Photoelectric material based on ultrathin protein nanofilm and preparation method and application thereof
By forming ultra-thin protein nanofilm on inert flexible polymer material and depositing conductive materials on it, the problem of unstable metal coating deposition in the prior art is solved, and efficient and stable photoelectric materials on inert materials are realized Prepared for multifunctional electronic and optical devices.
Patent Information
- Application Number
- CN202411051200.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-01
AI Technical Summary
The prior art is difficult to achieve stable metal coating deposition on inert flexible polymer materials, and existing methods such as the use of dopamine or Plassma modification have high cost or inapplicable problems and are difficult to apply in industrial production.
Using a method based on ultra-thin protein nanomembrane, a film with self-assembly formed an α-helix structure is unfolded and self-assembled by single-molecular proteins, the substrate surface is modified, and conductive material or metal layer is deposited thereon to form a stable photoelectric material.
The formation of stable metal layers on various substrates is achieved, which enhances the stability of the conductive coating, resists bending and stretching, reduces self-assembly defects, improves interface activity and adhesion, and is suitable for multifunctional electronics and Optical devices.
Smart Images

Figure CN118950437A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of biomaterials and optoelectronic materials, and specifically relates to a method for preparing a single-molecule protein ultra-thin nanofilm, and using the single-molecule protein ultra-thin nanofilm as an interlayer material to obtain a stable metal coating on various substrates, which is applied to secret information devices, Raman enhancement devices, smart window devices, printed devices, tactile sensors, etc. Background Art
[0002] By integrating multiple properties, the comprehensive performance of materials can be improved and the multifunctionality of flexible polymer materials can be achieved. For example, combining conductivity, optical properties and mechanical toughness can produce more efficient and flexible electronic and optical devices. At the same time, the development of multifunctional materials reduces the need to use different materials, reduces the waste of resources, and reduces the possibility of waste generation. This kind of comprehensive performance material can also promote the emergence of innovative applications and has a wide range of applications in electronic skin, medical implants, biological intelligence and other fields. It can realize the mutual conversion of information signals such as light and magnetism, and provide potential pillar materials for future information science changes. This material is expected to improve people's quality of life and provide more comfortable, safer and more convenient products and solutions.
[0003] It is crucial to broaden the application areas of flexible polymer materials and realize their versatility. One important method is to "compound" two or more different materials. However, the interfacial adhesion between the two materials requires a strong interaction at their interface, which is often difficult to achieve for inert flexible polymer materials. Therefore, the key to realizing multifunctional and multi-morphological materials is to modify flexible polymer materials using simple and non-toxic methods to form stable interfacial bonding with metal coatings. For example, through chemical methods, substances such as dopamine and tannic acid can be attached to the surface of any material by simple dip coating, or the substrate can be modified by the physical method Plassma to help the metal layer to be stably deposited on the substrate. However, since dopamine is expensive and takes a long time, and tannic acid has color and Plassma modification lasts for a short time, it may not be suitable for use in some scenarios. In industrial production, how to solve these limitations is extremely challenging.
[0004] CN112574578A discloses a protein / polysaccharide composite nanofilm and its application in preventing cracks in conductive coatings. The protein / polysaccharide composite nanofilm is a composite nanofilm with positive charge obtained by crosslinking a nanofilm formed by phase transition protein and polysaccharide at the solid-liquid interface with a crosslinking agent. The composite nanofilm has good stability and optical transmittance. Since the composite nanofilm has positive charge and multiple groups, it can adsorb the conductive coating and reduce the microcracks formed by the conductive coating under bending, maintain the stable conductivity of the flexible device, and when used as a substrate for making OLED devices, it can still maintain the stability of the light-emitting organic layer and the stability of the current density after bending. However, the composite nanofilm needs to add polysaccharides to increase the adhesion of the film, and a crosslinking agent needs to be added at the same time. The secondary structure of the protein in the composite nanofilm is a β-sheet structure, which has poor stability to the metal layer and is easily torn by 3M tape. Summary of the invention
[0005] In order to solve the problems of the prior art, the present invention provides an optoelectronic material based on an ultra-thin protein nanofilm and a preparation method thereof. The ultra-thin protein nanofilm is a protein film with a secondary structure mainly characterized by α-helix as the main component formed by the unfolding and self-assembly of a single-molecule protein. The film has stable adhesion and can play the role of stabilizing the metal layer on various substrates.
