Preparation method of silver nanowire film with high light transmittance and low emissivity
By cleaning the silver nanowire film with L-ascorbic acid, the problem of maintaining network integrity when removing PVP is solved, and the preparation of silver nanowire films with high light transmission and low emissivity is achieved, which simplifies the process and reduces production costs and avoids Bubble damage problem improves conductivity and infrared emissivity.
Patent Information
- Application Number
- CN202410919405.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, when preparing silver nanowire films, it is difficult to effectively remove PVP on the surface of silver nanowires to maintain network integrity. The use of sodium borohydride method will cause bubbles to destroy the film, increasing production costs and complexity.
The silver nanowire film was cleaned using the reduction ability of L-ascorbic acid, destroying the silver oxygen bonds on the PVP molecular chain, removing PVP and reducing the contact resistance of the silver nanowires, and maintaining network integrity through low temperature conditions and solvent evaporation welding.
The preparation of silver nanowire films with high light transmission and low emissivity is realized, which reduces the contact resistance of silver nanowires, maintains the network shape and adhesion, simplifies the process and reduces production costs, and avoids bubble damage problems.
Smart Images

Figure CN118951034A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optoelectronic materials, and in particular relates to a method for preparing a silver nanowire film with high light transmittance and low emissivity. Background Art
[0002] In the field of infrared imaging, infrared low-emissivity materials can be used to manufacture infrared cameras and thermal imaging equipment. These materials can reduce the thermal radiation of the equipment itself in the infrared band and improve the sensitivity and resolution of the imaging equipment. The transmittance of infrared low-emissivity materials is another important consideration. Transmittance refers to the degree of transmittance of visible light by the material, that is, the energy loss when light passes through the material. Infrared low-emissivity materials with higher transmittance are compatible with radiation in the infrared-visible light band and enhance the equipment's ability to detect and image targets.
[0003] In the field of infrared camouflage, infrared low-emissivity materials can be used to manufacture infrared camouflage coatings and materials. Infrared camouflage aims to reduce the thermal radiation characteristics of the target in the infrared band, making it difficult to detect or identify in infrared detection and infrared guidance systems. Infrared low-emissivity materials can effectively reduce the infrared radiation of the target, making it blend into the surrounding environment and improving the camouflage effect. In infrared camouflage, in addition to hiding the thermal radiation characteristics of the target in the infrared band, it is also necessary to keep the appearance of the target in the visible light band consistent with the surrounding environment to avoid being detected in visible light observation or infrared and visible light fusion systems. Therefore, selecting materials with high visible light transmittance can make the target have an appearance similar to the environment in the visible light band, improving the camouflage effect. Infrared low emissivity and high visible light transmittance have important tactical and strategic significance for military stealth technology, reconnaissance and infrared detection avoidance in assault missions.
[0004] As a new type of nanomaterial, silver nanowires have good optoelectronic properties. The assembled infrared low-emissivity film has excellent optoelectronic properties, transmittance, flexibility and many other functions. Therefore, it can perfectly adapt to a variety of application scenarios and is the first choice for designing modern visible light-infrared compatible materials. Therefore, it is particularly important to study the infrared low emissivity of the silver nanowire network near the 8-14 micron infrared band and the high transmittance in the visible light band. At present, the cost of the welding process to reduce the junction resistance between wires is high. At the same time, the insulating layer PVP introduced on the surface of the silver nanowire during synthesis requires a large amount of ethanol, water and acetone, including multiple centrifugation to remove it, which poses a risk of destroying the silver nanowire network; when using sodium borohydride solution, the hydrogen anions in the solution can be used to destroy the Ag-O bond between PVP and Ag atoms to achieve the purpose of removing PVP, but the bubbles generated during the reduction of hydrogen anions will destroy the silver nanowire network, so it is not convenient to use. Summary of the invention
[0005] The present invention provides a method for preparing a silver nanowire film with high light transmittance and low emissivity, which utilizes the mild reducing ability of L-ascorbic acid to clean and weld the silver nanowires through solvent evaporation, and can ensure the integrity of the silver nanowire network when the PVP on the surface of the silver nanowire is washed away.
