Lubricating layer for hot drawing of titanium alloy pipe and preparation method of lubricating layer

By forming a composite lubricating layer of porous molybdenum disulfide sheet and hydrolyzed latex particles combined with carbon aqueous slurry on the surface of the titanium alloy pipe, the poor lubrication effect and cleaning problems during the thermal drawing of titanium alloy pipes are solved, and the surface is improved Flatness and material yield reduce production costs.

CN118950428APending Publication Date: 2024-11-15ZHONGSHAN (CHANGZHOU) NEW MATERIAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411018774.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

During the thermal drawing process of existing titanium alloy pipes, the lubricant has poor thermal drawing effect, easy scratches on the surface and difficulty in removing cleaning, which affects product quality and material yield.

Method used

Porous molybdenum disulfide sheets and hydrolyzed latex particles are combined with carbon aqueous slurry to form a composite lubricating layer through chemical bonding, reducing surface scratches and simplifying the cleaning process.

Benefits of technology

The surface flatness and lubrication effect of the thermal drawing process are improved, the subsequent cleaning process is simplified, and the production cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950428A_ABST
    Figure CN118950428A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lubricant materials for hot drawing of pipes, in particular to a lubricating layer for hot drawing of a titanium alloy pipe and a preparation method of the lubricating layer. The lubricating layer for hot drawing of the titanium alloy pipe comprises a bottom coating, a middle layer and a surface layer, the bottom coating is a coupling agent treatment layer, the middle layer comprises porous molybdenum disulfide sheets and hydrolytic latex particles, and the middle layer is formed by connecting the porous molybdenum disulfide sheets through the hydrolytic latex particles; the surface of the porous molybdenum disulfide sheet is modified and connected with an interface modifier; the carbon aqueous slurry comprises graphite and / or graphene oxide. According to the invention, by selecting a proper lubricant and a coating manufacturing technology, the surface scratch of the product in the hot drawing process is reduced. And the surface treatment of the product after drawing is convenient, the subsequent surface cleaning procedure is simplified, and the overall production cost is saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lubricant materials for hot drawing of pipes, and in particular to a method for preparing a lubricating layer for hot drawing of titanium alloy pipes. Background Art

[0002] At present, in the field of titanium alloy pipe manufacturing, rolling processing is mostly used for production, but it has the disadvantages of insufficient flexibility for small batch products and high tooling costs, and special-shaped products (square, rectangular, etc.) cannot be produced by rolling. The existing special-shaped products (square, rectangular, etc.) are basically produced by bending and welding. The performance of special-shaped products formed by bending and welding is worse than that of seamless pipes, and the processing efficiency is low, and the yield rate is not high.

[0003] In the prior art, the production of titanium alloy pipes and special-shaped pipes is generally cold-drawn, with small deformation and many passes; when hot-drawing is used to produce titanium alloy pipes and special-shaped pipes, liquid lubricants are generally not used. If graphite lubricants are used, they can play a high-temperature lubricating role, but they bring new cleaning problems. If molybdenum disulfide aqueous lubrication is used, there is a problem of poor high-temperature resistance, which affects the quality of titanium alloy pipes and special-shaped pipes. In order to overcome the problems of poor hot-drawing lubrication effect, easy scratches on the surface, and difficult removal of lubricants that adhere to the surface in the prior art, the inventor provides a method for preparing a lubricating layer for hot-drawing of titanium alloy pipes. Summary of the invention

[0004] In order to solve the above technical problems, the present application provides a lubricating layer for hot drawing of titanium alloy pipes and a preparation method thereof.

[0005] The present application provides a method for preparing a lubricating layer for hot drawing of a titanium alloy tube, which is achieved by the following scheme:

[0006] A lubricating layer for hot drawing of titanium alloy pipes, comprising a primer layer, an intermediate layer and a surface layer, wherein the primer layer is a coupling agent treatment layer, wherein the coupling agent treatment layer is connected to the surface of the titanium alloy pipe by a hydrolyzed coupling agent through a chemical bond; the coupling agent used in the coupling agent treatment layer is at least one of a titanate coupling agent, an aminosilane coupling agent and a methacryloxysilane; the intermediate layer comprises porous molybdenum disulfide sheets and hydrolyzable latex particles, wherein the porous molybdenum disulfide sheets are connected by the hydrolyzable latex particles to form the intermediate layer; The surface of the porous molybdenum disulfide sheet is modified and connected with an interface modifier; the interface modifier is at least one of dopamine, linear polyethylene glycol, polyimide, chitosan, hyaluronic acid, and polylactic acid; the surface layer is made of carbon aqueous slurry; the carbon aqueous slurry includes graphite and / or graphene oxide, and the graphite is at least one of hydroxylated modified graphite, carboxylated graphite, and amino graphite; the graphene oxide is at least one of hydroxylated modified graphene oxide, carboxylated graphene oxide, and amino graphene oxide.

[0007] Preferably, the coupling agent used in the coupling agent treatment layer is one of titanate coupling agent KR138S and titanate coupling agent KR38S.

[0008] Preferably, the preparation method of the porous molybdenum disulfide sheet is as follows: first prepare nano-scale porous polymolybdate, then use a compound containing a negative divalent sulfur element as a sulfur source aqueous solution combined with a hydrothermal-gas phase in-situ sulfurization method, and use the sulfur source to be thermally decomposed in a hydrothermal system to generate H2S and react with porous molybdic acid aggregates to achieve in-situ sulfurization to obtain a porous molybdenum disulfide nanosheet.

[0009] Preferably, the carbon aqueous slurry includes graphite and graphene oxide, and the mass ratio of the graphite to the graphene oxide is (6-12):1.

[0010] Preferably, the graphite is amino graphite; and the graphene oxide is composed of hydroxylated modified graphene graphite and amino graphene oxide.

[0011] Preferably, the graphene oxide is composed of hydroxylated modified graphene oxide and amino modified graphene oxide in a composition mass ratio of (0.5-2):1.