[0006] In view of the above purpose, the present invention provides a method for preparing an ultrathin protein nanofilm-based optoelectronic material, comprising the following steps:
[0007] Step 1: After adjusting the pH value of a 1-50 mmol / L reducing agent solution to 4.5-5.5 with NaOH, uniformly mix the solution with a 0.1-2 mg / mL protein solution at a volume ratio of 1:1 to obtain a mixed solution; drip a layer of the mixed solution on the surface of a hydrophobic material and maintain a moist environment, then invert the substrate on the dripped droplets to make the surface of the substrate fully contact with the droplets, react at room temperature for 20-60 minutes, form a layer of colorless transparent single-molecule protein ultrathin nanofilm at the solid-liquid interface between the substrate and the droplets, absorb excess solution on the surface of the substrate with filter paper, and then dry naturally in the air to obtain an ultrathin protein nanofilm-modified substrate with a thickness of 3-15 nm.
[0008] Step 2: Depositing a layer of inorganic conductive material or conductive OLED material on the surface of the ultra-thin protein nanofilm modified substrate by ion sputtering or evaporation to obtain a photoelectric material; or immersing the ultra-thin protein nanofilm modified substrate in a 1-50 mmol / L ammonium tetrachloropalladate aqueous solution, leaving it in the dark for 5-30 minutes, and then immersing it in a metal electroless deposition solution to deposit a metal conductive coating on the surface of the substrate to obtain a photoelectric material; or immersing the ultra-thin protein nanofilm modified substrate in a 0.5-20 mg / mL metal dispersion, leaving it in the dark for 5-30 minutes. The substrate is placed in a shaker and shaken for 30 to 120 minutes to allow the metal conductive coating to be adsorbed on the surface of the substrate to obtain a photoelectric material; or the substrate modified with the ultra-thin protein nanofilm is immersed in an aqueous solution containing 1 to 20 mg / mL ferric chloride and 0.05 to 5 mg / mL conductive polymer monomer, and allowed to stand for 30 to 60 minutes to allow the conductive polymer to be adsorbed on the surface of the substrate to obtain a photoelectric material; or the perovskite precursor solution is spin-coated on the surface of the ultra-thin protein nanofilm modified substrate, and annealing is performed after spin coating to form a photoelectric material with a surface modified perovskite crystal film.
[0009] In the above step 1, the protein is but not limited to: lysozyme, lactalbumin, insulin, β-lactoglobulin, bovine serum albumin, human serum albumin, α-lactalbumin, fibrinogen, β-amyloid protein, transferrin, collagen, pepsin, keratin, myoglobin, hemoglobin, lactoferrin, albumin, albumin, thyrolactoglobulin, prion protein, Aβ peptide, α-synuclein, α-amylase, pepsin, horseradish peroxidase, ribonuclease A, cytochrome c, cystatin C, DNA polymerase, casein, huntingtin protein, immunoglobulin light chain, fibrinogen, keratin, soy protein isolate, pea protein isolate, zein, gliadin, gluten, oat protein, potato protein, hemp seed protein, walnut protein, etc. Any one or more.
[0010] In the above step 1, the reducing agent is but not limited to: cysteine, tris (2-carboxyethyl) phosphine hydrochloride, reduced glutathione, 2-mercaptoethanol, dithiothreitol, dimercaptosuccinic acid, sodium sulfite, β-mercaptoethanol, hydrogen peroxide, ozone, sodium ferrate, trivalent cobalt salt, chlorate, potassium permanganate, persulfate, potassium dichromate, concentrated sulfuric acid, hydrochloric acid, nitric acid, hydrobromic acid, hydroiodic acid, perchloric acid, fluorine gas, chlorine gas, sodium bismuthate, periodic acid, lead dichloride, guanidine hydrochloride, urea, trifluoroethanol, hexafluoroisopropanol, trifluoroacetic acid, malonamide, thiourea, selenourea, tellurium urea, arginine ketoacid, arginine ester, arginine amide, citrulline ketoacid, citrulline ester, citrulline amide, ornithine ketoacid, ornithine ester, ornithine amide, xanthine, hypoxanthine, trioxypurine, theophylline, theobromine, caffeine, etc. Any one or more.
[0011] The reducing agent solution and protein solution are prepared by using 4-hydroxyethylpiperazineethanesulfonic acid buffer solution or ultrapure water as solvent.
[0012] In the above step 1, the hydrophobic material is but not limited to: any one of polytetrafluoroethylene, polyvinylidene fluoride, polyvinyl fluoride, polyethylene, polyacrylonitrile, polyacrylic acid or its derivatives, polypropylene, silicone rubber, nano-coating materials with hydrophobic function, etc.
[0013] In the above step 1, the substrate is a flexible substrate or a non-flexible substrate, the non-flexible substrate is but not limited to any one of silicon, glass, quartz, mica, porcelain, etc., and the flexible substrate is but not limited to any one of polyamide, polyacetal, polymethylpentene, polyvinyl chloride (PVC), polyurethane, polyoxyxylene, polysulfide xylene, polyether ketone, polyaromatic ester, polysulfone, polyetherimide, polystyrene, acrylonitrile-butadiene-styrene copolymer, polyoxyxylene resin, polydimethylsiloxane (PDMS), polymethyl methacrylate, polyethylene, polyethylene terephthalate (PET), polypropylene (BOPP), polycarbonate (PC), photosensitive polyimide (PI), cellulose film, polytetrafluoroethylene film (PTFE), polyvinylidene fluoride film, nylon film, etc.