[0006] To achieve the above objectives, the present invention adopts the following technical solutions: A method for preparing a silver nanowire film with high light transmittance and low emissivity comprises the following steps: (1) adding 0.1-0.5 g of silver nitrate, 0.1-1.6 g of PVP and 0.05-0.1 g of copper nitrate to 80-100 ml of ethylene glycol, and keeping the mixture at 160-180° C. for 7-12 hours. The obtained product is centrifuged, washed and dispersed to obtain a silver nanowire suspension; (2) using a spray gun to spray the prepared silver nanowire suspension onto a PET substrate to obtain a silver nanowire film; (3) Dissolve L-ascorbic acid in deionized water and stir magnetically to prepare a solution with a concentration of 0.19-0.3 mol / L; (4) placing the silver nanowire film in the solution and keeping it at 15-25°C for 120-250 seconds to remove the polyvinyl pyrrolidone (PVP) on the surface of the silver nanowire film; (5) After taking out the silver nanowire film from the solution, wash it with deionized water and vacuum dry it for 1 hour to obtain a clean silver nanowire film.
[0007] Beneficial effects: The present invention provides a method for preparing a silver nanowire film with high light transmittance and low emissivity. The environmentally friendly and unregulated L-ascorbic acid is used to clean the silver nanowires under low temperature conditions. The L-ascorbic acid destroys the silver oxygen bond between the carbonyl oxygen and the silver atom on the PVP molecular chain, so that the non-conductive PVP is separated from the surface of the nanowires. Under the premise of maintaining the silver nanowire network morphology and the adhesion between the substrate, the contact resistance of the silver nanowires is effectively reduced, thereby improving the conductivity, and finally obtaining a silver nanowire film with both high light transmittance and low emissivity. The traditional sodium borohydride method will cause film damage due to bubbles generated by the solution, while the L-ascorbic acid cleaning technology proposed in the present invention can maintain the integrity of the silver nanowire network, and the PVP ligand on the surface of the silver nanowire is removed. Because of the insulating properties of PVP itself, the contact resistance of the treated silver nanowire is significantly reduced, and finally the infrared emissivity in the 8-14 micron band is reduced. In addition, the preparation process of the present invention is simple and easy to operate, and the production cost is low, which can be applied to the preparation and improvement of silver nanowire films. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Figure 1 is an XRD pattern of the silver nanowire film after washing with L-ascorbic acid in Example 1 of the present invention; Figure 2 This is an infrared photograph of the silver nanowire film after being cleaned with L-ascorbic acid in Example 1 of the present invention; Figure 3 is a graph showing the ultraviolet-visible light transmittance of the silver nanowire film in Example 1 of the present invention; Figure 4 is an XRD pattern of the silver nanowire film after washing with L-ascorbic acid in Example 2 of the present invention; Figure 5 This is an infrared photograph of the silver nanowire film after being cleaned with L-ascorbic acid in Example 2 of the present invention; Figure 6 This is a graph showing the UV-visible light transmittance of the silver nanowire film in Example 2 of the present invention; Figure 7 is an XRD pattern of the silver nanowire film after washing with L-ascorbic acid in Example 3 of the present invention; Figure 8 This is an infrared photograph of the silver nanowire film after being washed with L-ascorbic acid in Example 3 of the present invention; Fig. 9 This is a graph of the ultraviolet visible light transmittance of the silver nanowire film in Example 3 of the present invention; Fig.10 PET substrate without silver nanowire coverage; Fig.11 This is an infrared photo of an untreated silver nanowire film; Fig.12 Silver nanowire film treated with sodium borohydride solution. DETAILED DESCRIPTION
[0009] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments: Example 1
[0010] A method for preparing a silver nanowire film with high light transmittance and low emissivity comprises the following steps: Step (1), add 0.5 g of silver nitrate, 1.6 g of PVP and 0.05 g of copper nitrate into 80 ml of ethylene glycol, keep warm at 160° C. for 7 hours, and the obtained product is centrifuged, washed and dispersed to obtain a silver nanowire suspension.