[0012] The present invention selects suitable lubricants and coating manufacturing technology, first forms a titanate coupling agent bottom layer on the surface of the titanium alloy pipe, the titanate coupling agent bottom layer is a hydrolyzed titanate coupling agent, firmly connects the middle layer and the surface of the titanium alloy pipe together, and applies a carbon aqueous slurry on the surface of the middle layer at low temperature. The porous molybdenum disulfide sheet and hydrolyzed latex particles in the middle layer are chemically bonded with the surface-modified graphite and / or graphene oxide, and the graphite and / or graphene oxide are relatively uniformly fixed to form a composite lubricating layer, thereby reducing surface scratches in the product hot drawing process. It also makes the surface treatment of the product after drawing convenient, simplifies the subsequent surface cleaning process, and saves the overall production cost.

[0013] A method for preparing a lubricating layer for hot drawing of a titanium alloy pipe comprises the following steps:

[0014] Step 1, performing sandblasting on the surface of the titanium alloy raw material pipe, and then cleaning and drying it after sandblasting for standby use;

[0015] Step 2: placing the titanium alloy raw material pipe in a hydrolytic coupling agent liquid for ultrasonic dispersion treatment and drying to form a primer layer;

[0016] Step 3: The porous molybdenum disulfide sheet treated with hydrolyzed latex particles is mixed with a polymer colloidal emulsion, a suspending agent, and a dispersing agent to form a slurry, the obtained slurry is evenly coated on a release paper and dried to form a semi-cured film, and the obtained semi-cured film is coated on the primer layer of the titanium alloy raw material pipe and hot-pressed and dried to form an intermediate layer;

[0017] Step 4: coating the carbon aqueous slurry on the middle layer of the titanium alloy raw material pipe and drying it to form a surface layer; the base coating, the middle layer and the surface layer are composited to form a lubricating layer for hot drawing of the finished titanium alloy pipe.

[0018] The preparation method of the present invention is relatively simple, has relatively low operating difficulty, and is easy to implement industrial production.

[0019] Preferably, the polymer colloidal emulsion in the slurry prepared in step 3 is an aqueous polyurethane emulsion, the diameter of the polyurethane latex particles contained in the aqueous polyurethane emulsion is 100-300nm, and the glass transition temperature Tg≤0°C; the suspending agent is xanthan gum and / or konjac gum; the dispersant is deionized water or a mixed dispersant formed by water and acetone in a volume ratio of (1-4): (0.5-2).

[0020] Preferably, the polyurethane latex particles in the slurry prepared in step three have a content of 0.6-1.2wt%, and the suspending agent content has a content of 0.05-0.15wt%.

[0021] By adopting the above technical solution, the surface of the porous molybdenum disulfide sheet is chemically bonded with the interface modifier, the interface modifier is chemically bonded with the polyurethane latex particles, the void structure on the surface of the porous molybdenum disulfide sheet is capillary adsorbed with the polyurethane latex particles, the polyurethane latex particles are chemically bonded with the surface-modified graphite and / or graphene oxide in the carbon aqueous slurry, and the graphite and / or graphene oxide are relatively evenly fixed to form a composite lubricating layer, which can further reduce the surface scratches during the hot drawing process of the product. In addition, the hydrolyzed latex particles contained in the slurry are degraded in a weakly alkaline environment at 50-70°C, making the surface cleaning of the product after drawing convenient and efficient, simplifying the subsequent surface cleaning process, and saving overall production costs.

[0022] Preferably, the slurry in step 3 comprises deionized water, an emulsifier, a surface-modified porous molybdenum disulfide sheet, polyurethane acrylate, epoxy-modified acrylate, 1,6-hexanediol diacrylate, tripropylene glycol diacrylate, polyethylene glycol, and 2-hydroxy-2-methyl-1-phenyl-1-propanone, and the solid content is controlled at 10-35%;

[0023] In the step 3, the interface modifier is first prepared into a 4-8wt% interface modifier aqueous solution, 1-2 parts of the porous molybdenum disulfide sheet is mixed with 10 parts of the 4-8wt% interface modifier aqueous solution, and ultrasonic dispersion treatment is performed for 5-15 minutes, and the semi-finished surface-modified porous molybdenum disulfide sheet is obtained by draining, taking out, and drying;

[0024] The aqueous polyurethane emulsion with a solid content of 20-45% is diluted with deionized water to a 0.1-0.5wt% solid content aqueous polyurethane emulsion, 5-10 parts of porous molybdenum disulfide sheets are placed in 80-100 parts of the 0.1-0.5wt% solid content aqueous polyurethane emulsion for ultrasonic dispersion treatment for 5-15 minutes, drained, taken out, and dried to obtain a finished surface-modified porous molybdenum disulfide sheet, and the finished surface-modified porous molybdenum disulfide sheet is placed in the aqueous polyurethane emulsion. , deionized water, emulsifier, polyurethane acrylate, epoxy modified acrylate, 1,6-hexanediol diacrylate, tripropylene glycol diacrylate, polyethylene glycol, and 2-hydroxy-2-methyl-1-phenyl-1-propanone are prepared into a slurry with a solid content controlled at 10-35%, the obtained slurry is evenly coated on release paper and dried to form a semi-cured film with a thickness of 20-60 microns, and the obtained semi-cured film is coated on the base coating of the titanium alloy raw material pipe and hot-pressed and dried to form an intermediate layer.

[0025] By adopting the above technical solution, the intermediate layer formed by the semi-cured film coating and hot pressing and drying has excellent flatness as a whole compared with the intermediate layer formed by the coating method, and can effectively improve the uniformity of graphite and / or graphene oxide, and can further reduce surface scratches during the hot drawing process of the product.

[0026] In summary, this application has the following advantages:

[0027] 1. The present invention reduces surface scratches during the hot drawing process of the product by selecting suitable lubricants and coating manufacturing technology. It also facilitates the surface treatment of the product after drawing, simplifies the subsequent surface cleaning process, and saves overall production costs.

[0028] 2. The preparation method of the present invention is relatively simple, the operation difficulty is relatively low, and it is easy to realize industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 Schematic diagram of the surface morphology of the titanium alloy tube after sandblasting in Example 1.

[0030] Figure 2 It is a schematic diagram of the surface morphology of the titanium alloy tube after auxiliary ultrasonic cleaning after hot drawing in Example 1.

[0031] Figure 3 This is a schematic diagram of the surface morphology of the titanium alloy tube in the control group after auxiliary ultrasonic cleaning after hot drawing. DETAILED DESCRIPTION

[0032] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples and comparative examples.