[0014] In the above step 2, the inorganic conductive material is but not limited to: any one of gold, platinum, silver, copper, indium tin oxide (ITO), zinc oxide (ZnO), titanium dioxide (TiO2) doped with aluminum, titanium nitride (TiN), sodium tungstate (NaWO3), lead iodide (CsPbI3), etc.
[0015] In the above step 2, the conductive OLED material is but not limited to: poly(p-phenylene vinylene) (PPV), poly(9,9-dioctylfluorene) (PFO), poly(3,4-ethylenedioxythiophene) (PEDOT) doped polystyrene sulfonic acid (PSS), polyfluorene (PF) derivative triphenylamine derivative (TPD), tri(8-hydroxyquinoline)aluminum (Alq3), anthracene, polycarbazole (PCz), gallium arsenide (GaAs), gallium nitride (GaN), gallium phosphide (GaP), zinc sulfide (ZnS), indium gallium nitride (InGaN), aluminum gallium nitride (AlGaN), aluminum gallium arsenide (AlGaAs), etc.
[0016] In the above step 2, the metal in the metal electroless deposition solution is but not limited to: any one of copper, silver, nickel, gold, etc. The electroless deposition solution of copper, silver, nickel, gold is the same as the electroless deposition solution disclosed in the prior art.
[0017] In the above step 2, the metal dispersion is but not limited to: a dispersion solution of any one of silver nanowires, ITO powder, MXene, carbon black, carbon nanotubes, graphene, carbon fiber, quantum dots, etc. formed in water or an organic solvent.
[0018] In the above step 2, the conductive polymer is, but not limited to, any one of polyaniline, polypyrrole, polyacetylene, polyphenylene sulfide, polyphenylene, polyphenylene ethylene, polydiyne, polymer liquid crystal, etc.
[0019] In the above step 2, the perovskite precursor is but not limited to: cesium lead bromide (CsPbBr3), cesium tin iodide (CsSnI3), cesium silver bismuth halide (Cs2AgBiBr6), cesium zinc tin halide (Cs2ZnSnI6), diphenylmethane ammonium lead halide ((Ph2CH2NH3)PbX3), fulvethyl ammonium lead halide (C6H5CH2NH3PbX3), etc.
[0020] During the preparation process of the above step 2, when the substrate is a flexible substrate, the substrate modified with the ultra-thin protein nanofilm is further stretched to prepare a photoelectric material.
[0021] The flexible optoelectronic material based on ultrathin protein nanofilm of the present invention can be used to prepare any one of secret information devices, Raman enhancement devices, smart window devices, printed devices, and tactile sensors. The substrate of the optoelectronic material used to prepare the secret information device or smart window device is a flexible substrate, and the substrate of the optoelectronic material used to prepare the Raman enhancement device, printed device, and tactile sensor is a flexible substrate or a non-flexible substrate.
[0022] The beneficial effects of the present invention are as follows:
[0023] 1. The secondary structure of the ultra-thin protein nanofilm of the present invention is mainly α-helix. The unfolded protein forms a new disulfide bond at a specific site through the thiol group. The single molecule undergoes exquisite self-assembly at the solid-liquid interface to form an ultra-thin protein nanofilm. The preparation method is simple, and does not require the addition of polysaccharides, cross-linking agents and other substances. The conditions are mild, efficient, safe, and can be prepared on a large area. It has no selectivity for the shape of the substrate, strong adhesion, excellent optical transparency, and good chemical stability and mechanical stability.
[0024] 2. The thickness of the ultra-thin protein nanofilm of the present invention can be controlled according to the concentration of the protein, the concentration of the reducing agent, the pH value and the reaction time. As the thickness of the film increases, the adhesion weakens.
[0025] 3. The thickness of the ultra-thin protein nanofilm of the present invention is about 3 to 15 nm, and the adhesion is enhanced by balancing the adhesion contribution of the interface and cohesion. The ultra-thin film can effectively reduce the defects in the self-assembly process, reduce the possibility of fracture in the middle of the film, and enhance the interfacial activity.
[0026] 4. The present invention modifies the substrate through an ultra-thin protein nanofilm, which can increase the number of oxygen-containing functional groups on the substrate surface, including thiol groups, to form interactions such as gold-sulfur bonds, van der Waals forces or hydrogen bonds, thereby improving the adhesion properties of the substrate surface. At the same time, due to its ultra-thin characteristics, the adhesion of the ultra-thin film body is weakened, the interface adhesion is enhanced, and the possibility of breaking from the middle is prevented. Based on this ultra-thin protein nanofilm, the adhesion between the substrate surface and the conductive coating is effectively enhanced, the stability of the conductive coating is maintained, and it can withstand the tearing of 3M Tape, immersion in various solvents, and harsh environments such as ultrasound.