[0011] Step (2), using a spray gun to spray the prepared silver nanowire suspension onto a PET substrate to obtain a silver nanowire film (400 mg / m -2 ); Step (3), dissolving L-ascorbic acid in deionized water and stirring with a magnetic force to prepare a solution A with a concentration of 0.2 mol / L; Step (4), placing the silver nanowire film into solution A, heating to 20° C., and keeping the temperature for 209 s; Step (5), after removing the silver nanowire film from the solution, washing with deionized water and vacuum drying for 1 hour, a clean silver nanowire film is obtained.
[0012] The infrared emissivity of the silver nanowire film prepared in this embodiment was measured using an infrared camera; like Figure 1 As shown in the figure, the diffraction peaks of silver at 38.1°, 44.2°, 64.4° and 77.5° correspond to the (111), (200), (220) and (311) crystal planes of silver, respectively, and it can be seen that the silver nanowires are in a face-centered cubic phase after cleaning; like Figure 2 As shown, infrared photos of the silver nanowire film before and after washing with L-ascorbic acid show that, at the same actual temperature, the film covered with silver nanowires emits infrared energy with lower intensity (emissivity is 0.33) compared to the high-brightness background; Figure 3 3 is the UV-visible light transmittance diagram of the silver nanowire film of this embodiment. It can be seen that the transmittance at 550nm is 92.38%. Example 2
[0013] A method for preparing a silver nanowire film with high light transmittance and low emissivity comprises the following steps: Step (1), adding 0.3 g of silver nitrate, 1 g of PVP and 0.1 g of copper nitrate into 80 ml of ethylene glycol, keeping the mixture at 160° C. for 7 hours, and centrifuging, washing and dispersing the obtained product to obtain a silver nanowire suspension; Step (2), weigh a certain amount of L-ascorbic acid, dissolve it in deionized water and stir it magnetically to prepare a 0.3 mol / L A solution for later use; Step (3), spray the silver nanowire suspension onto the PET substrate using a spray gun to obtain a silver nanowire film (400 mg / m -2 );spare; Step (4), placing the silver nanowire film into solution A, heating to 15° C., and keeping the temperature for 250 seconds; Step (5), after removing the silver nanowire film from the solution, washing with deionized water and vacuum drying for 1 hour, a clean silver nanowire film is obtained.
[0014] The infrared emissivity of the silver nanowire film prepared in this example was measured using an infrared camera; like Figure 4As shown in the figure, the diffraction peaks of silver at 38.1°, 44.2°, 64.4° and 77.5° correspond to the (111), (200), (220) and (311) crystal planes of silver, respectively, and it can be seen that the silver nanowires are in a face-centered cubic phase after cleaning; Figure 5 Infrared photos of the silver nanowire film before and after washing with L-ascorbic acid in this example. Under the same actual temperature, compared with the high-brightness background, the film covered with silver nanowires emits infrared energy with lower intensity, and the infrared emissivity is 0.35; Figure 6 3 is the UV-visible light transmittance diagram of the silver nanowire film of this embodiment. It can be seen that the transmittance at 550nm is 92.66%. Example 3
[0015] A method for preparing a silver nanowire film with high light transmittance and low emissivity comprises the following steps: Step (1), adding 0.1 g of silver nitrate, 0.1 g of PVP and 0.1 g of copper nitrate into 80 ml of ethylene glycol, keeping the mixture at 160° C. for 7 hours, and centrifuging, washing and dispersing the obtained product to obtain a silver nanowire suspension; Step (2), weigh a certain amount of L-ascorbic acid, dissolve it in deionized water and stir it magnetically to prepare a 0.19 mol / L A solution for later use; Step (3), spray the silver nanowire suspension onto the PET substrate using a spray gun to obtain a silver nanowire film (400 mg / m -2 );spare; Step (4), placing the silver nanowire film into solution A, heating to 25° C., and keeping the temperature for 120 seconds; Step (5), after taking out the above silver nanowire film from the solution, washing it with deionized water, and vacuum drying it to obtain a clean silver nanowire film.
