Method for preparing aluminum oxide reinforced aluminum-based composite material through auto-oxidation accumulative roll bonding

Through self-oxidation accumulation stacking technology, the problem of difficulty in dispersing alumina particles in aluminium-based composite materials is solved, and the material performance is improved and process simplified is achieved, which is suitable for large-scale production.

CN118950702AActive Publication Date: 2024-11-15HAI AN & TAIYUAN UNIV OF TECH ADVANCED MFG & INTELLIGENT EQUIP IND RES INST
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411227060.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-15
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

In the existing preparation methods for alumina reinforced aluminum-based composite materials, it is difficult to achieve uniform dispersion of alumina particles, resulting in complex processes, high costs and limited performance.

Method used

By adopting self-oxidation accumulation stacking technology, the alumina layer is uniformly distributed in the aluminum-based composite material by controlling the heating temperature, heating time and rolling process, the alumina layer is uniformly distributed by cross-corrugated rolling, avoiding agglomeration of alumina particles and uneven interfaces. sex.

Benefits of technology

The uniform distribution of alumina particles in aluminum-based composite materials is achieved, which reduces production costs, improves the comprehensive performance of the material, such as toughness, strength and wear resistance, and simplifies the process flow, which is suitable for large-scale continuous production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950702A_ABST
    Figure CN118950702A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing an aluminum oxide reinforced aluminum-based composite material through auto-oxidation accumulative roll bonding, and belongs to the technical field of aluminum-based composite material preparation. The method for preparing the aluminum oxide reinforced aluminum-based composite material through auto-oxidation accumulative roll bonding comprises the following steps that an aluminum plate is taken and heated in an oxygen-containing atmosphere to form an aluminum oxide layer, and an oxidation layer aluminum plate 1 is obtained; taking the two oxide layer aluminum plates 1, stacking the two oxide layer aluminum plates 1 together to form a group blank, and rolling the group blank by using a two-roller mill of which the upper roller and the lower roller are crossed corrugated rollers to obtain a composite plate 1; and cutting off the composite plate 1 along the transverse direction in a centering manner, heating in an oxygen-containing atmosphere to form an aluminum oxide layer, carrying out accumulative ply rolling, rolling by using a two-roller rolling mill of which the upper roller and the lower roller are flat rollers to obtain a metal composite plate, and annealing to obtain the aluminum oxide reinforced aluminum-based composite plate. And after multi-pass rolling, the aluminum oxide strengthening phase is uniformly distributed in the aluminum-based composite material, so that the comprehensive performance of the aluminum-based composite material is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum-based composite material preparation, and in particular to a method for preparing aluminum oxide-reinforced aluminum-based composite material through self-oxidation cumulative rolling. Background Art

[0002] Aluminum-based composite materials are a new type of material with strong vitality that was born with the needs of modern scientific development. It has the advantages of light weight, good toughness, small thermal expansion coefficient, high strength, strong wear resistance, etc. It is a structural material with excellent comprehensive performance and is widely used in aerospace, transportation, electrical and electronic fields.

[0003] Aluminum-based composite materials are mainly made of aluminum or aluminum alloy as the matrix, SiC, Al2O3, graphite and other particles as reinforcements, and are prepared through a composite process. Compared with other reinforcements, alumina particles have better interface bonding properties with the aluminum matrix. Alumina-reinforced aluminum-based composite materials not only have properties such as high temperature resistance and wear resistance, but also have higher specific stiffness and specific strength, and have high research value.