[0033] Example

[0034] A lubricating layer for hot drawing of a titanium alloy pipe comprises a base coating, an intermediate layer and a surface layer.

[0035] The primer layer is a coupling agent treatment layer, which uses a hydrolyzed coupling agent to connect with the surface of the titanium alloy pipe through a chemical bond; the coupling agent used in the coupling agent treatment layer is at least one of a titanate coupling agent, an aminosilane coupling agent, and a methacryloxysilane.

[0036] The middle layer includes porous molybdenum disulfide sheets and hydrolyzable latex particles, and the porous molybdenum disulfide sheets are connected by the hydrolyzable latex particles to form the middle layer. The preparation method of the porous molybdenum disulfide sheet is as follows: first prepare nano-scale porous polymolybdate, then use a compound containing a negative divalent sulfur element as a sulfur source aqueous solution combined with a hydrothermal-gas phase in-situ vulcanization method, and use the sulfur source to be thermally decomposed in a hydrothermal system to generate H2S and react with porous molybdic acid aggregates to achieve in-situ vulcanization to obtain a porous molybdenum disulfide nanosheet. The surface of the porous molybdenum disulfide sheet is modified and connected with an interface modifier. The interface modifier is at least one of dopamine, linear polyethylene glycol, polyimide, chitosan, hyaluronic acid, and polylactic acid.

[0037] The surface layer is made of carbon aqueous slurry. The carbon aqueous slurry includes graphite and / or graphene oxide. Graphite is at least one of hydroxylated modified graphite, carboxylated graphite, and amino graphite. Graphene oxide is at least one of hydroxylated modified graphene oxide, carboxylated graphene oxide, and amino graphene oxide. Preferably, the carbon aqueous slurry includes graphite and graphene oxide, and the mass ratio of graphite to graphene oxide is (6-12):1. Graphite is amino graphite; graphene oxide is composed of hydroxylated modified graphene graphite and amino graphene oxide. Graphene oxide is composed of hydroxylated modified graphene oxide and amino graphene oxide in a composition mass ratio of (0.5-2):1.

[0038] A method for preparing a lubricating layer for hot drawing of a titanium alloy pipe comprises the following steps:

[0039] Step 1, performing sandblasting on the surface of the titanium alloy raw material pipe, and then cleaning and drying it after sandblasting for standby use;

[0040] Step 2: placing the titanium alloy raw material pipe in a hydrolytic coupling agent liquid for ultrasonic dispersion treatment and drying to form a primer layer;

[0041] Step 3: The porous molybdenum disulfide sheet treated with hydrolyzed latex particles is mixed with a polymer colloidal emulsion, a suspending agent, and a dispersing agent to form a slurry, the obtained slurry is evenly coated on a release paper and dried to form a semi-cured film, and the obtained semi-cured film is coated on the primer layer of the titanium alloy raw material pipe and hot-pressed and dried to form an intermediate layer;

[0042] Preferably, the polymer colloidal emulsion in the slurry prepared in step 3 is an aqueous polyurethane emulsion, the diameter of the polyurethane latex particles contained in the aqueous polyurethane emulsion is 100-300nm, and the glass transition temperature Tg≤0°C; the suspending agent is xanthan gum and / or konjac gum; the dispersant is deionized water or a mixed dispersant formed by water and acetone in a volume ratio of (1-4): (0.5-2); the polyurethane latex particle content in the prepared slurry is 0.6-1.2wt%, and the suspending agent content is 0.05-0.15wt%;

[0043] Specifically, the slurry in step 3 includes deionized water, an emulsifier, a surface-modified porous molybdenum disulfide sheet, polyurethane acrylate, epoxy-modified acrylate, 1,6-hexanediol diacrylate, tripropylene glycol diacrylate, polyethylene glycol, and 2-hydroxy-2-methyl-1-phenyl-1-propanone, and the solid content is controlled at 10-35%;

[0044] In step 3, the interface modifier is first prepared into a 4-8wt% interface modifier aqueous solution, 1-2 parts of the porous molybdenum disulfide sheet is mixed with 10 parts of the 4-8wt% interface modifier aqueous solution, and ultrasonic dispersion treatment is performed for 5-15 minutes, and the semi-finished surface-modified porous molybdenum disulfide sheet is obtained by draining, taking out, and drying;

[0045] The aqueous polyurethane emulsion with a solid content of 20-45% is diluted with deionized water to a 0.1-0.5wt% solid content aqueous polyurethane emulsion, 5-10 parts of porous molybdenum disulfide sheets are placed in 80-100 parts of the 0.1-0.5wt% solid content aqueous polyurethane emulsion for ultrasonic dispersion treatment for 5-15 minutes, drained, taken out, and dried to obtain a finished surface-modified porous molybdenum disulfide sheet, and the finished surface-modified porous molybdenum disulfide sheet is placed in the aqueous polyurethane emulsion. , deionized water, emulsifier, polyurethane acrylate, epoxy modified acrylate, 1,6-hexanediol diacrylate, tripropylene glycol diacrylate, polyethylene glycol, 2-hydroxy-2-methyl-1-phenyl-1-propanone are prepared into a slurry with a solid content of 10-35%, the obtained slurry is evenly coated on release paper and dried to form a semi-cured film with a thickness of 20-60 microns, and the obtained semi-cured film is coated on the primer layer of the titanium alloy raw material pipe and hot-pressed and dried to form an intermediate layer;

[0046] Step 4: coating the carbon aqueous slurry on the middle layer of the titanium alloy raw material pipe and drying it to form a surface layer; the base coating layer, the middle layer and the surface layer are composited to form a lubricating layer for hot drawing of the finished titanium alloy pipe.

[0047] Embodiment 1: A lubricating layer for hot drawing of titanium alloy pipes includes a primer, an intermediate layer, and a surface layer. The primer is formed by a titanate coupling agent KR138S. The intermediate layer includes porous molybdenum disulfide sheets and hydrolyzable latex particles, and the porous molybdenum disulfide sheets are connected by the hydrolyzable latex particles to form the intermediate layer. The surface of the porous molybdenum disulfide sheet is modified with an interface modifier dopamine, and the dopamine is chemically bonded with polyurethane latex particles, and the surface of the porous molybdenum disulfide sheet also adsorbs polyurethane latex particles. The surface layer is made of carbon aqueous slurry, and the carbon aqueous slurry is made of 5wt% carboxylated graphite (800 mesh flake graphite obtained by oxidation treatment with potassium permanganate), 0.1wt% xanthan gum, and 94.9wt% deionized water.