[0027] 5. The ultra-thin protein nanofilm prepared by the present invention has strong adhesion. After modifying the surface of the substrate, metal layers of different thicknesses can be deposited on the surface of the modified substrate by magnetron ion sputtering. The metal layers of different thicknesses have different colors, and flexible metal printing of different colors can be achieved. After being bent and folded 1,000 times, it can still resist the tearing of 3M Tape.
[0028] 6. The ultra-thin protein nanofilm prepared by the present invention has strong stability and can enhance the stability of the metal layer on the flexible substrate. When the substrate is in a stretched state, the metal layer is subjected to magnetron ion sputtering, and the resulting photoelectric material can withstand multiple ultrasonic cleanings and be reused. Hidden information can be displayed during stretching, and the effect of enhancing the Raman spectrum signal is still maintained after being bent and stretched 1,000 times, and can be used to prepare secret information devices or Raman enhancement devices.
[0029] 7. After the ultra-thin protein nanofilm prepared by the present invention is attached to the surface of the substrate, the metal layer is magnetron ion sputtered when the substrate is in different stretching states. The metal coating is used to form wrinkles to produce optical diffraction, which can make the resulting photoelectric material change from a transparent state to an opaque state, thereby achieving transparency control. After being stretched 1000 times, the transparency control function is still maintained, and it can be used to prepare smart window devices.
[0030] 8. After the surface of the substrate is modified by the ultra-thin protein nanofilm of the present invention, two types of flexible tactile sensors are designed through the scale structure. This device can be stretched, folded, and twisted. The point tactile sensor can control the rotation of the robot arm, and the multi-layer tactile sensor can identify different materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 These are transparency photos and optical images of the ultrathin protein nanofilm prepared in Example 1.
[0032] Figure 2 This is a thickness diagram of the ultrathin protein nanofilm prepared in Example 1.
[0033] Figure 3 It is the secondary structure diagram of the ultrathin protein nanomembrane prepared in Example 1.
[0034] Figure 4 These are microscope optical images of the gold layer deposited by ion sputtering on the surface of the ultra-thin protein nanofilm modified PDMS in Example 1, after being soaked in various solvents, resisting tearing with 3M tape.
[0035] Figure 5 These are optical pictures of the gold layer deposited by ion sputtering on the surface of PDMS modified with protein nanofilms of different thicknesses obtained by standing at room temperature for different reaction times in Example 1, resisting tearing with 3M tape after a 180-degree peeling test using a tensile machine.
[0036] Figure 6 This is an optical picture of secret information transmission of optoelectronic materials in Example 2.
[0037] Figure 7 These are optical photographs and SEM images of the optoelectronic material of Example 3 before and after the 3M tape is torn off.
[0038] Figure 8 The effect of bending on the usability of the photovoltaic material of Example 3.
[0039] Fig. 9 The effect of stretching on the usability of the optoelectronic material of Example 3.
[0040] Fig.10 is an optical picture of the photovoltaic material of Example 4 (transparent to opaque).
[0041] Fig.11 is an optical picture of the photovoltaic material of Example 5 (opaque to transparent).
[0042] Fig.12 This is an optical picture of the optoelectronic material of Example 6.
[0043] Fig.13 This is a capacitance response diagram of the optoelectronic material of Example 7 before and after the 3M tape is torn.
[0044] Fig.14 This is an optical image of the control robot arm of the optoelectronic material of Example 7.
[0045] Fig.15 This is an optical picture of the optoelectronic material of Example 7.
[0046] Fig.16 This is a diagram of the secondary structure of ultra-thin protein nanomembranes prepared from different proteins. DETAILED DESCRIPTION
[0047] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments, but the protection scope of the present invention is not limited to these embodiments.