[0004] At present, there are many methods for preparing aluminum-based composite materials reinforced by alumina. According to the state of the matrix material and the reinforcement phase when they are combined, the preparation methods of aluminum-based composite materials reinforced by alumina can be divided into liquid casting, spray deposition, powder metallurgy, etc. Among them, the liquid casting method is a method in which nano-alumina particles and aluminum molten metal are mixed evenly by stirring or other means, and then cast and solidify; this method has a flexible preparation process, high production efficiency and low cost, but its process control is difficult, and agglomeration is very likely to occur during the addition of reinforcements, resulting in reinforcement segregation, uneven mixing, coarse organization and other problems; at the same time, the liquid casting method is also prone to defects such as pores and cracks in the process of preparing aluminum-based composite materials, which affects the performance of the composite material. The spray deposition method is a method in which aluminum molten metal is atomized by high-speed spraying, mixed with nano-alumina particles, and then sprayed onto a preheated substrate for rapid solidification; but due to the limitations of material density and production cost, this method is mostly used to prepare thin film materials with a thickness below the millimeter level. Powder metallurgy is a method of preparing aluminum-based composite materials by mixing aluminum powder and alumina for pre-pressing, and then sintering, rolling, annealing and other processes. This method is currently the most commonly used method for preparing aluminum-based composite materials because it has the advantages of relatively uniform distribution of the reinforcement phase and controllable volume fraction. However, its preparation process is complex, the material is easily contaminated, and the production cycle is long, which will limit the performance and application of the prepared aluminum-based composite materials. In summary, the difficulty in preparing aluminum-based composite materials reinforced with alumina particles is to achieve uniform dispersion of the reinforcement phase. Therefore, further research is urgently needed to achieve efficient preparation of aluminum-based composite materials with controllable distribution of alumina particles. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing alumina-reinforced aluminum-based composite materials by self-oxidation cumulative rolling, so as to solve the above-mentioned problems in the background technology. The present invention adopts aluminum plate self-oxidation technology, takes aluminum plate as raw material, and realizes the preparation of alumina reinforcing phase by controlling heating temperature, heating time and rolling process. Alumina is not required as the initial material, which reduces production costs and improves product performance. The preparation process of the present invention is simple, the required equipment requirements are low, and large-scale and continuous production can be achieved. After multiple rolling passes, the alumina reinforcing phase is evenly distributed in the aluminum-based composite material, ensuring the comprehensive performance of the aluminum-based composite material.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] One of the technical solutions of the present invention is to provide a method for preparing alumina reinforced aluminum-based composite materials by self-oxidation rolling, comprising the following steps:

[0008] (1) taking an aluminum plate, removing oil stains and oxide film on the surface and grinding it to make it rough, and heating it in an oxygen-containing atmosphere to form an aluminum oxide layer with a thickness of 0.1 to 1 μm on the surface of the aluminum plate, thereby obtaining an oxide layer aluminum plate 1;

[0009] Take two pieces of the oxide layer aluminum plates 1, stack them together to form an embryonic assembly, and roll them using a two-roller mill with both upper and lower rolls being cross-corrugated rolls, and then straighten and trim them to obtain a composite plate 1;

[0010] (2) cutting the composite plate 1 in the middle in the transverse direction to obtain two composite plate 1 sub-plates of the same size; removing the oil stains and oxide film on the surface of the composite plate 1 sub-plate and grinding it to be rough, and then heating it in an oxygen-containing atmosphere to form an aluminum oxide layer with a thickness of 0.1 to 1 μm on the surface of the aluminum plate, thereby obtaining an oxide layer aluminum plate 2;

[0011] The two oxide-layer aluminum plates 2 are stacked together to form an embryonic assembly, and rolled using a two-roller rolling mill in which both the upper and lower rollers are cross-corrugated rollers, and straightened, trimmed, and head and tail cut to prepare a composite plate 2;

[0012] (3) Repeat step (2) n times to obtain composite plate n+2;

[0013] (4) cutting the composite plate n+2 in the middle in the transverse direction to obtain two composite plate n+2 sub-plates of the same size; removing the oil stains and oxide film on the surface of the composite plate n+2 sub-plate and grinding it to be rough, and then heating it in an oxygen-containing atmosphere to form an aluminum oxide layer with a thickness of 0.1 to 1 μm on the surface of the aluminum plate, thereby obtaining an oxide layer aluminum plate n+3;

[0014] The two pieces of the oxide layer aluminum plates n+3 are stacked together to form an embryonic embryo, and rolled using a two-roll rolling mill with both upper and lower rolls being flat rolls, and straightened, trimmed, and head and tail cut to prepare a metal composite plate;

[0015] (5) Annealing, straightening and trimming the metal composite plate to obtain the alumina reinforced aluminum-based composite plate.

