Grinding process method for regulating and controlling residual stress distribution of bearing raceway
By using the combination of high grinding wheel linear speed and high workpiece speed in bearing raceway grinding, the process parameters are optimized and the raceway residual stress distribution is regulated, and the problem of unconsidered raceway residual stress distribution in traditional technology is solved, which is significantly improved. Fatigue life and performance of bearings.
Patent Information
- Application Number
- CN202410901353.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional bearing raceway grinding technology lacks consideration and control of raceway residual stress distribution, resulting in short fatigue life of domestic bearings, insufficient service performance and safety, and limited market competitiveness.
Adopt the combination of high grinding wheel linear velocity and high workpiece speed to optimize grinding process parameters, increase the raceway peak residual compressive stress and compressive stress depth, reduce the peak residual tensile stress and stress extreme difference, and pass the specific grinding wheel speed and workpiece speed parameters Design and regulate the residual stress distribution of raceways.
It effectively improves the grinding quality and fatigue life of bearings, significantly extends the actual operating stability, narrows the service life gap with imported high-end bearings, and enhances the market competitiveness of domestic bearings.
Smart Images

Figure CN118951967A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of bearing manufacturing, and in particular relates to a grinding process method for regulating the residual stress distribution of a bearing raceway. Background Art
[0002] Bearing raceway grinding is one of the most critical processes in bearing manufacturing. The grinding quality of the raceway will directly affect the performance and fatigue life of the bearing. Traditional bearing raceway grinding usually only considers dimensional tolerances, form and position tolerances, and surface roughness, without considering surface integrity issues such as residual stress distribution in the raceway caused by grinding. The surface integrity defects of the raceway will greatly shorten the fatigue life of the bearing. Since traditional bearing manufacturing lacks key surface integrity indicators to control the surface quality of the bearing raceway, and lacks process methods to regulate key indicators, the fatigue life of domestic bearings is much lower than that of internationally renowned brands. Therefore, in response to the demand for improving bearing fatigue life, it is necessary to provide the key indicators that affect bearing fatigue life, namely, the characterization parameters of the residual stress distribution of the raceway, as well as the grinding process methods to regulate the residual stress distribution of the bearing raceway.
[0003] The technical problems existing in the existing bearing raceway grinding technology mainly include the following points:
[0004] 1. Lack of comprehensive quality control indicators: Traditional bearing raceway grinding mainly focuses on dimensional tolerance, geometric tolerance and surface roughness, but ignores surface integrity issues such as residual stress distribution in the raceway that may be caused during the grinding process. This limitation leads to an incomplete assessment of bearing raceway quality.
[0005] 2. Raceway surface integrity defects: Since surface integrity issues such as raceway residual stress caused by grinding are not considered, the raceway may have defects such as microcracks and stress concentration, which will significantly shorten the fatigue life of the bearing.
[0006] 3. Lack of key indicator control technology: Traditional bearing manufacturing lacks key surface integrity indicators for controlling the surface quality of the bearing raceway, such as the characterization parameters of the residual stress distribution of the raceway. At the same time, there is also a lack of specific process methods for controlling these key indicators.
[0007] 4. Short fatigue life of domestic bearings: Due to the above technical problems, the fatigue life of domestic bearings is much lower than that of internationally renowned brands. This not only affects the performance and safety of bearings, but also limits the market competitiveness of domestic bearings.
[0008] 5. Insufficient optimization of grinding process parameters: The existing grinding process parameters may not be fully optimized and cannot effectively control key indicators such as the residual stress distribution of the raceway. Therefore, it is necessary to further study and optimize the grinding process parameters to improve the grinding quality of the bearing raceway.
[0009] In summary, the existing technology has many problems in bearing raceway grinding, especially the lack of consideration and control of surface integrity issues such as raceway residual stress distribution. In order to solve these problems, it is necessary to conduct in-depth research on the key indicators that affect the fatigue life of bearings and develop corresponding control process methods to improve the quality and fatigue life of domestic bearings. Summary of the invention
[0010] In view of the problems existing in the prior art, the present invention provides a grinding process method for regulating the residual stress distribution of a bearing raceway.
