Construction solid waste regenerated green cement blanket and preparation method thereof
By extruding the broken PP plastic and antioxidants and other additives out of recycled fibers, combined with the calcined base material and fine aggregates, a green cement blanket of construction solid waste recycled is formed, solving the environmental pollution problems caused by traditional treatment methods. , realizes effective recycling of resources and efficient regeneration of building materials.
Patent Information
- Application Number
- CN202411105741.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional construction waste and industrial solid waste treatment methods lead to environmental pollution and low resource utilization.
Recycled fibers are obtained by extruding the broken PP plastic by adding antioxidants and ultraviolet absorbers, mixing them to make a fiber web, and combining them with the calcined base material and fine aggregates to form a solid waste regeneration through a needle puncture process Green cement blanket.
It realizes the resource utilization of construction waste and industrial solid waste, reduces environmental pollution, provides an environmentally friendly and low-cost green preparation method for solid waste regeneration, and has good physical and mechanical properties and weather resistance.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of industrial solid waste recycling, and in particular to a green cement blanket recycled from construction solid waste and a preparation method thereof. Background Art
[0002] With the acceleration of urbanization, the treatment of construction waste and industrial solid waste (such as PP polypropylene plastic) has become an increasingly serious problem. Traditional treatment methods not only occupy a large amount of land resources, but also may cause environmental pollution. Therefore, the development of new materials that can effectively utilize these wastes has become a research focus. Summary of the invention
[0003] In order to overcome the defects of the prior art, a green cement blanket recycled from construction solid waste and a preparation method thereof are provided to solve the problem that traditional treatment methods of construction waste may cause environmental pollution.
[0004] In order to achieve the above purpose, a green cement blanket for recycling construction solid waste is provided, comprising:
[0005] Crushing the waste PP plastic;
[0006] Add antioxidants and ultraviolet absorbers to the crushed waste PP plastics to extrude and obtain recycled fibers;
[0007] chopping the regenerated fiber and mixing it with polyester fiber to form a fiber web;
[0008] Mixing steel slag, mineral slag and desulfurized gypsum to obtain a base material;
[0009] The base material is calcined and ground to a specific surface area of 500 m 2 / kg~800m 2 / kg, adding activator to the grinding train;
[0010] The ground base material is mixed evenly with fine aggregate to obtain dry mortar powder;
[0011] The mortar dry powder is spread between two layers of fiber mesh and the two layers of fiber mesh are tightly connected by needle punching to form a green cement blanket for recycling solid waste from construction.
[0012] Furthermore, an auxiliary antioxidant is added to the crushed waste PP plastic.
[0013] Furthermore, the added amount of the antioxidant is 0.1% to 0.5% of the waste PP plastic, the added amount of the ultraviolet absorber is 0.1% to 0.5% of the waste PP plastic, and the added amount of the auxiliary antioxidant is 0.1% to 0.3% of the waste PP plastic.
[0014] Furthermore, the ultraviolet absorber is 2,6-di-tert-butyl-4-methylphenol or 2,4-di-tert-butylphenyl antioxidant, the ultraviolet absorber is 2'-hydroxy-5'-methylphenyl ultraviolet absorber, and the auxiliary antioxidant is calcium stearate.
[0015] Furthermore, the mass ratio of the steel slag, the slag and the desulfurized gypsum is 30-40:45-55:10-20.
[0016] Furthermore, the activator is CaO or Na2SO4.
[0017] Furthermore, the fine aggregate is iron tailings with a particle size less than 0.5 mm.
[0018] Furthermore, the fiber web has a thickness of 3 to 5 mm and a density of 600 to 1000 g / m 2 .
[0019] The present invention provides a green cement blanket recycled from construction solid waste, characterized in that the green cement blanket recycled from construction solid waste is prepared by adopting the above-mentioned preparation method of the green cement blanket recycled from construction solid waste.
[0020] The beneficial effect of the present invention is that the green cement blanket recycled from construction solid waste of the present invention is a green cement blanket prepared by recycling construction waste. The green cement blanket recycled from construction solid waste of the present invention can be used as a temporary or permanent building material and can realize the resource utilization of solid waste.
[0021] The preparation method of the green cement blanket recycled from construction solid waste of the present invention is an environmentally friendly and low-cost green preparation method for solid waste recycling. The method can effectively utilize waste PP plastics and industrial solid waste, reduce environmental pollution, and improve resource utilization.
[0022] The construction solid waste recycled green cement blanket of the present invention fully utilizes waste PP plastics and industrial solid waste, realizes the effective recycling of resources, and helps to reduce the impact of construction waste and industrial solid waste on the environment. DETAILED DESCRIPTION
[0023] The present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the relevant invention, rather than to limit the invention.
[0024] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below in conjunction with the embodiments.
[0025] The present invention provides a green cement blanket for recycling construction solid waste, comprising:
[0026] S1. Crushing the waste PP plastic.
[0027] In this embodiment, waste PP plastics are collected, cleaned and decontaminated, and then crushed.