[0016] Preferably, n is an integer ≥1.

[0017] Preferably, the aluminum plate is made of industrial pure aluminum, 3-series aluminum alloy, 4-series aluminum alloy, 6-series aluminum alloy or 7-series aluminum alloy; and the thickness of the aluminum plate is 2 to 10 mm.

[0018] Preferably, in steps (1), (2) and (3), the heating temperature is 70% to 90% of the melting point of the aluminum plate.

[0019] Preferably, in steps (1) and (2), the surface of the cross-corrugated roller is a curved surface formed by the intersection of transverse corrugations and longitudinal corrugations, and the corrugation curve is a sine curve, a cosine curve or a parabola; the wavelength of the corrugation curve is ≤8 mm, and the amplitude is ≤1 mm.

[0020] Preferably, in steps (1), (2) and (3), the rolling reduction ratio is 50% to 70%.

[0021] The second technical solution of the present invention is to provide an alumina reinforced aluminum-based composite material prepared by the above method.

[0022] The beneficial technical effects of the present invention are as follows:

[0023] The present invention adopts cumulative rolling technology, using upper and lower crossed corrugated rollers to make the slab deform unevenly in the thickness direction, so that the interface to be composited is subjected to uneven force, which promotes the tearing of the interface to be composited and the crushing of the oxide layer, and then promotes the dispersed redistribution of the crushed alumina particles around the interface, forming an enhancement of alumina particles in the area around the interface; at the same time, the fresh metal exposure of the interface is more conducive to the realization of effective interface bonding. Furthermore, multiple cross-corrugated roller rolling can make the alumina particles more evenly distributed in the thickness direction of the aluminum plate.

[0024] The present invention uses the cross-corrugated texture of the roller to control the generation and distribution of alumina. In the process of forming the alumina layer by high-temperature heating, the cross-corrugated concave-convex texture on the surface of the composite plate not only increases the surface area of ​​the oxidation reaction, but also effectively promotes the uniform distribution and growth of alumina by guiding the growth direction of alumina crystals. In addition, by adjusting the rolling reduction rate and the number of rolling passes, the alumina content in the alumina-reinforced aluminum-based composite material can be estimated and controlled.

[0025] The present invention adopts aluminum plate self-oxidation technology, uses aluminum plate as raw material, and realizes the preparation of aluminum oxide reinforcement phase by controlling heating temperature, heating time and rolling process. Aluminum oxide is not required as the initial material, and there is no excessive material loss in the whole process. The utilization rate of raw materials is relatively high, which reduces production costs and improves product performance. At the same time, compared with other aluminum-based composite material preparation technologies such as traditional powder metallurgy and liquid casting, the present invention avoids a series of complicated steps such as mixing powder, molding, sintering, etc., making the overall preparation process simpler. In addition, the cumulative rolling process can be realized by relying on relatively simple traditional rolling equipment. These equipments are more economical in cost and maintenance, and can realize large-scale and continuous production. After multiple rolling passes, the aluminum oxide reinforcement phase is evenly distributed in the aluminum-based composite material, ensuring the comprehensive properties of the aluminum-based composite material such as toughness, strength, corrosion resistance and wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 This is a schematic process diagram of the method for preparing alumina-reinforced aluminum-based composite materials by self-oxidation cumulative rolling according to Examples 1-3 of the present invention.

[0028] Figure 1 Among them, aluminum plate A—(1), aluminum plate B—(2), grinding device—(3), heating furnace—(4), upper cross corrugated roller—(5), lower cross corrugated roller—(6), upper flat roller—(7), lower flat roller—(8), corrugated surface metal composite plate (A / B) 1—(9), metal composite plate (A / B) 11—(10), metal composite plate (A / B) 21—(11), corrugated surface metal composite plate (A / B) n-2 —(12), Metal composite plate (A / B) 1n-2—(13), Metal composite plate (A / B) 2n-2—(14), Corrugated metal composite plate (A / B) n-1 —(15), Metal composite plate (A / B) 1n-1—(16), Metal composite plate (A / B) 2n-1—(17), Metal composite plate (A / B) n —(18). DETAILED DESCRIPTION

[0029] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.