[0016] The infrared emissivity of the silver nanowire film was measured using an infrared camera; like Figure 7 As shown in the figure, the diffraction peaks of silver at 38.1°, 44.2°, 64.4° and 77.5° correspond to the (111), (200), (220) and (311) crystal planes of silver, respectively, and it can be seen that the silver nanowires are in a face-centered cubic phase after cleaning; Figure 8 Infrared photos of the silver nanowire film before and after washing with L-ascorbic acid in this example. Under the same actual temperature, compared with the high-brightness background, the film covered with silver nanowires emits infrared energy with lower intensity, and the emissivity is 0.31; Fig. 9: is the UV-visible light transmittance diagram of the silver nanowire film of this embodiment. It can be seen that the transmittance at 550nm is 92.55%.
[0017] Fig.10 It is a PET substrate without silver nanowires covering, and the emissivity is close to 1; Fig.11 This is an infrared photo of an untreated silver nanowire film. It can be seen that the infrared emissivity of the untreated silver nanowire is between 0.5 and 0.6, which is much higher than the emissivity of the film treated with L-ascorbic acid solution. This indicates that the method of the present invention effectively reduces the contact resistance of the silver nanowire after treatment, thereby improving the conductivity. Fig.12 It is a silver nanowire film treated with sodium borohydride solution in the prior art. It can be seen that the bubbles generated by the sodium borohydride solution cause large-scale shedding of the silver nanowires, while after treatment by the method of the present invention, face-centered cubic phase of the silver nanowires can be seen, indicating that the method of the present invention can maintain the network morphology of the silver nanowires and the adhesion between the substrate on the basis of removing PVP on the surface of the silver nanowires.
[0018] The above-described embodiments are only preferred embodiments of the present invention, and the protection scope of the present invention is not limited thereto. Any equivalent substitutions or changes made by those skilled in the art on the basis of the present invention are within the protection scope of the present invention.
Claims
1. A method for preparing a silver nanowire film with high light transmittance and low emissivity, characterized in that: The following steps are involved: preparing a silver nanowire suspension; spraying the prepared silver nanowire suspension on a substrate to obtain a silver nanowire film; An L-ascorbic acid solution is prepared, and the silver nanowire film is placed in the solution, and the solution is kept warm under low temperature conditions to remove polyvinyl pyrrolidone on the surface of the silver nanowire film; and a clean silver nanowire film is obtained after washing and drying.
2. The method for preparing a silver nanowire film with high light transmittance and low emissivity according to claim 1, characterized in that: The specific process of preparing the silver nanowire suspension is as follows: silver nitrate, PVP and copper nitrate are added to ethylene glycol, and the mixture is kept at 160-180° C. for 7-12 hours. The obtained product is centrifuged, washed and dispersed to obtain the silver nanowire suspension.
3. The method for preparing a silver nanowire film with high light transmittance and low emissivity according to claim 2, characterized in that: The silver nitrate is 0.1-0.5 grams, the PVP is 0.1-1.6 grams, and the copper nitrate is 0.05-0.1 grams.
4. The method for preparing a silver nanowire film with high light transmittance and low emissivity according to claim 2 or 3, characterized in that: The ethylene glycol is 80-100 ml.
5. The method for preparing a silver nanowire film with high light transmittance and low emissivity according to claim 1, characterized in that: The concentration of the L-ascorbic acid solution is 0.19-0.3 mol / L.
6. The method for preparing a silver nanowire film with high light transmittance and low emissivity according to claim 1, characterized in that: The low temperature condition is 15-25℃.
7. The method for preparing a silver nanowire film with high light transmittance and low emissivity according to claim 1 or 6, characterized in that: The low temperature insulation time is 120-250s.
8. The method for preparing a silver nanowire film with high light transmittance and low emissivity according to claim 1, characterized in that: The drying process was vacuum drying for 1 hour.
9. The method for preparing a silver nanowire film with high light transmittance and low emissivity according to claim 1, characterized in that: The substrate is a PET substrate.