite ore rich in calcium magnesium silicate minerals is crushed and ultra-finely ground, sulfuric acid is added for pickling, and an anion collector is used for slurry adjustment, and the material after slurry adjustment is subjected to reverse flotation to remove magnesium, and the product in the tank is a reverse flotation concentrate; sodium carbonate, organic silicon inhibitors, and fatty acid collectors are added to the reverse flotation concentrate for slurry adjustment, and positive flotation desiliconization is performed after slurry adjustment, and the foam is a positive flotation concentrate, and the phosphate concentrate product is obtained through concentration, filtration, and drying. The present invention performs ultra-fine grinding and pickling on the collophanite rich in calcium magnesium silicate minerals and having a complex symbiotic relationship, and realizes the dissociation of apatite and calcium magnesium silicate minerals such as olivine and anorthite in the collophanite; pickling and adding organic silicon inhibitors overcome the problem that the interface properties of calcium magnesium silicate gangue and collophanite are similar, improves the sorting property of flotation, and improves the concentrate yield, grade, and recovery rate indicators.
[0046] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for separating collophanite rich in calcium magnesium silicate minerals, characterized in that: The following steps are involved: S1, crushing, ball milling, ultrafine grinding and slurry preparation of collophanite ore rich in calcium magnesium silicate minerals to obtain slurry; S2, acid-washing and dissociating the slurry, adding a first collector to obtain a first slurry material, and performing reverse flotation to obtain a reverse flotation concentrate; and / or, S3, adding a forward flotation pH adjuster to the reverse flotation concentrate, and then adding an organosilicon inhibitor and a second collector to obtain a second slurry material, and performing forward flotation to obtain a forward flotation concentrate; The reverse flotation concentrate and / or the direct flotation concentrate is post-processed to obtain phosphate concentrate.
2. The method for separating collophanite rich in calcium magnesium silicate minerals according to claim 1, characterized in that: In step S1, the ultrafine grinding has a grinding fineness of -0.037 mm and a content of 60% to 98%.
3. The method for separating collophanite rich in calcium magnesium silicate minerals according to claim 1, characterized in that: In step S1, the concentration of the slurry is 35-40%.
4. The method for separating collophanite rich in calcium magnesium silicate minerals according to claim 1, characterized in that: In step S2, the pickling dissociation is to add acid to the slurry to adjust the pH value to 0.5-5; The acid solution is a sulfuric acid solution with a mass concentration of 20%; The pickling dissociation time is 5 to 30 minutes; The first collector is an anionic collector MG-7.
5. The method for separating collophanite rich in calcium magnesium silicate minerals according to claim 1, characterized in that: In step S2, reverse flotation comprises the following steps: The first slurry material is subjected to reverse flotation roughing to obtain reverse flotation concentrate, wherein the dosage of the first collector is 2.5-3.5 kg / t of raw ore; or, The first slurry material is subjected to reverse flotation roughing to obtain a roughing concentrate and a foam tailing, and the roughing concentrate is added with a first collector for reverse flotation concentration to obtain a reverse flotation concentrate; the amount of the first collector in the reverse flotation roughing is 1.5-2.5 kg / t of original ore, and the amount of the first collector in the reverse flotation concentration is 0.4-0.6 kg / t of original ore.
6. The method for separating collophanite rich in calcium magnesium silicate minerals according to claim 1, characterized in that: In step S2, the speed of reverse flotation is 800-1600 r / min, and the aeration volume is 0.06-0.12 m 3 / h.
7. The method for separating collophanite rich in calcium magnesium silicate minerals according to claim 1, characterized in that: In step S3, the forward flotation pH adjuster includes sodium carbonate; the forward flotation pH adjuster is added to the reverse flotation concentrate to adjust the pH value to 9.5-11; The organosilicon inhibitor includes methyl silicate; The second collector includes a fatty acid collector.
8. The method for separating collophanite rich in calcium magnesium silicate minerals according to claim 1, characterized in that: In step S3, the positive flotation specifically includes the following steps: The second slurry material is subjected to roughing to obtain roughing tailings and roughing concentrate; The roughing tailings are added with a second collector for scavenging to obtain tailings in the first tank and foamed middlings; The roughing concentrate is added with a positive flotation pH adjuster and an organosilicon inhibitor, and is subjected to 1-2 positive flotation concentrations to obtain tailings in the second tank and a positive flotation concentrate.
9. The method for separating collophanite rich in calcium magnesium silicate minerals according to claim 8, characterized in that: In the roughing step, the dosage of the organosilicon inhibitor is 1-5 kg / t of raw ore, and the dosage of the second collector is 0.5-1.4 kg / t of raw ore; in the scavenging step, the dosage of the second collector is 0.8-1.6 kg / t of raw ore; in each positive flotation selection step, the dosage of the positive flotation pH adjuster is 0.3-0.8 kg / t of raw ore, and the dosage of the organosilicon inhibitor is 0.4-1.0 kg / t of raw ore.
10. The method for separating collophanite rich in calcium magnesium silicate minerals according to claim 1, characterized in that: The temperature of positive flotation is 20~60℃, the speed is 1000~2000r / min, and the aeration volume is 0.06~0.12m 3 / h.
Citation Information
Patent Citations
Phosphate rock floating process
CN101020159A
Reverse / direct flotation technology of collophanite
CN102744152A
Flotation technology for removing sesquioxides and magnesium impurities in silicon-calcium collophanite
CN110142145A
Silicate mineral inhibitor and preparation method thereof, and application of silicate mineral inhibitor
CN110947519A
Method for preparing phosphoric acid and derivatives thereof from phosphorite
CN116768170A