[0030] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0031] Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention pertains. Although only preferred methods and materials are described herein, any methods and materials similar or equivalent to those described herein may also be used in the practice or testing of the present invention.

[0032] The words “include,” “including,” “have,” “contain,” etc. used in the present invention are open-ended terms, meaning including but not limited to.

[0033] The melting point of the industrial pure aluminum used in the following embodiments of the present invention is 660°C, the melting point of the 6061 aluminum alloy is 610°C, and the melting point of the 7075 aluminum alloy is 525°C.

[0034] All raw materials used in the following embodiments of the present invention are commercially available products.

[0035] Example 1

[0036] A method for preparing alumina-reinforced aluminum-based composite materials by auto-oxidation cumulative rolling, comprising the following steps:

[0037] S1, plate preparation: prepare a 1060 aluminum plate A(1) with a length×width×height of 250 mm×100 mm×2 mm and made of industrial pure aluminum, prepare a 1060 aluminum plate B(2) with a length×width×height of 250 mm×100 mm×2 mm and made of industrial pure aluminum, remove the oil stains and oxide film on the surfaces of the aluminum plates A(1) and B(2), then grind the surfaces to be composited of the aluminum plates A(1) and B(2) to make them rough and set aside;

[0038] S2, surface self-oxidation heating: the aluminum plate A (1) and the aluminum plate B (2) obtained in step S1 are heated to 550° C. in a heating furnace (4) without anti-oxidation measures, so that a 0.1 μm thick aluminum oxide layer is formed on the surface of the aluminum plate A (1) and the aluminum plate B (2);

[0039] S3, preparing a corrugated metal composite plate (A / B) 1: stacking the aluminum plates heated in step S2 in a manner such that the aluminum plate A (1) is at the bottom and the aluminum plate B (2) is at the top and the surfaces to be composited are in contact to form an assembly embryo, and rolling is performed with a rolling reduction rate of 50% using a two-roll rolling mill composed of an upper cross corrugated roller (5) and a lower cross corrugated roller (6), and after straightening, trimming, and trimming, a corrugated metal composite plate (A / B) 1 (9) is prepared;

[0040] S4, preparing the corrugated metal composite plate (A / B) 2: the corrugated metal composite plate (A / B) 1 (9) prepared in step S3 is cut in the center along the transverse direction to obtain two metal composite plates (A / B) 11 (10) and metal composite plates (A / B) 21 (11) of the same size; the oil stains and oxide films on the surfaces of the metal composite plates (A / B) 11 (10) and the metal composite plates (A / B) 21 (11) are removed and the surfaces are roughened (this grinding removes the oil stains and oxide films, which is beneficial to the subsequent plate compounding and does not affect the morphology of the knurling pattern of the composite plate after rolling), and then heated in a heating furnace without anti-oxidation measures. (4) heating to 550°C to form a 0.1 μm thick aluminum oxide layer on the surface of the metal composite plate (A / B) 11 (10) and the metal composite plate (A / B) 21 (11); then stacking the metal composite plate (A / B) 11 (10) at the bottom and the metal composite plate (A / B) 21 (11) at the top so that the surfaces to be composited are in contact to form an embryonic assembly, and rolling is performed with a rolling reduction rate of 50% using a two-roll rolling mill composed of an upper cross corrugated roller (5) and a lower cross corrugated roller (6), and after straightening, trimming, and trimming, a corrugated surface metal composite plate (A / B) 2 is prepared;

[0041] S5, repeat step S4 until a corrugated metal composite plate (A / B) 4 (15) is prepared;