[0048] A method for preparing a lubricating layer for hot drawing of a titanium alloy pipe comprises the following steps:

[0049] Step 1, sandblasting the surface of the titanium alloy raw material pipe, first using 100 mesh corundum for sandblasting, then using 325 mesh corundum for sandblasting, and finally using 2000 mesh corundum for sandblasting twice, so that the surface roughness of the titanium alloy pipe after sandblasting is Ra1.0-Ra2.5, the titanium alloy raw material pipe after sandblasting is washed with deionized water, and the obtained titanium alloy raw material pipe is placed at 80°C for drying and standby;

[0050] Step 2: dissolving titanate coupling agent KR138S in deionized water to prepare a 5wt% titanate coupling agent KR138S aqueous solution, placing the titanium alloy raw material pipe in the 5wt% titanate coupling agent KR138S aqueous solution, performing ultrasonic dispersion treatment at a water temperature of 40°C for 5 minutes, an ultrasonic frequency of 40kHz, and a power of 800W. After the ultrasonic dispersion treatment, the obtained titanium alloy raw material pipe is placed at 80°C for drying to form a primer coating on the titanium alloy raw material pipe for standby use;

[0051] The porous molybdenum disulfide sheet is prepared as follows: 3 g of ammonium molybdate tetrahydrate and 6 g of sodium chloride are weighed and dissolved in 50 mL of deionized water respectively, and the mixture is mixed under magnetic stirring. When the temperature is raised to 70°C, the clear solution begins to become turbid, and white floccules precipitate after a few minutes. The reaction is stopped for 0.5 h, filtered while hot, washed with deionized water for multiple times to obtain a white flocculent solid, and dried at room temperature to obtain a nano-porous polymolybdate; 5.07 g of nano-polymolybdate and 15.1 g of thiourea are weighed, the nano-porous polymolybdate is put into a polytetrafluoroethylene beaker, thiourea is added to the lining of a polytetrafluoroethylene reactor, and 2 g of deionized water is poured into the slurry. Then, the beaker containing the nano-porous polymolybdate was placed in a polytetrafluoroethylene reactor in a nested relationship, and the reaction was carried out at 180°C for 48 hours. After the reaction was completed, the product was cooled to room temperature, and the obtained product was washed with ammonia water, deionized water and anhydrous ethanol for multiple times in sequence, dried at 60°C, and then placed in a planetary ball mill at 60 rpm for 15 minutes to obtain porous defect-rich molybdenum disulfide;

[0052] Step 3: first prepare a 5wt% dopamine aqueous solution, mix 5g of a porous molybdenum disulfide sheet with 100g of a 5wt% dopamine aqueous solution, add a 3wt% potassium hydroxide aqueous solution to adjust the pH value of the system to 10, heat to 65°C and perform ultrasonic dispersion treatment for 5min, the ultrasonic frequency is 40kHz, the power is 800W, drain, take out, and place at 80°C to dry to obtain a semi-finished surface-modified porous molybdenum disulfide sheet;

[0053] 50wt% high solid content soft resin FS-151650 ordered by Qingdao Ruikesi New Material Technology Co., Ltd. was diluted with deionized water to a 0.5wt% solid content aqueous polyurethane emulsion, 5g of the semi-finished surface modified porous molybdenum disulfide sheet was placed in 100g of the 0.5wt% solid content aqueous polyurethane emulsion for ultrasonic dispersion treatment for 10min, the ultrasonic frequency was 40kHz, the power was 800W, drained, taken out, and placed at 80°C for drying to obtain the finished surface modified porous molybdenum disulfide sheet;

[0054] 17 g of the obtained finished surface-modified porous molybdenum disulfide sheet, 70 g of deionized water, 2 g of emulsifier OP, 1 g of TX-4 alkylphenol polyoxyethylene ether, 6 g of polyurethane acrylate, 1.5 g of epoxy-modified acrylate, 1 g of 1,6-hexanediol diacrylate, 0.5 g of tripropylene glycol diacrylate, 0.6 g of polyethylene glycol PEG600, and 0.4 g of 2-hydroxy-2-methyl-1-phenyl-1-propanone are prepared into a slurry with a solid content of 30 wt %, the obtained slurry is evenly coated on a release paper, and is placed at 60° C. and dried to form a semi-cured film with a thickness of 30-35 μm, and the obtained semi-cured film is coated on the primer layer of the titanium alloy raw material pipe, and is hot-pressed and dried to form an intermediate layer;

[0055] Step 4, 5g of 800 mesh flake graphite is placed in 50ml of 10wt% potassium permanganate aqueous solution, heated to 60°C and oxidized for 30min under 200rpm magnetic stirring to obtain carboxylated graphite, 50g of carboxylated graphite, 1g of xanthan gum, and 949g of deionized water are prepared into a carbon aqueous slurry, and the obtained carbon aqueous slurry is coated on the middle layer of the titanium alloy raw material pipe and dried to form a surface layer with a thickness of 45-50 microns, that is, a lubricating layer for hot drawing of the titanium alloy pipe is formed on the surface of the titanium alloy pipe.

[0056] The difference between Example 2 and Example 1 is that: Step 2, KH570 coupling agent is dissolved in deionized water to prepare a 5wt% KH570 coupling agent aqueous solution, the titanium alloy raw material pipe is placed in the 5wt% KH570 coupling agent aqueous solution, and ultrasonic dispersion treatment is performed at a water temperature of 40°C for 5 minutes, an ultrasonic frequency of 40kHz, and a power of 800W. After the ultrasonic dispersion treatment, the titanium alloy raw material pipe is placed at 80°C for drying to form a primer coating on the titanium alloy raw material pipe cost for standby use.

[0057] The difference between Example 3 and Example 1 is that: Step 3, first prepare a 5wt% hyaluronic acid solution, mix 5g of the porous molybdenum disulfide sheet with 100g of a 5wt% hyaluronic acid aqueous solution, heat to 40°C and perform ultrasonic dispersion treatment for 5min, ultrasonic frequency 40kHz, power 800W, drain, take out, and place at 80°C to dry to obtain a semi-finished surface-modified porous molybdenum disulfide sheet.