[0048] Example 1
[0049] Step 1: Add 0.7165g tris(2-carboxyethyl)phosphonate to 50mL ultrapure water to prepare a 50mmol / L tris(2-carboxyethyl)phosphonate aqueous solution, and adjust its pH value to 5 with a 5mol / LNaOH aqueous solution; add 100mg bovine serum albumin to 50mL ultrapure water to prepare a 2mg / mL bovine serum albumin aqueous solution; then evenly mix the two solutions at a volume ratio of 1:1 to obtain a mixed solution; drip a layer of the mixed solution on the surface of the polypropylene film, and maintain a moist environment, then invert the PDMS substrate on the droplets dripped on the surface of the polypropylene film to allow the surface of the PDMS substrate to fully contact the droplets, and let it stand at room temperature for 40 minutes to form a layer of colorless, transparent, single-molecule protein ultrathin nanofilm at the solid-liquid interface between the PDMS substrate and the droplets. Use filter paper to absorb excess solution on the surface of the PDMS substrate, and then dry it naturally in the air to obtain an ultrathin protein nanofilm modified PDMS. Figure 1 It can be seen that the film formed on the PDMS surface is colorless and transparent, and its transmittance in the visible light band is close to 100%; Figure 2 It can be seen that the thickness of the film is 5.5 nm, which is very thin and close to a monomolecular layer, and can effectively reduce the probability of the bioadhesive layer breaking in the middle. Figure 3 It can be seen that the protein secondary structure of the obtained ultrathin protein nanomembrane is α-helix, while the secondary structure of the protein in the traditional protein nanomembrane is β-sheet (preparation method see DOI:10.1002 / adma.202000128, the membrane thickness is about 50nm).
[0050] Step 2: Place the PDMS modified with the ultrathin protein nanofilm in step 1 in a magnetron ion sputtering instrument, and perform magnetron ion sputtering for 90 seconds to deposit a layer of Au on the surface of the ultrathin protein nanofilm in an unstretched state to obtain a composite photoelectric material of the Au layer, the ultrathin protein nanofilm and the PDMS.
[0051] The photoelectric materials obtained above were immersed in deionized water, pH = 1 HCl aqueous solution, pH = 11 NaOH aqueous solution, DMSO, ethanol, pepsin, trypsin, 1 mmol / L vitamin C aqueous solution, and 1% sodium dodecyl sulfate (SDS) aqueous solution for 1 hour, and then tested by atomic force microscopy (see Figure 4). Then, the room temperature reaction time in step 1 was extended to 1.5 hours and 6 hours to prepare two different thicknesses of protein nanofilm-modified PDMS and deposit the Au layer, and the optical images were taken with a camera using the hundred-grid knife test method (see Figure 5 ).Depend on Figure 4 and Figure 5 It can be seen that the Au layer on the optoelectronic material modified by the ultra-thin protein nanofilm (mainly α-helixt structure) can resist the tearing of 3M tape and the immersion in various solvents, while the thick protein nanofilm (mainly β-sheet structure) prepared by prolonging the reaction time cannot achieve this effect.
[0052] Example 2
[0053] Step 1 of this embodiment is the same as step 1 of embodiment 1, and an ultrathin protein nanofilm-modified PDMS is prepared. In step 2 of this embodiment, the ultrathin protein nanofilm-modified PDMS in step 1 is placed in a magnetron ion sputtering instrument, a five-pointed star template is placed on the unstretched PDMS, and magnetron ion sputtering is performed for 5 seconds to deposit a five-pointed star-shaped Au layer on the surface of the ultrathin protein nanofilm, thereby obtaining a photoelectric material composited with a five-pointed star-shaped Au layer, an ultrathin protein nanofilm, and PDMS.
[0054] Depend on Figure 6 It can be seen that in the unstretched state, the five-pointed star information is hidden because the PDMS and Au coatings have similar light reflectivity. However, after stretching, the hidden five-pointed star pattern appears. This is because the cracks are formed perpendicular to the stretching direction, and the Poisson effect enhances light scattering, which can show the hidden five-pointed star information, indicating that it has the function of hiding information. And the five-pointed star Au layer is sputtered on the surface of the PDMS modified by the ultra-thin protein nanofilm, which can resist multiple 3M tape tearing. Therefore, the optoelectronic material of this embodiment can be used to prepare a secret information device.
[0055] Example 3
[0056] Step 1 of this embodiment is the same as step 1 of embodiment 1, and an ultrathin protein nanofilm-modified PDMS is prepared. In step 2 of this embodiment, the ultrathin protein nanofilm-modified PDMS in step 1 is pre-stretched by 50% and then placed in a magnetron ion sputtering instrument, and magnetron ion sputtering is performed for 90 seconds to deposit a layer of Au on the surface of the ultrathin protein nanofilm, thereby obtaining an Au layer, an ultrathin protein nanofilm, and a PDMS composite photoelectric material.
[0057] After the Au layer deposited by magnetron sputtering on the surface of PDMS modified by ultrathin protein nanofilm and the Au layer deposited by magnetron ion sputtering directly on the surface of PDMS were ultrasonicated in deionized water with a power of 150W, the Au layer deposited by magnetron sputtering on the surface of PDMS modified by ultrathin protein nanofilm was more stable and the Au layer was basically intact, as shown in Figure 2. Figure 7 .