[0042] S6, preparing the metal composite plate (A / B) 5: cutting the corrugated metal composite plate (A / B) 4 (15) in the center along the transverse direction to obtain two metal composite plates (A / B) 14 (16) and metal composite plates (A / B) 24 (17) of the same size; removing the oil stains and oxide films on the surfaces of the metal composite plates (A / B) 14 (16) and the metal composite plates (A / B) 24 (17) and grinding them to a rough surface, and then heating them to 550° C. in a heating furnace (4) without anti-oxidation measures to make the metal composite plates (A / B) )14(16) and the metal composite plate (A / B)24(17) are both provided with an aluminum oxide layer of 0.1 μm thick; then, the metal composite plate (A / B)14(16) is stacked together with the metal composite plate (A / B)24(17) on the top so that the surfaces to be composited are in contact with each other to form an embryonic assembly; a two-roll rolling mill consisting of an upper flat roll (7) and a lower flat roll (8) is used to perform rolling with a reduction rate of 50%; after straightening, trimming, and head and tail trimming, a metal composite plate (A / B)5(18) is prepared;

[0043] S7, annealing the metal composite plate (A / B) 5 (18) prepared in step S6 at 380°C for 1.5 hours, followed by air cooling, and finally straightening and trimming to obtain an alumina reinforced aluminum-based composite plate.

[0044] The surface of the cross-corrugated roller used in Example 1 is a curved surface formed by the intersection of transverse corrugations and longitudinal corrugations. The corrugation curve is a sine curve with a wavelength of 3.14 mm and an amplitude of 0.2 mm.

[0045] Comparative Example 1

[0046] The only difference from Example 1 is that the heating furnace without anti-oxygen measures is modified into a vacuum heating furnace.

[0047] The alumina reinforced aluminum-based composite material prepared in Example 1 was sampled and tensile tested in accordance with the relevant provisions of GB / T 6396-2008, and its tensile strength was measured to be as high as 170 MPa, which is about 25 MPa higher than that of the 1060 aluminum plate (Comparative Example 1) that has not been oxidized and is rolled in the same manner, demonstrating the good mechanical properties of the alumina reinforced aluminum-based composite material.

[0048] Example 2

[0049] A method for preparing alumina-reinforced aluminum-based composite materials by auto-oxidation cumulative rolling, comprising the following steps:

[0050] S1, plate preparation: prepare an aluminum plate A (1) with a length × width × height of 280 mm × 120 mm × 6 mm and made of 6061 aluminum alloy, prepare an aluminum plate B (2) with a length × width × height of 280 mm × 120 mm × 6 mm and made of 6061 aluminum alloy, remove oil stains and oxide films on the surfaces of the aluminum plates A (1) and B, and then grind the surfaces to be composited of the aluminum plates A (1) and B (2) to roughen them for later use;

[0051] S2, surface self-oxidation heating: the aluminum plate A (1) and the aluminum plate B (2) obtained in step S1 are heated to 470° C. in a heating furnace (4) without anti-oxidation measures, so that a 0.5 μm thick aluminum oxide layer is formed on the surface of the aluminum plate A (1) and the aluminum plate B (2);

[0052] S3, preparing a corrugated metal composite plate (A / B) 1: stacking the aluminum plates heated in step S2 in a manner such that the aluminum plate A (1) is at the bottom and the aluminum plate B (2) is at the top and the surfaces to be composited are in contact to form an assembly embryo, and rolling is performed with a rolling reduction rate of 60% using a two-roll rolling mill composed of an upper cross corrugated roller (5) and a lower cross corrugated roller (6), and after straightening, trimming, and trimming, a corrugated metal composite plate (A / B) 1 (9) is prepared;