[0058] The difference between Example 4 and Example 1 is that: Step 3, first prepare a 5wt% polyethylene glycol PEG400 solution, mix 5g of the porous molybdenum disulfide sheet with 100g of the 5wt% polyethylene glycol PEG400 aqueous solution, heat to 40°C and perform ultrasonic dispersion treatment for 5min, ultrasonic frequency 40kHz, power 800W, drain, take out, and place at 80°C to dry to obtain a semi-finished surface-modified porous molybdenum disulfide sheet.

[0059] The difference between Example 5 and Example 1 is that in step 3, the 50wt% high-solid soft resin FS-151650 ordered by Qingdao Ruikos New Material Technology Co., Ltd. is diluted with deionized water to become an aqueous polyurethane emulsion with a solid content of 0.1wt%, and 5g of the semi-finished surface-modified porous molybdenum disulfide sheet is placed in 100g of an aqueous polyurethane emulsion with a solid content of 0.1wt% and subjected to ultrasonic dispersion treatment for 10min, with an ultrasonic frequency of 40kHz and a power of 800W. The sheet is drained, taken out, and dried at 80°C to obtain a finished surface-modified porous molybdenum disulfide sheet.

[0060] The difference between Example 6 and Example 1 is that in step 3, the 50wt% high-solid soft resin FS-151650 ordered by Qingdao Ruikos New Material Technology Co., Ltd. is diluted with deionized water to form an aqueous polyurethane emulsion with a solid content of 0.3wt%, and 5g of the semi-finished surface-modified porous molybdenum disulfide sheet is placed in 100g of an aqueous polyurethane emulsion with a solid content of 0.1wt% and subjected to ultrasonic dispersion treatment for 10min, with an ultrasonic frequency of 40kHz and a power of 800W. The sheet is drained, taken out, and dried at 80°C to obtain a finished surface-modified porous molybdenum disulfide sheet.

[0061] The difference between Example 7 and Example 1 is that in step three, 12g of the finished surface modified porous molybdenum disulfide sheet, 70g of deionized water, 2g of emulsifier OP, 1g of TX-4 alkylphenol polyoxyethylene ether, 6g of polyurethane acrylate, 1.5g of epoxy modified acrylate, 1g of 1,6-hexanediol diacrylate, 0.5g of tripropylene glycol diacrylate, 0.6g of polyethylene glycol PEG600, and 0.4g of 2-hydroxy-2-methyl-1-phenyl-1-propanone are configured into a slurry with a solid content controlled at 25wt%, the obtained slurry is evenly coated on a release paper and dried at 60°C to form a semi-cured film with a thickness of 30-35 microns, and the obtained semi-cured film is coated on the base coating of the titanium alloy raw material pipe and hot-pressed and dried to form an intermediate layer.

[0062] The difference between Example 8 and Example 1 is that in step three, 22g of the finished surface modified porous molybdenum disulfide sheet, 70g of deionized water, 2g of emulsifier OP, 1g of TX-4 alkylphenol polyoxyethylene ether, 6g of polyurethane acrylate, 1.5g of epoxy modified acrylate, 1g of 1,6-hexanediol diacrylate, 0.5g of tripropylene glycol diacrylate, 0.6g of polyethylene glycol PEG600, and 0.4g of 2-hydroxy-2-methyl-1-phenyl-1-propanone are configured into a slurry with a solid content controlled at 35wt%, the obtained slurry is evenly coated on a release paper and dried at 60°C to form a semi-cured film with a thickness of 30-35 microns, and the obtained semi-cured film is coated on the primer layer of the titanium alloy raw material pipe and hot-pressed and dried to form an intermediate layer.

[0063] The difference between Example 9 and Example 1 is that: Step 4, 5g of 800 mesh flake graphite is placed in 50ml of 10wt% potassium permanganate aqueous solution, heated to 60°C and oxidized for 30min under 200rpm magnetic stirring to obtain carboxylated graphite, 45g of carboxylated graphite, 2.5g of hydroxyl graphene oxide HGO3111 (Angxing New Carbon Material Changzhou Co., Ltd.), 2.5g of amino graphene oxide (Suzhou Beike Nano Technology Co., Ltd., BKMK2009-02), 1g of xanthan gum, and 949g of deionized water are prepared into a carbon aqueous slurry, and the obtained carbon aqueous slurry is coated on the middle layer of the titanium alloy raw material pipe and dried to form a surface layer with a thickness of 45-50 microns, that is, a lubricating layer for hot drawing of titanium alloy pipe is formed on the surface of the titanium alloy pipe.

[0064] The difference between Example 10 and Example 1 is that: Step 4, 5g of 800 mesh flake graphite is placed in 50ml of 10wt% potassium permanganate aqueous solution, heated to 60°C and oxidized for 30min under magnetic stirring at 200rpm to obtain carboxylated graphite, 2g of 1,6-hexanediamine is added, the temperature is raised to 80°C and oxidized for 30min under magnetic stirring at 200rpm to obtain amino graphite, 45g of amino graphite, 2.5g of hydroxyl graphene oxide HGO3111 (Angxing New Carbon Materials Changzhou Co., Ltd.), 2.5g of amino graphene oxide (Suzhou Beike Nano Technology, BKMK2009-02), 1g of xanthan gum, and 949g of deionized water are prepared into a carbon aqueous slurry, and the obtained carbon aqueous slurry is coated on the middle layer of the titanium alloy raw material pipe and dried to form a surface layer with a thickness of 45-50 microns, that is, a lubricating layer for hot drawing of titanium alloy pipe is formed on the surface of the titanium alloy pipe.