[0058] Rhodamine B is a strong fluorescent dye with a significant Raman scattering cross section. When Rhodamine B molecules are adsorbed on a metal surface with a nanostructure (such as gold or silver nanoparticles), its Raman signal will be significantly enhanced, which is the SERS effect. Due to its strong Raman signal, Rhodamine B is often used as a standard probe molecule in SERS research to calibrate and evaluate SERS. Rhodamine B was used to perform SERS testing on the optoelectronic material obtained in this embodiment. The Raman spectrum showed that the Au layer deposited by magnetron sputtering on the PDMS surface modified with ultra-thin protein nanofilm has the effect of enhancing the Raman spectrum and can be reused many times. Figure 8 and Fig. 9 It shows that after being stretched or bent 1000 times by ultrasound, the Raman characteristic spectrum of Rhodamine B still exists stably, which proves that the photoelectric material prepared in this embodiment can be used to prepare Raman enhancement devices and can be reused many times.
[0059] Example 4
[0060] Step 1 of this embodiment is the same as step 1 of embodiment 1, and an ultrathin protein nanofilm-modified PDMS is prepared. In step 2 of this embodiment, the ultrathin protein nanofilm-modified PDMS in step 1 is placed in a magnetron ion sputtering instrument, and magnetron ion sputtering is performed for 90 seconds in an unstretched state to deposit a layer of Au on the surface of the ultrathin protein nanofilm, thereby obtaining an Au layer, an ultrathin protein nanofilm, and a PDMS composite photoelectric material. At the same time, a comparative experiment was performed using an Au layer directly deposited by magnetron ion sputtering on the PDMS surface. The results show that the photoelectric material obtained without stretching exhibits an opaque property, and the photoelectric material obtained after stretching exhibits a transparent property. Fig.10 The optical photographs show that the optoelectronic material of this embodiment still has the ability to reversibly change the optical properties after being torn, and can resist multiple tearing of the 3M tape. Therefore, the optoelectronic material prepared in this embodiment can be used to prepare smart window devices.
[0061] Example 5
[0062] Step 1 of this embodiment is the same as step 1 of embodiment 1, and an ultra-thin protein nanofilm-modified PDMS is prepared. In step 2 of this embodiment, the ultra-thin protein nanofilm-modified PDMS in step 1 is pre-stretched by 50%, and then placed in a magnetron ion sputtering instrument, and magnetron ion sputtering is performed for 90 seconds to deposit an Au layer on the surface of the ultra-thin protein nanofilm, thereby obtaining an Au layer, an ultra-thin protein nanofilm, and a PDMS composite photoelectric material. The results show that the photoelectric material obtained by pre-stretching PDMS by 50% and then magnetron ion sputtering the Au layer shows an opaque property, but the photoelectric material shows transparency after stretching. Fig.11The optical photographs show that the optoelectronic material of this embodiment still has the ability to reversibly change the optical properties after being torn, and can resist multiple tearing of the 3M tape. Therefore, the optoelectronic material prepared in this embodiment can be used to prepare smart window devices.
[0063] Example 6
[0064] Step 1 of this embodiment is the same as step 1 of embodiment 1, and an ultra-thin protein nanofilm-modified PDMS is prepared. In step 2 of this embodiment, the ultra-thin protein nanofilm-modified PDMS not pre-stretched in step 1 is placed in a magnetron ion sputtering instrument, and the ultra-thin protein nanofilm-modified PDMS is covered with a five-pointed star template, and magnetron ion sputtering is performed for different times to obtain Au layers of different thicknesses. Fig.12 As can be seen from the optical pictures, the obtained optoelectronic material reflects light in different colors and has the ability of flexible metal printing. Therefore, the optoelectronic material prepared in this embodiment can be used to prepare printed devices.
[0065] Example 7
[0066] Step 1 of this embodiment is the same as step 1 of embodiment 1, and an ultra-thin protein nanofilm-modified PDMS is prepared. In step 2 of this embodiment, the ultra-thin protein nanofilm-modified PDMS in step 1 is pre-stretched by 50% and then placed in a magnetron ion sputtering instrument, the template covers the ultra-thin protein nanofilm-modified PDMS, and magnetron ion sputtering is performed for 90 seconds to deposit a patterned Au layer on the surface of the ultra-thin protein nanofilm, thereby obtaining a patterned Au layer, an ultra-thin protein nanofilm, and a PDMS composite photoelectric material. Fig.13 The capacitance response graph shows that compared with the Au layer deposited directly on the PDMS surface by magnetron ion sputtering, the PDMS modified with ultrathin protein nanofilm has better stability to the Au layer and still maintains sensitive responsiveness when tested before and after the 3M tape is torn off. Fig.14 As can be seen from the optical picture, the optoelectronic material of this embodiment can be integrated into the robot to control the robot arm. Fig.15 It can be seen that the optoelectronic material of this embodiment is stretchable, bendable, foldable and has good skin-friendliness. Therefore, the optoelectronic material prepared in this embodiment can be used to prepare a tactile sensor.