[0053] S4, preparing the corrugated metal composite plate (A / B) 2: the corrugated metal composite plate (A / B) 1 (9) prepared in step S3 is cut in the center along the transverse direction to obtain two metal composite plates (A / B) 11 (10) and metal composite plates (A / B) 21 (11) of the same size; the oil stains and oxide films on the surfaces of the metal composite plates (A / B) 11 (10) and the metal composite plates (A / B) 21 (11) are removed and the surfaces are roughened; then, the metal composite plates (A / B) 11 (10) and the surfaces are heated to 470° C. in a heating furnace (4) without anti-oxidation measures to make the metal composite plates (A / B) 21 (11) A 0.5 μm thick aluminum oxide layer is formed on the surface of the metal composite plate (A / B) 11 (10) and the metal composite plate (A / B) 21 (11); the metal composite plate (A / B) 11 (10) is stacked together with the metal composite plate (A / B) 21 (11) on the top, and the surfaces to be composited are contacted to form an embryonic assembly; a two-roll rolling mill composed of an upper cross corrugated roller (5) and a lower cross corrugated roller (6) is used to perform rolling with a reduction rate of 60%, and after straightening, trimming, head and tail trimming, a corrugated surface metal composite plate (A / B) 2 is prepared;

[0054] S5, repeat step S4 until a corrugated metal composite plate (A / B) 9 (15) is prepared;

[0055] S6, preparation of metal composite plate (A / B) 10: The corrugated metal composite plate (A / B) 9 (15) is cut in the middle along the transverse direction to obtain two metal composite plates (A / B) 19 (16) and metal composite plates (A / B) 29 (17) of the same size; the oil stains and oxide films on the surfaces of the metal composite plates (A / B) 19 (16) and the metal composite plates (A / B) 29 (17) are removed and the surfaces are roughened; then, the metal composite plates (A / B) 19 (16) and the metal composite plates (A / B) 29 (17) are heated to 470° C. in a heating furnace (4) without anti-oxidation measures to make the metal composite plates (A / B) 19 (1 6) forming a 0.5 μm thick aluminum oxide layer on the surface of the metal composite plate (A / B) 29 (17); then stacking the metal composite plate (A / B) 19 (16) at the bottom and the metal composite plate (A / B) 29 (17) at the top so that the surfaces to be composited are in contact with each other to form an embryonic assembly, and rolling is performed with a rolling reduction rate of 60% using a two-roll rolling mill composed of an upper flat roll (7) and a lower flat roll (8), and after straightening, trimming, and trimming, a metal composite plate (A / B) is prepared. 10 (18);

[0056] S7, the metal composite plate (A / B) prepared in step S6 10 (18) The aluminum matrix composite plate was uniformly annealed at 550 °C for 2 h, followed by quenching and low-temperature aging treatment, and finally straightened and trimmed to obtain an alumina-reinforced aluminum-based composite plate.

[0057] The surface of the cross corrugated roller used in Example 2 is a curved surface formed by the intersection of transverse corrugations and longitudinal corrugations. The corrugation curve is a cosine curve with a wavelength of 6.28 mm and an amplitude of 0.5 mm.

[0058] Example 3

[0059] A method for preparing alumina-reinforced aluminum-based composite materials by auto-oxidation cumulative rolling, comprising the following steps:

[0060] S1, plate preparation: prepare an aluminum plate A(1) with a length×width×height of 300 mm×150 mm×10 mm and a material of 7075 aluminum alloy, prepare an aluminum plate B(2) with a length×width×height of 300 mm×150 mm×10 mm and a material of 7075 aluminum alloy, remove oil stains and oxide films on the surfaces of the aluminum plates A(1) and B(2), then grind the surfaces to be composited of the aluminum plates A(1) and B(2) to make them rough and set aside;

[0061] S2, surface self-oxidation heating: the aluminum plate A (1) and the aluminum plate B (2) obtained in step S1 are heated to 370° C. in a heating furnace (4) without anti-oxidation measures, so that a 1 μm thick aluminum oxide layer is formed on the surface of the aluminum plate A (1) and the aluminum plate B (2);

[0062] S3, preparing a corrugated metal composite plate (A / B) 1: stacking the aluminum plates heated in step S2 in a manner such that the aluminum plate A (1) is at the bottom and the aluminum plate B (2) is at the top and the surfaces to be composited are in contact to form an assembly embryo, and rolling is performed with a rolling reduction rate of 70% using a two-roll rolling mill composed of an upper cross corrugated roller (5) and a lower cross corrugated roller (6), and after straightening, trimming, head and tail trimming, a corrugated metal composite plate (A / B) 1 (9) is prepared;