[0065] Comparative Example

[0066] The difference between Comparative Example 1 and Example 1 is that: a method for preparing a lubricating layer for hot drawing of a titanium alloy pipe comprises the following steps:

[0067] Step 1, sandblasting the surface of the titanium alloy raw material pipe, first using 100 mesh corundum for sandblasting, then using 325 mesh corundum for sandblasting, and finally using 2000 mesh corundum for sandblasting twice, so that the surface roughness of the titanium alloy pipe after sandblasting is Ra1.0-Ra2.5, the titanium alloy raw material pipe after sandblasting is washed with deionized water, and the obtained titanium alloy raw material pipe is placed at 80°C for drying and standby;

[0068] The porous molybdenum disulfide sheet is prepared as follows: 3 g of ammonium molybdate tetrahydrate and 6 g of sodium chloride are weighed and dissolved in 50 mL of deionized water respectively, and the mixture is mixed under magnetic stirring. When the temperature is raised to 70°C, the clear solution begins to become turbid, and white floccules precipitate after a few minutes. The reaction is stopped for 0.5 h, filtered while hot, washed with deionized water for multiple times to obtain a white flocculent solid, and dried at room temperature to obtain a nano-porous polymolybdate; 5.07 g of nano-polymolybdate and 15.1 g of thiourea are weighed, the nano-porous polymolybdate is put into a polytetrafluoroethylene beaker, thiourea is added to the lining of a polytetrafluoroethylene reactor, and 2 g of deionized water is poured into the slurry. Then, the beaker containing the nano-porous polymolybdate was placed in a polytetrafluoroethylene reactor in a nested relationship, and the reaction was carried out at 180°C for 48 hours. After the reaction was completed, the product was cooled to room temperature, and the obtained product was washed with ammonia water, deionized water and anhydrous ethanol for multiple times in sequence, dried at 60°C, and then placed in a planetary ball mill at 60 rpm for 15 minutes to obtain porous defect-rich molybdenum disulfide;

[0069] Step 3: first prepare a 5wt% dopamine aqueous solution, mix 5g of a porous molybdenum disulfide sheet with 100g of a 5wt% dopamine aqueous solution, add a 3wt% potassium hydroxide aqueous solution to adjust the pH value of the system to 10, heat to 65°C and perform ultrasonic dispersion treatment for 5min, the ultrasonic frequency is 40kHz, the power is 800W, drain, take out, and place at 80°C to dry to obtain a semi-finished surface-modified porous molybdenum disulfide sheet;

[0070] 50wt% high solid content soft resin FS-151650 ordered by Qingdao Ruikesi New Material Technology Co., Ltd. was diluted with deionized water to a 0.5wt% solid content aqueous polyurethane emulsion, 5g of the semi-finished surface modified porous molybdenum disulfide sheet was placed in 100g of the 0.5wt% solid content aqueous polyurethane emulsion for ultrasonic dispersion treatment for 10min, the ultrasonic frequency was 40kHz, the power was 800W, drained, taken out, and placed at 80°C for drying to obtain the finished surface modified porous molybdenum disulfide sheet;

[0071] 17 g of the obtained finished surface-modified porous molybdenum disulfide sheet, 70 g of deionized water, 2 g of emulsifier OP, 1 g of TX-4 alkylphenol polyoxyethylene ether, 6 g of polyurethane acrylate, 1.5 g of epoxy-modified acrylate, 1 g of 1,6-hexanediol diacrylate, 0.5 g of tripropylene glycol diacrylate, 0.6 g of polyethylene glycol PEG600, and 0.4 g of 2-hydroxy-2-methyl-1-phenyl-1-propanone are prepared into a slurry with a solid content of 30 wt %, the obtained slurry is evenly coated on a release paper, and is placed at 60° C. and dried to form a semi-cured film with a thickness of 30-35 μm, and the obtained semi-cured film is coated on the surface of a titanium alloy raw material pipe and hot-pressed and dried to form an intermediate layer;

[0072] Step 4, 5g of 800 mesh flake graphite is placed in 50ml of 10wt% potassium permanganate aqueous solution, heated to 60°C and oxidized for 30min under 200rpm magnetic stirring to obtain carboxylated graphite, 50g of carboxylated graphite, 1g of xanthan gum, and 949g of deionized water are prepared into a carbon aqueous slurry, and the obtained carbon aqueous slurry is coated on the middle layer of the titanium alloy raw material pipe and dried to form a surface layer with a thickness of 45-50 microns, that is, a lubricating layer for hot drawing of the titanium alloy pipe is formed on the surface of the titanium alloy pipe.

[0073] The difference between Comparative Example 2 and Example 1 is that: a method for preparing a lubricating layer for hot drawing of a titanium alloy tube comprises the following steps:

[0074] Step 1, sandblasting the surface of the titanium alloy raw material pipe, first using 100 mesh corundum for sandblasting, then using 325 mesh corundum for sandblasting, and finally using 2000 mesh corundum for sandblasting twice, so that the surface roughness of the titanium alloy pipe after sandblasting is Ra1.0-Ra2.5, the titanium alloy raw material pipe after sandblasting is washed with deionized water, and the obtained titanium alloy raw material pipe is placed at 80°C for drying and standby;

[0075] Step 2: 5 g of 800 mesh flake graphite is placed in 50 ml of 10 wt% potassium permanganate aqueous solution, heated to 60 ° C and oxidized for 30 min under 200 rpm magnetic stirring to obtain carboxylated graphite; 50 g of carboxylated graphite, 1 g of xanthan gum, and 949 g of deionized water are used to prepare a carbon aqueous slurry; the obtained carbon aqueous slurry is coated on the surface of the titanium alloy raw material pipe and dried to form a surface layer with a thickness of 45-50 microns, that is, a lubricating layer for hot drawing of the titanium alloy pipe is formed on the surface of the titanium alloy pipe.