[0011] In order to slow down the initiation and expansion of raceway fatigue cracks and improve the contact fatigue performance of the raceway, the present invention needs to increase the peak residual compressive stress and residual compressive stress depth of the raceway, reduce the peak residual tensile stress and its depth, and reduce the residual stress range. (1) The grinding process method and process parameter design for regulating the residual stress distribution of the bearing raceway should preferably adopt a combination of high grinding wheel linear speed and high workpiece speed; (2) The regulation target of the residual stress distribution of the bearing raceway needs to increase the peak residual compressive stress σ c and residual compressive stress depth h c , reducing the peak residual tensile stress σ t and its depth h t , and reduce the residual stress extreme difference σ d .
[0012] Furthermore, (3) the residual stress extreme difference σ of bearing raceway grinding d represents the peak residual tensile stress σ t Value and peak residual compressive stress σ c The difference of values is expressed as:
[0013] σ d =σ t -σ c
[0014] In the formula, σ t is the peak residual tensile stress value, σ c is the peak compressive residual stress.
[0015] Furthermore, (4) a grinding process method for regulating the residual stress distribution of a bearing raceway and a design of process parameters thereof are characterized in that, under the condition that the bearing material is a high carbon chromium alloy (DIN100Cr6) and a ceramic sintered corundum grinding wheel (Saint-Gobain-Norton), the grinding wheel linear speed v can be selected. s =80m / s, workpiece speed v w Grinding parameters: feed speed f = 2.51 m / s, feed speed f = 10 μm / s.
[0016] In combination with the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solutions to be protected by the present invention are as follows:
[0017] First, the present invention includes a grinding process method for regulating the residual stress distribution of a bearing raceway and a control target for the residual stress distribution of a bearing raceway. The grinding process method for regulating the residual stress distribution of a bearing raceway mainly includes a combination of grinding wheel speed and workpiece speed parameters that meet the design requirements of process parameters.
[0018] Second, the present invention can effectively regulate the residual stress distribution of the bearing raceway, overcome the problems of poor grinding quality of the rolling bearing raceway surface and difficulty in optimizing the grinding process parameters, and provide a reasonable and effective machining process method and process parameters for improving the service performance and fatigue life of high-end bearing products. By effectively regulating the residual stress distribution of the bearing raceway, the present invention can significantly improve the long-term stability of the actual operation of the bearing and its fatigue life, and narrow the life gap with imported high-end bearings.
[0019] Third, as auxiliary evidence of the inventiveness of the claims of the present invention, it is also reflected in the following important aspects:
[0020] (1) The grinding process method of the bearing raceway proposed in the present invention effectively regulates the residual stress distribution of the bearing raceway, and can usually significantly improve the actual test life of the bearing. In engineering practice, the actual test life range of the bearing manufactured using the technical solution of the present invention is sometimes relatively large. The reason is that there are many parts processing and assembly processes for the bearing, and the production environment of each process, the processing errors of the bearing-related parts, the stability of the automatic loading and unloading mechanism, the wear of the grinding wheel and other process conditions cause inconsistencies and instabilities.
[0021] (2) The technical solution of the present invention overcomes the traditional technical prejudice in bearing manufacturing and breaks through the existing process technology and methods.
[0022] (3) The expected benefits and commercial value of the technical solution of the present invention after transformation are:
[0023] Taking the test bearing model 7002P4 used for fatigue life test of the present invention as an example, since there is a big gap between the fatigue life of domestic bearings, especially high-end bearings and international famous brand bearings, according to the current market price, the price of international famous brand bearings (such as NSK) is generally 3 times or more than that of domestic bearings.