[0063] S4, preparing the corrugated metal composite plate (A / B) 2: the corrugated metal composite plate (A / B) 1 (9) prepared in step S3 is cut in the center along the transverse direction to obtain two metal composite plates (A / B) 11 (10) and metal composite plates (A / B) 21 (11) of the same size; the oil stains and oxide films on the surfaces of the metal composite plates (A / B) 11 (10) and the metal composite plates (A / B) 21 (11) are removed and the surfaces are roughened; then, the metal composite plates (A / B) 11 (10) and the surfaces are heated to 370° C. in a heating furnace (4) without anti-oxidation measures to make the metal composite plates ( A 1 μm thick aluminum oxide layer is formed on the surface of the metal composite plate (A / B) 11 (10) and the metal composite plate (A / B) 21 (11); then the metal composite plate (A / B) 11 (10) is stacked together with the metal composite plate (A / B) 21 (11) on the top, and the surfaces to be composited are contacted to form an embryonic assembly, and a two-roll rolling mill composed of an upper cross corrugated roller (5) and a lower cross corrugated roller (6) is used to roll the metal composite plate (A / B) 2 at a rolling reduction rate of 70%, and after straightening, trimming, head and tail trimming, a corrugated surface metal composite plate (A / B) 2 is prepared;

[0064] S5, repeat step S4 until a corrugated metal composite plate (A / B) is prepared 11 (15);

[0065] S6, preparation of metal composite plate (A / B) 12 :Corrugated metal composite plate (A / B) 11 (15) cutting the metal composite plate (A / B) 111 (16) and the metal composite plate (A / B) 211 (17) in the transverse direction to obtain two pieces of the same size; removing the oil stains and oxide film on the surface of the metal composite plate (A / B) 111 (16) and the metal composite plate (A / B) 211 (17) and grinding them to a rough surface; then heating the metal composite plate (A / B) 111 (16) and the metal composite plate (A / B) 211 (17) to 370° C. in a heating furnace (4) without anti-oxidation measures to make the metal composite plate (A / B) 111 (16) and the metal composite plate (A / B) 211 (17) A 1 μm thick aluminum oxide layer is formed on the surface of the composite plate (A / B) 211 (17); then, the metal composite plate (A / B) 111 (16) is stacked on the bottom and the metal composite plate (A / B) 211 (17) is stacked on the top so that the surfaces to be composited are in contact with each other to form an assembly embryo; a two-roll rolling mill consisting of an upper flat roll (7) and a lower flat roll (8) is used to roll the composite plate at a reduction rate of 70%; and after straightening, trimming, and head and tail trimming, a metal composite plate (A / B) is prepared.12 (18);

[0066] S7, the metal composite plate (A / B) prepared in step S6 12 (18) The aluminum matrix composite plate was uniformly annealed at 410 °C for 3 h, followed by low-temperature aging treatment, and finally straightened and trimmed to obtain an alumina-reinforced aluminum-based composite plate.

[0067] The surface of the cross-corrugated roller used in Example 3 is a curved surface formed by the intersection of transverse corrugations and longitudinal corrugations. The corrugation curve is a parabola with a wavelength of 8 mm and an amplitude of 1 mm.

[0068] Figure 1 This is a schematic process diagram of the method for preparing alumina-reinforced aluminum-based composite materials by self-oxidation cumulative rolling according to Examples 1-3 of the present invention.

[0069] Figure 1 Among them, aluminum plate A—(1), aluminum plate B—(2), grinding device—(3), heating furnace—(4), upper cross corrugated roller—(5), lower cross corrugated roller—(6), upper flat roller—(7), lower flat roller—(8), corrugated surface metal composite plate (A / B) 1—(9), metal composite plate (A / B) 11—(10), metal composite plate (A / B) 21—(11), corrugated surface metal composite plate (A / B) n-2 —(12), Metal composite plate (A / B) 1n-2—(13), Metal composite plate (A / B) 2n-2—(14), Corrugated metal composite plate (A / B) n-1 —(15), Metal composite plate (A / B) 1n-1—(16), Metal composite plate (A / B) 2n-1—(17), Metal composite plate (A / B) n —(18).