[0076] The difference between Comparative Example 3 and Example 1 is that: a method for preparing a lubricating layer for hot drawing of a titanium alloy tube comprises the following steps:

[0077] Step 1, sandblasting the surface of the titanium alloy raw material pipe, first using 100 mesh corundum for sandblasting, then using 325 mesh corundum for sandblasting, and finally using 2000 mesh corundum for sandblasting twice, so that the surface roughness of the titanium alloy pipe after sandblasting is Ra1.0-Ra2.5, the titanium alloy raw material pipe after sandblasting is washed with deionized water, and the obtained titanium alloy raw material pipe is placed at 80°C for drying and standby;

[0078] Step 2: dissolving titanate coupling agent KR138S in deionized water to prepare a 5wt% titanate coupling agent KR138S aqueous solution, placing the titanium alloy raw material pipe in the 5wt% titanate coupling agent KR138S aqueous solution, performing ultrasonic dispersion treatment at a water temperature of 40°C for 5 minutes, an ultrasonic frequency of 40kHz, and a power of 800W. After the ultrasonic dispersion treatment, the obtained titanium alloy raw material pipe is placed at 80°C for drying to form a primer coating on the titanium alloy raw material pipe for standby use;

[0079] Step three, 5g of 800 mesh flake graphite is placed in 50ml of 10wt% potassium permanganate aqueous solution, heated to 60°C and oxidized for 30min under 200rpm magnetic stirring to obtain carboxylated graphite, 50g of carboxylated graphite, 1g of xanthan gum, and 949g of deionized water are prepared into a carbon aqueous slurry, and the obtained carbon aqueous slurry is coated on the primer layer of the titanium alloy raw material pipe and dried to form a surface layer with a thickness of 45-50 microns, that is, a lubricating layer for hot drawing of the titanium alloy pipe is formed on the surface of the titanium alloy pipe.

[0080] The difference between Comparative Example 4 and Example 1 is that: Step 3, the 50wt% high-solid soft resin FS-151650 ordered by Qingdao Ruikos New Material Technology Co., Ltd. is diluted with deionized water to a 0.5wt% solid content aqueous polyurethane emulsion, 5g of unsurface-modified porous molybdenum disulfide sheet is placed in 100g of 0.5wt% solid content aqueous polyurethane emulsion for ultrasonic dispersion treatment for 10min, ultrasonic frequency 40kHz, power 800W, drained, taken out, and placed at 80°C to dry to obtain a finished surface-modified porous molybdenum disulfide sheet; 17g and 70g of the obtained finished surface-modified porous molybdenum disulfide sheet are ... Deionized water, 2g of emulsifier OP, 1g of TX-4 alkylphenol polyoxyethylene ether, 6g of polyurethane acrylate, 1.5g of epoxy modified acrylate, 1g of 1,6-hexanediol diacrylate, 0.5g of tripropylene glycol diacrylate, 0.6g of polyethylene glycol PEG600, and 0.4g of 2-hydroxy-2-methyl-1-phenyl-1-propanone are prepared into a slurry with a solid content controlled at 30wt%. The obtained slurry is evenly coated on a release paper and dried at 60°C to form a semi-cured film with a thickness of 30-35 microns. The obtained semi-cured film is coated on the base coating of the titanium alloy raw material pipe and hot-pressed and dried to form an intermediate layer.

[0081] The difference between Comparative Example 5 and Example 1 is that in step three, 17g of the finished surface modified porous molybdenum disulfide sheet, 60g of deionized water, 2g of emulsifier OP, and 20g of 50wt% high-solid soft resin FS-151650 ordered by Qingdao Ruikos New Material Technology Co., Ltd. are prepared into a slurry with a solid content controlled at 30wt%. The obtained slurry is evenly coated on a release paper and dried at 60°C to form a semi-cured film with a thickness of 30-35 microns. The obtained semi-cured film is coated on the base coating of the titanium alloy raw material pipe and hot-pressed and dried to form an intermediate layer.

[0082] The difference between the control group and Example 1 is that: Step 4, 5g of 800 mesh flake graphite is placed in 50ml of 10wt% potassium permanganate aqueous solution, heated to 60°C and oxidized for 30min under magnetic stirring at 200rpm to obtain carboxylated graphite, 50g of carboxylated graphite, 1g of xanthan gum, and 949g of 50wt% high solid soft resin FS-151650 ordered by Qingdao Ruikos New Material Technology Co., Ltd. are made into carbon slurry, and the obtained carbon aqueous slurry is coated on the middle layer of the titanium alloy raw material pipe and dried to form a surface layer with a thickness of 45-50 microns, that is, a lubricating layer for hot drawing of titanium alloy pipe is formed on the surface of the titanium alloy pipe.

[0083] Performance test: The friction characteristics are tested using a UMT-3 friction tester, the friction form is steel ball-steel disk (the ball is made of titanium alloy / tungsten steel ball, the disk is made of GCr15, and the steel ball diameter is 9.53mm), and the friction test conditions are: rotation radius 5mm, rotation speed 30r / m, test load 50N, temperature: 650℃, test time: 30s. Cleaning effect test method: The titanium alloy pipe with a lubricating layer is placed in a weak alkaline liquid environment with a pH value of 8 at 50 and 70℃ for auxiliary ultrasonic cleaning for 300s, with an ultrasonic frequency of 44kHz and an ultrasonic power of 600W. After the ultrasonic cleaning is completed, it is washed twice with deionized water and dried to observe the adhesion and scratches of the lubricating layer on the surface of the titanium alloy pipe, and the records are summarized and tabulated for analysis.

[0084] Table 1: Test parameters of the composite lubricating layer in Examples 1-10 and Comparative Examples 1-5

[0085]

[0086]

[0087] It can be seen from Examples 1-10 and Comparative Examples 1-5 and Table 1 that the present invention, by selecting a suitable lubricant and coating manufacturing technology, first forms a titanate coupling agent bottom layer on the surface of the titanium alloy tube, the titanate coupling agent bottom layer is a hydrolyzed titanate coupling agent, the intermediate layer and the surface of the titanium alloy tube are firmly connected together, the carbon aqueous slurry is coated on the surface of the intermediate layer at low temperature, the porous molybdenum disulfide sheet and the hydrolyzed latex particles in the intermediate layer are chemically bonded to the surface-modified graphite and / or graphene oxide, the graphite and / or graphene oxide are relatively uniformly fixed to form a composite lubricating layer, and the surface scratches of the product during the hot drawing process are reduced.

[0088] It can be seen from Examples 1-10 and Comparative Examples 1-5 and Table 1 that the hydrolyzable latex particles contained in the slurry prepared in the present application degrade in a weakly alkaline environment at 50-70°C, making the surface cleaning of the product after drawing convenient and efficient, simplifying the subsequent surface cleaning process and saving overall production costs.