[0028] S2. Add antioxidants and ultraviolet absorbers to the crushed waste PP plastics and extrude them to obtain recycled fibers.
[0029] As a preferred embodiment, an auxiliary antioxidant is also added to the crushed waste PP plastic.
[0030] In this embodiment, the amount of antioxidant added is 0.1% to 0.5% of the mass of the waste PP plastic. The amount of ultraviolet absorber added is 0.1% to 0.5% of the mass of the waste PP plastic. The amount of auxiliary antioxidant added is 0.1% to 0.3% of the mass of the waste PP plastic.
[0031] Specifically, the ultraviolet absorber is 2,6-di-tert-butyl-4-methylphenol or 2,4-di-tert-butylphenyl antioxidant.
[0032] The ultraviolet absorber is 2'-hydroxy-5'-methylphenyl ultraviolet absorber.
[0033] The auxiliary antioxidant is calcium stearate.
[0034] Specifically, step S2 includes: feeding the crushed PP plastic into a single-screw or twin-screw extruder, and performing melt extrusion at a temperature of 200° C. to 230° C. and a speed of 200 m / min to 600 m / min.
[0035] At this stage, 0.1% to 0.5% of 2,6-di-tert-butyl-4-methylphenol or 2,4-di-tert-butylphenyl antioxidant, 0.1% to 0.5% of 2'-hydroxy-5'-methylphenyl UV absorber and 0.1% to 0.3% of auxiliary antioxidant calcium stearate are added.
[0036] The extruded regenerated fiber is cooled by a water bath at 10°C to 20°C to rapidly cool and solidify the fiber.
[0037] S3, chopping the regenerated fiber into short pieces and mixing them with polyester fiber to form a fiber web.
[0038] As a preferred embodiment, the thickness of the fiber mesh is 3-5 mm and the density is 600-1000 g / m 2 .
[0039] Specifically, step S3 includes:
[0040] S31, cutting the regenerated fibers after cooling and solidification into short fibers of 5 mm to 10 mm, and using an opener to loosen the fibers.
[0041] S32, mix the short-cut fibers and polyester fibers evenly to ensure that the fibers are evenly distributed. Use an air-laid web machine or a mechanical web machine to lay the mixed fibers into a web having a thickness of 3 to 5 mm and a density of 600 to 1000 g / m 2 Fiber web.
[0042] S33, through the needle machine at 300 needles / cm 2 Up to 600 stitches / cm 2 The fiber web is needle-punched at a density of 200 to 300 times / min to improve its strength and stability.
[0043] S34, finally undergoing a heat treatment at 120°C to 180°C to ensure that the fiber web has good thermal stability and dimensional stability.
[0044] S4. Mix steel slag, mineral slag and desulfurized gypsum to obtain a base material.
[0045] As a preferred implementation mode, the mass ratio of steel slag, slag and desulfurized gypsum is 30-40:45-55:10-20.
[0046] Specifically, step S4 includes:
[0047] S41, use finely ground steel slag (specific surface area 600 ~ 800m 2 / kg), ground slag (specific surface area 500~700m 2 / kg), desulfurized gypsum (specific surface area 700~900m 2 / kg) as the main component, and compounded in proportion of 30-40 parts by mass of steel slag, 45-55 parts by mass of slag, and 10-20 parts by mass of desulfurized gypsum.
[0048] S42, putting the compounded base material into a mixer, mixing at a speed of 100 rpm to 300 rpm, and mixing time of 10 min to 20 min.
[0049] S43. The premixed base material is sent into a rotary kiln or a fluidized bed calcining furnace and calcined at a temperature of 600°C to 800°C for 1 to 2 hours. Low-temperature calcination can activate the active components in the slag and steel slag and improve the early strength of the cementitious material.
[0050] S5. After calcining the base material, grind it to a specific surface area of 500m 2 / kg~800m 2 / kg, adding activator in the grinding train.
[0051] As a preferred embodiment, the activator is CaO or Na2SO4.
[0052] Specifically, step S5 includes grinding the calcined base material in a ball mill or a vertical mill until the specific surface area is 500m 2 / kg~800m 2 / kg. 1% to 3% (mass percentage) of activator is added during the grinding process. The activator is CaO (quicklime) or Na2SO4, etc., to improve the activity of the cementitious material.
[0053] S6. Evenly mix the ground base material and fine aggregate to obtain dry mortar powder.
[0054] In this embodiment, the fine aggregate is iron tailings with a particle size less than 0.5 mm.
[0055] S7. Spread the mortar dry powder between the two layers of fiber mesh and connect the two layers of fiber mesh tightly by needle punching to form a green cement blanket for recycling solid waste from construction.
[0056] Specifically, step S7 includes:
[0057] S71. Spread the mortar dry powder evenly between the upper and lower layers of fiber mesh.
[0058] S72. The upper and lower layers of fiber mesh are connected vertically by a needle punching process to form a dense vertical mesh, so as to relatively fix the mortar dry powder and ensure a relatively uniform distribution of the mortar dry powder.