[0024] In summary, the process method proposed in the present invention will significantly improve the fatigue life of domestic bearings and bring huge profits and commercial value to enterprises. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1It is a flow chart of a grinding process method for regulating the residual stress distribution of a bearing raceway provided by an embodiment of the present invention;
[0026] Figure 2 is a schematic diagram of residual stress distribution of a bearing raceway provided by an embodiment of the present invention;
[0027] Figure 3 It is a schematic diagram of the bearing raceway residual stress distribution control effect provided by an embodiment of the present invention. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0029] like Figure 1 As shown, the grinding process method for regulating the residual stress distribution of the bearing raceway provided by the embodiment of the present invention comprises the following steps:
[0030] S101: A combination of high grinding wheel speed and high workpiece speed should be preferred;
[0031] S102: Need to increase the raceway peak residual compressive stress σ c and residual compressive stress depth h c , reducing the peak residual tensile stress σ t and its depth h t , and reduce the residual stress extreme difference σ d .
[0032] Embodiment 1:
[0033] The grinding process method for regulating the residual stress distribution of the bearing raceway provided in the embodiment of the present invention should adopt a combination of grinding wheel speed and workpiece speed parameters that meet the design requirements of process parameters; it is necessary to increase the peak residual compressive stress σ c and residual compressive stress depth h c , reducing the peak residual tensile stress σ t and its depth h t , and reduce the residual stress extreme difference σ d . ;
[0034] The residual stress range of bearing raceway grinding d represents the peak residual tensile stress σ t Value and peak residual compressive stress σ c The difference of values is expressed as:
[0035] σ d =σ t -σ c
[0036] In the formula, σ t is the peak residual tensile stress value, σ c is the peak compressive residual stress.
[0037] When the bearing material is high carbon chromium alloy (DIN100Cr6) and ceramic sintered corundum grinding wheel (Saint-Gobain-Norton), the combination of high grinding wheel speed and high workpiece speed should be preferred.
[0038] It should be noted that the embodiments of the present invention can be implemented by hardware, software, or a combination of software and hardware. The hardware part can be implemented using dedicated logic; the software part can be stored in a memory and executed by an appropriate instruction execution system, such as a microprocessor or dedicated design hardware. It can be understood by a person of ordinary skill in the art that the above-mentioned devices and methods can be implemented using computer executable instructions and / or contained in a processor control code, such as a carrier medium such as a disk, CD or DVD-ROM, a programmable memory such as a read-only memory (firmware), or a data carrier such as an optical or electronic signal carrier. Such code is provided on the carrier medium. The device and its modules of the present invention can be implemented by hardware circuits such as very large-scale integrated circuits or gate arrays, semiconductors such as logic chips, transistors, etc., or programmable hardware devices such as field programmable gate arrays, programmable logic devices, etc., can also be implemented by software executed by various types of processors, and can also be implemented by a combination of the above-mentioned hardware circuits and software, such as firmware.
[0039] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.
Claims
1. A grinding process method for regulating the residual stress distribution of a bearing raceway, It is characterized in that In order to slow down the initiation and expansion of raceway fatigue cracks and improve the contact fatigue performance of the raceway, it is necessary to increase the peak residual compressive stress and residual compressive stress depth of the raceway, reduce the peak residual tensile stress and its depth, and reduce the residual stress range. Under the condition that the bearing material is made of high carbon chromium alloy and ceramic sintered corundum grinding wheel, the grinding process method for regulating the residual stress distribution of the bearing raceway should preferably adopt a combination of high grinding wheel linear speed and high workpiece speed.
2. The grinding process for regulating the residual stress distribution of the bearing raceway according to claim 1, It is characterized in that The control target of the bearing raceway residual stress distribution is to increase the raceway peak residual compressive stress σ c and residual compressive stress depth h c , reducing the peak residual tensile stress σ t and its depth h t , and reduce the residual stress extreme difference σ d . Residual stress extreme value σ d represents the peak residual tensile stress σ t Value and peak residual compressive stress σ c The difference in values.
3. The grinding process for regulating the residual stress distribution of the bearing raceway according to claim 1, It is characterized in that The combination of high grinding wheel linear speed and high workpiece speed should be used first. When the bearing material is high carbon chromium alloy and ceramic sintered corundum grinding wheel, the grinding wheel linear speed v can be selected. s =80m / s, workpiece speed v w Grinding parameters: feed speed f = 2.51 m / s, feed speed f = 10 μm / s.
Citation Information
Patent Citations
Bearing raceway high-speed grinding method considering surface integrity, parameters and application
CN117161834A