[0067] In step 1 of the above embodiment, the 2 mg / mL bovine serum albumin aqueous solution in Example 1 is replaced with an equal volume of 2 mg / mL lysozyme aqueous solution or 2 mg / mL insulin aqueous solution or 2 mg / mL human serum albumin aqueous solution, and the room temperature reaction is shortened to 10 minutes. The other steps of this step are the same as those in Example 1 to obtain an ultrathin protein nanofilm. Fig.16 It can be seen that lysozyme ( Fig.16 a) Insulin ( Fig.16 b) Human serum albumin ( Fig.16 c) The secondary structure of the proteins in the prepared ultrathin protein nanofilms is α-helix.
Claims
1. A method for preparing an optoelectronic material based on an ultrathin protein nanofilm, characterized in that: The method comprises the following steps: Step 1: After adjusting the pH value of a 1-50 mmol / L reducing agent solution to 4.5-5.5 with NaOH, uniformly mix the solution with a 0.1-2 mg / mL protein solution at a volume ratio of 1:1 to obtain a mixed solution; dripping a layer of the mixed solution on the surface of a hydrophobic material and maintaining a wet environment, then inverting a substrate on the dripped droplets to allow the surface of the substrate to fully contact the droplets, reacting at room temperature for 20-60 minutes, forming a layer of colorless, transparent, single-molecule protein ultrathin nanofilm at the solid-liquid interface between the substrate and the droplets, absorbing excess solution on the surface of the substrate with filter paper, and then drying naturally in the air to obtain an ultrathin protein nanofilm-modified substrate with a thickness of 3-15 nm; Step 2: Depositing a layer of inorganic conductive material or conductive OLED material on the surface of the substrate modified with the ultra-thin protein nanofilm by ion sputtering or evaporation to obtain a photoelectric material; Alternatively, the substrate modified with the ultra-thin protein nanofilm is immersed in a 1-50 mmol / L aqueous solution of ammonium tetrachloropalladate, placed in the dark for 5-30 minutes, and then immersed in a metal electroless deposition solution to deposit a metal conductive coating on the surface of the substrate to obtain a photoelectric material; Alternatively, the substrate modified with the ultra-thin protein nanofilm is immersed in a 0.5-20 mg / mL metal dispersion and shaken in a shaker for 30-120 minutes to allow the metal conductive coating to be adsorbed on the surface of the substrate to obtain a photoelectric material; Alternatively, the substrate modified with the ultra-thin protein nanofilm is immersed in an aqueous solution containing 1-20 mg / mL ferric chloride and 0.05-5 mg / mL conductive polymer monomer, and allowed to stand for 30-60 minutes to allow the conductive polymer to be adsorbed on the surface of the substrate to obtain a photoelectric material. Alternatively, the perovskite precursor solution is spin-coated on the surface of the substrate modified with the ultra-thin protein nanofilm, and then annealed to form a photoelectric material with a surface modified perovskite crystal film.
2. The method for preparing an ultrathin protein nanofilm-based optoelectronic material according to claim 1, characterized in that: In step 1, the protein is selected from any one or more of lysozyme, lactalbumin, insulin, β-lactoglobulin, bovine serum albumin, human serum albumin, α-lactalbumin, fibrinogen, β-amyloid protein, transferrin, collagen, pepsin, keratin, myoglobin, hemoglobin, lactoferrin, albumin, albumin, thyrolactoglobulin, prion protein, Aβ peptide, α-synuclein, α-amylase, pepsin, horseradish peroxidase, ribonuclease A, cytochrome c, cystatin C, DNA polymerase, casein, huntingtin, immunoglobulin light chain, fibrinogen, keratin, soy protein isolate, pea protein isolate, zein, gliadin, gluten, oat protein, potato protein, hemp seed protein, and walnut protein.
3. The method for preparing an ultrathin protein nanofilm-based optoelectronic material according to claim 1, characterized in that: In step 1, the reducing agent is selected from cysteine, tris(2-carboxyethyl)phosphine hydrochloride, reduced glutathione, 2-mercaptoethanol, dithiothreitol, dimercaptosuccinic acid, sodium sulfite, β-mercaptoethanol, hydrogen peroxide, ozone, sodium ferrate, trivalent cobalt salt, chlorate, potassium permanganate, persulfate, potassium dichromate, concentrated sulfuric acid, hydrochloric acid, nitric acid, hydrobromic acid, hydroiodic acid, perchloric acid, fluorine gas, chlorine gas, sodium bismuthate, periodic acid, lead dichloride, guanidine hydrochloride, urea, trifluoroethanol, hexafluoroisopropanol, trifluoroacetic acid, malonamide, thiourea, selenourea, tellurium urea, arginine ketoacid, arginine ester, arginine amide, citrulline ketoacid, citrulline ester, citrulline amide, ornithine ketoacid, ornithine ester, ornithine amide, xanthine, hypoxanthine, trioxypurine, theophylline, theobromine, caffeine and any one or more thereof.