[0070] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing alumina reinforced aluminum-based composite materials by self-oxidation rolling, characterized in that: The following steps are involved: (1) taking an aluminum plate, removing oil stains and oxide film on the surface and grinding it to make it rough, and heating it in an oxygen-containing atmosphere to form an aluminum oxide layer with a thickness of 0.1 to 1 μm on the surface of the aluminum plate, thereby obtaining an oxide layer aluminum plate 1; Take two pieces of the oxide layer aluminum plates 1, stack them together to form an embryonic assembly, and roll them using a two-roller mill with both upper and lower rolls being cross-corrugated rolls, and then straighten and trim them to obtain a composite plate 1; (2) cutting the composite plate 1 in the middle along the transverse direction to obtain two composite plate 1 sub-plates of the same size; The oil stains and oxide film on the surface of the sub-plate of the composite plate 1 are removed and the surface is roughened, and then heated in an oxygen-containing atmosphere to form an aluminum oxide layer with a thickness of 0.1 to 1 μm on the surface of the aluminum plate to obtain an oxide layer aluminum plate 2; The two oxide-layer aluminum plates 2 are stacked together to form an embryonic assembly, and are rolled using a two-roller rolling mill in which both the upper and lower rolls are cross-corrugated rolls, and are straightened, trimmed, and head and tail trimmed to prepare a composite plate 2; (3) Repeat step (2) n times to obtain composite plate n+2; (4) cutting the composite plate n+2 in the center along the transverse direction to obtain two composite plate n+2 sub-plates of the same size; Removing the oil stains and oxide film on the surface of the n+2 sub-plate of the composite plate and grinding it to be rough, and then heating it in an oxygen-containing atmosphere to form an aluminum oxide layer with a thickness of 0.1 to 1 μm on the surface of the aluminum plate, thereby obtaining an oxide layer aluminum plate n+3; The two pieces of the oxide layer aluminum plates n+3 are stacked together to form an embryonic embryo, and rolled using a two-roll rolling mill with both upper and lower rolls being flat rolls, and straightened, trimmed, and head and tail cut to prepare a metal composite plate; (5) Annealing, straightening and trimming the metal composite plate to obtain the alumina reinforced aluminum-based composite plate.

2. The method according to claim 1, characterized in that The n is an integer ≥1.

3. The method according to claim 1, characterized in that The material of the aluminum plate is industrial pure aluminum, 3 series aluminum alloy, 6 series aluminum alloy or 7 series aluminum alloy; the thickness of the aluminum plate is 2 to 10 mm.

4. The method according to claim 1, characterized in that In steps (1), (2) and (3), the heating temperature is 70% to 90% of the melting point of the aluminum plate.

5. The method according to claim 1, characterized in that In steps (1) and (2), the surface of the cross-corrugated roller is a curved surface formed by the intersection of transverse corrugations and longitudinal corrugations, and the corrugation curve is a sine curve, a cosine curve or a parabola; the wavelength of the corrugation curve is ≤8mm, and the amplitude is ≤1mm.

6. The method according to claim 1, characterized in that In steps (1), (2) and (3), the rolling reduction rate is 50% to 70%.

7. An alumina reinforced aluminum-based composite material prepared according to the method according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Continuous laminating and rolling method for corrugated interface double-metal composite board

    CN108746204A

  • Method for smoothing continuous ply rolling of metal-based composite plates

    CN108971226A

  • Processing technology of steel-aluminum composite plate

    CN110509632A

  • Preparation method of aluminum-based composite material with controllable reinforcement phase distribution

    CN114083103A

  • Efficient rolling forming method for high-performance steel-aluminum-aluminum alloy transition joint

    CN116393512A