[0089] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A lubricating layer for hot drawing of titanium alloy pipes, characterized in that: The lubricating layer for hot drawing of titanium alloy pipes comprises a primer layer, an intermediate layer and a surface layer, wherein the primer layer is a coupling agent treatment layer, and the coupling agent treatment layer is connected to the surface of the titanium alloy pipe by a hydrolysis coupling agent through a chemical bond; the coupling agent used in the coupling agent treatment layer is at least one of a titanate coupling agent, an aminosilane coupling agent and a methacryloxysilane; the intermediate layer comprises porous molybdenum disulfide sheets and hydrolyzable latex particles, and the porous molybdenum disulfide sheets are connected by the hydrolyzable latex particles to form the intermediate layer; The surface of the porous molybdenum disulfide sheet is modified and connected with an interface modifier; the interface modifier is at least one of dopamine, linear polyethylene glycol, polyimide, chitosan, hyaluronic acid, and polylactic acid; the surface layer is made of carbon aqueous slurry; the carbon aqueous slurry includes graphite and / or graphene oxide, and the graphite is at least one of hydroxylated modified graphite, carboxylated graphite, and amino graphite; the graphene oxide is at least one of hydroxylated modified graphene oxide, carboxylated graphene oxide, and amino graphene oxide.

2. The lubricating layer for hot drawing of titanium alloy pipe according to claim 1, characterized in that: The coupling agent used in the coupling agent treatment layer is one of titanate coupling agent KR138S and titanate coupling agent KR38S.

3. The lubricating layer for hot drawing of titanium alloy pipe according to claim 1, characterized in that: The preparation method of the porous molybdenum disulfide sheet is as follows: first prepare nano-scale porous polymolybdate, then use a compound containing a negative divalent sulfur element as a sulfur source aqueous solution combined with a hydrothermal-gas phase in-situ sulfurization method, and use the H2S generated by the thermal decomposition of the sulfur source in a hydrothermal system to react with porous molybdenum acid aggregates to achieve in-situ sulfurization to obtain a porous molybdenum disulfide nanosheet.

4. The lubricating layer for hot drawing of titanium alloy pipe according to claim 1, characterized in that: The carbon aqueous slurry includes graphite and graphene oxide, and the mass ratio of the graphite to the graphene oxide is (6-12):

1.

5. The lubricating layer for hot drawing of titanium alloy pipe according to claim 4, characterized in that: The graphite is amino graphite; the graphene oxide is composed of hydroxylated modified graphene graphite and amino graphene oxide.

6. The method for preparing a lubricating layer for hot drawing of a titanium alloy tube according to claim 5, characterized in that: The graphene oxide is composed of hydroxylated modified graphene oxide and amination modified graphene oxide in a composition mass ratio of (0.5-2):

1.

7. A method for preparing a lubricating layer for hot drawing of a titanium alloy tube according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1, performing sandblasting on the surface of the titanium alloy raw material pipe, and then cleaning and drying it after sandblasting for standby use; Step 2: placing the titanium alloy raw material pipe in a hydrolytic coupling agent liquid for ultrasonic dispersion treatment and drying to form a primer layer; Step 3: The porous molybdenum disulfide sheet treated with hydrolyzed latex particles is mixed with a polymer colloidal emulsion, a suspending agent, and a dispersing agent to form a slurry, the obtained slurry is evenly coated on a release paper and dried to form a semi-cured film, and the obtained semi-cured film is coated on the primer layer of the titanium alloy raw material pipe and hot-pressed and dried to form an intermediate layer; Step 4: coating the carbon aqueous slurry on the middle layer of the titanium alloy raw material pipe and drying it to form a surface layer; the base coating, the middle layer and the surface layer are composited to form a lubricating layer for hot drawing of the finished titanium alloy pipe.

8. The method for preparing a lubricating layer for hot drawing of a titanium alloy tube according to claim 7, characterized in that: The polymer colloidal emulsion in the slurry prepared in step 3 is an aqueous polyurethane emulsion, the diameter of the polyurethane latex particles contained in the aqueous polyurethane emulsion is 100-300nm, and the glass transition temperature Tg≤0°C; the suspending agent is xanthan gum and / or konjac gum; the dispersant is deionized water or a mixed dispersant formed by water and acetone in a volume ratio of (1-4):(0.5-2).

9. The method for preparing a lubricating layer for hot drawing of a titanium alloy tube according to claim 8, characterized in that: In the step 3, the polyurethane latex particles in the prepared slurry have a content of 0.6-1.2wt% and the suspending agent content has a content of 0.05-0.15wt%.

10. The method for preparing a lubricating layer for hot drawing of a titanium alloy tube according to claim 9, characterized in that: The slurry in step 3 includes deionized water, an emulsifier, a surface-modified porous molybdenum disulfide sheet, polyurethane acrylate, epoxy-modified acrylate, 1,6-hexanediol diacrylate, tripropylene glycol diacrylate, polyethylene glycol, and 2-hydroxy-2-methyl-1-phenyl-1-propanone, and the solid content is controlled at 10-35%; In the step 3, the interface modifier is first prepared into a 4-8wt% interface modifier aqueous solution, 1-2 parts of the porous molybdenum disulfide sheet is mixed with 10 parts of the 4-8wt% interface modifier aqueous solution, and ultrasonic dispersion treatment is performed for 5-15 minutes, and the semi-finished surface-modified porous molybdenum disulfide sheet is obtained by draining, taking out, and drying; The aqueous polyurethane emulsion with a solid content of 20-45% is diluted with deionized water to a 0.1-0.5wt% solid content aqueous polyurethane emulsion, 5-10 parts of porous molybdenum disulfide sheets are placed in 80-100 parts of the 0.1-0.5wt% solid content aqueous polyurethane emulsion for ultrasonic dispersion treatment for 5-15 minutes, drained, taken out, and dried to obtain a finished surface-modified porous molybdenum disulfide sheet, and the finished surface-modified porous molybdenum disulfide sheet is placed in the aqueous polyurethane emulsion. , deionized water, emulsifier, polyurethane acrylate, epoxy modified acrylate, 1,6-hexanediol diacrylate, tripropylene glycol diacrylate, polyethylene glycol, and 2-hydroxy-2-methyl-1-phenyl-1-propanone are prepared into a slurry with a solid content controlled at 10-35%, the obtained slurry is evenly coated on release paper and dried to form a semi-cured film with a thickness of 20-60 microns, and the obtained semi-cured film is coated on the base coating of the titanium alloy raw material pipe and hot-pressed and dried to form an intermediate layer.