4. The method for preparing an optoelectronic material based on an ultrathin protein nanofilm according to claim 1, characterized in that: In step 1, the hydrophobic material is selected from any one of polytetrafluoroethylene, polyvinylidene fluoride, polyvinyl fluoride, polyethylene, polyacrylonitrile, polyacrylic acid or its derivatives, polypropylene, silicone rubber, and nano-coating materials containing hydrophobic function.
5. The method for preparing an ultrathin protein nanofilm-based optoelectronic material according to claim 1, characterized in that: In step 1, the substrate is a flexible substrate or a non-flexible substrate, the non-flexible substrate is selected from any one of silicon, glass, quartz, mica, and porcelain, and the flexible substrate is selected from any one of polyamide, polyacetal, polymethylpentene, polyvinyl chloride, polyurethane, polyoxyxylene, polysulfide xylene, polyether ketone, polyaromatic ester, polysulfone, polyetherimide, polystyrene, acrylonitrile-butadiene-styrene copolymer, polyoxyxylene resin, polydimethylsiloxane, polymethyl methacrylate, polyethylene, polyethylene terephthalate, polypropylene, polycarbonate, photosensitive polyimide, cellulose film, polytetrafluoroethylene film, polyvinylidene fluoride film, and nylon film.
6. The method for preparing an optoelectronic material based on an ultrathin protein nanofilm according to claim 5, characterized in that: In step 2, when the substrate is a flexible substrate, the substrate modified with the ultra-thin protein nanofilm is stretched to prepare the optoelectronic material.
7. The method for preparing an ultrathin protein nanofilm-based optoelectronic material according to claim 1, characterized in that: In step 2, the inorganic conductive material is selected from any one of gold, platinum, silver, copper, indium tin oxide, zinc oxide, titanium dioxide doped with aluminum, titanium nitride, sodium tungstate, and lead iodide.
8. The method for preparing an ultrathin protein nanofilm-based optoelectronic material according to claim 1, characterized in that: In step 2, the conductive OLED material is selected from any one of poly(p-phenylene vinylene), poly(9,9-dioctylfluorene), poly(3,4-ethylenedioxythiophene) doped polystyrene sulfonic acid, polyfluorene derivatives, triphenylamine derivatives, tri(8-hydroxyquinoline)aluminum, anthracene, polycarbazole, gallium arsenide, gallium nitride, gallium phosphide, zinc sulfide, indium gallium nitride, aluminum gallium nitride, and aluminum gallium arsenide.
9. The method for preparing an ultrathin protein nanofilm-based optoelectronic material according to claim 1, characterized in that: In step 2, the metal in the metal electroless deposition solution is any one of copper, silver, nickel and gold.
10. The method for preparing optoelectronic materials based on ultrathin protein nanofilms according to claim 1, characterized in that: In step 2, the metal dispersion is a dispersed solution of any one of silver nanowires, ITO powder, MXene, carbon black, carbon nanotubes, graphene, carbon fiber, and quantum dots in water or an organic solvent.
11. The method for preparing an ultrathin protein nanofilm-based optoelectronic material according to claim 1, characterized in that: In step 2, the conductive polymer is selected from any one of polyaniline, polypyrrole, polyacetylene, polyphenylene sulfide, polyphenylene, polyphenylene ethylene, polydiacetylene, and polymer liquid crystal.
12. The method for preparing an ultrathin protein nanofilm-based optoelectronic material according to claim 1, characterized in that: In step 2, the perovskite precursor is selected from any one of cesium lead bromide, cesium tin iodide, cesium silver bismuth halide, cesium zinc tin halide, diphenylmethane ammonium lead halide, and fulvenemethylammonium lead halide.
13. Photoelectric material based on ultrathin protein nanofilm prepared by any one of the preparation methods of claims 1 to 12.
14. Use of the optoelectronic material based on ultrathin protein nanofilm according to claim 13 in the preparation of any one of secret information devices, Raman enhanced devices, smart window devices, printed devices, and tactile sensors, wherein the substrate of the optoelectronic material used to prepare the secret information device or smart window device is a flexible substrate, and the substrate of the optoelectronic material used to prepare the Raman enhanced device, printed device, and tactile sensor is a flexible substrate or a non-flexible substrate.
Citation Information
Patent Citations
Biological protein two-dimensional nano-film prepared by using lysozyme and preparation method of biological protein two-dimensional nano-film
CN105153443A
Method for performing metal electroless deposition based on lysozyme two-dimension nano-film
CN105296977A
Preparation method of self-supporting two-dimensional metal film welded through protein
CN108505023A
Modified water-based material as well as preparation method and application thereof
CN114712332A
Redox protein immobilization nanostructure electrode
JP2011069727A