[0059] The green cement blanket recycled from construction solid waste of the present invention is a green cement blanket prepared by recycling construction waste. The green cement blanket recycled from construction solid waste of the present invention can be used as a temporary or permanent building material and can realize the resource utilization of solid waste.
[0060] The preparation method of the green cement blanket recycled from construction solid waste of the present invention is an environmentally friendly and low-cost green preparation method for solid waste recycling. The method can effectively utilize waste PP plastics and industrial solid waste, reduce environmental pollution, and improve resource utilization.
[0061] The construction solid waste recycled green cement blanket of the present invention fully utilizes waste PP plastics and industrial solid waste, realizes the effective recycling of resources, and helps to reduce the impact of construction waste and industrial solid waste on the environment.
[0062] The green cement blanket recycled from construction solid waste of the present invention has good physical and mechanical properties and weather resistance, and its tensile strength is ≥3MPa, and its compressive strength is ≥20MPa. It can meet the strength requirements of general slope protection and temporary facilities and is suitable for the construction of temporary facilities in various construction occasions.
[0063] The method for using the green cement blanket recycled from construction solid waste of the present invention comprises the following steps:
[0064] a. Preparation before construction: roll the solid waste recycled green cement blanket into dry storage.
[0065] b. Construction process: When laying, be careful not to use machinery or other equipment to drag too hard.
[0066] c. Watering and maintenance: 6kg / m2 of water is required per square meter. 2 ~9kg / m 2 Water the surface evenly (calculated based on 10mm thickness) and spray evenly from the edge to the middle until the color of the cement blanket becomes darker.
[0067] About 2 hours after the first watering, water it for the second time, with less water than the first time. Water it for the third time after an interval of about 20 hours, with less water than the second time. After the second watering, wait for the water to evaporate and dry before solidifying. When the average day and night temperature is higher than 30℃, the surface should be covered with plastic film, etc.
[0068] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the inventive concept. For example, the above features are replaced with (but not limited to) technical features with similar functions disclosed in the present application.
Claims
1. A method for preparing green cement blanket recycled from construction solid waste, characterized in that: include: Crushing the waste PP plastic; Add antioxidants and ultraviolet absorbers to the crushed waste PP plastics to extrude and obtain recycled fibers; chopping the regenerated fiber and mixing it with polyester fiber to form a fiber web; Mixing steel slag, mineral slag and desulfurized gypsum to obtain a base material; The base material is calcined and ground to a specific surface area of 500 m 2 / kg~800m 2 / kg, adding activator to the grinding train; The ground base material is mixed evenly with fine aggregate to obtain dry mortar powder; The mortar dry powder is spread between two layers of fiber mesh and the two layers of fiber mesh are tightly connected by needle punching to form a green cement blanket for recycling solid waste from construction.
2. The method for preparing green cement blanket recycled from construction solid waste according to claim 1, characterized in that: Auxiliary antioxidants are also added to the crushed waste PP plastics.
3. The method for preparing green cement blanket recycled from construction solid waste according to claim 2, characterized in that: The added amount of the antioxidant is 0.1% to 0.5% of the waste PP plastic, the added amount of the ultraviolet absorber is 0.1% to 0.5% of the waste PP plastic, and the added amount of the auxiliary antioxidant is 0.1% to 0.3% of the waste PP plastic.
4. The method for preparing green cement blanket recycled from construction solid waste according to claim 3, characterized in that: The ultraviolet absorber is 2,6-di-tert-butyl-4-methylphenol or 2,4-di-tert-butylphenyl antioxidant, the ultraviolet absorber is 2'-hydroxy-5'-methylphenyl ultraviolet absorber, and the auxiliary antioxidant is calcium stearate.
5. The method for preparing green cement blanket recycled from construction solid waste according to claim 1, characterized in that: The mass ratio of the steel slag, the slag and the desulfurized gypsum is 30-40:45-55:10-20.
6. The method for preparing green cement blanket recycled from construction solid waste according to claim 1, characterized in that: The activator is CaO or Na2SO4.
7. The method for preparing green cement blanket recycled from construction solid waste according to claim 1, characterized in that: The fine aggregate is iron tailings with a particle size less than 0.5 mm.
8. The method for preparing green cement blanket recycled from construction solid waste according to claim 1, characterized in that: The fiber web has a thickness of 3 to 5 mm and a density of 600 to 1000 g / m 2 .
9. A green cement blanket recycled from construction solid waste, characterized in that: The green cement blanket recycled from construction solid waste is prepared by the preparation method of the green cement blanket recycled from construction solid waste as described in any one of claims 1 to 8.
Citation Information
Patent Citations
Method for enhancing mechanical properties of paste filling material by using plastic waste
CN106007502A
Method for processing cement pipe piles by carbon fibers and recycled concrete
CN109400029A
All-solid-waste-based low-carbon green ecological cementing material and manufacturing method thereof
CN115321848A
Cement blanket and manufacturing method and application thereof
CN116330758A
Solid waste-based gel, paste, preparation method and filling method
CN116675473A