Preparation method of super-hydrophobic antifouling anti-drag cilia array surface

By preparing magnetic microcilia arrays under the action of static and dynamic magnetic fields, and combining laser marking machine to process micropore arrays, the problems of high cost and complex process in the existing technology are solved, and low-cost and environmentally friendly superhydrophobicity are achieved Anti-fouling and drag-reducing surface reduces biological pollution and frictional resistance when ships navigate in the ocean.

CN118953570APending Publication Date: 2024-11-15JILIN UNIVERSITY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411034478.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing superhydrophobic surface preparation methods are costly, complex in processes and contain hazardous chemicals, which are difficult to widely use in marine applications and cannot effectively reduce the biological pollution and frictional resistance of ships when navigating in the ocean.

Method used

Under the action of static and dynamic magnetic fields, magnetic microcilia arrays were prepared using a magnetic solution mixed with polydimethylsiloxane and carbonyl iron powder, and superhydrophobic magnetic micro-microns were formed by hexadecyl trimethoxysilane modified SiO2 particles to form superhydrophobic magnetic micro-microns by forming cetyl trimethoxysilane-modified SiO2 particles. Cilia arrays are made by laser marking machine to prepare low-cost, environmentally friendly ultra-hydrophobic anti-fouling and drag-reducing surfaces.

Benefits of technology

Achieving a low-cost, environmentally friendly ultra-hydrophobic anti-fouling and drag-reducing surface, optimizing anti-fouling and drag-reducing performance by regulating the cilia array structure, reducing biofouling and frictional resistance of ships in the ocean, reducing energy consumption, and suitable for a variety of Base material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118953570A_ABST
    Figure CN118953570A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a super-hydrophobic antifouling anti-drag cilia array surface. The preparation method comprises the following steps: processing an ordered micropore array on a polydimethylsiloxane flexible substrate by adopting an ultraviolet laser marking machine, casting a mixed magnetic solution of a PDMS prepolymer and carbonyl iron powder on the ordered micropore array, growing magnetic microcilia under the action of static and dynamic magnetic fields and micropores, and then immersing the surface into a mixed solution of modified nano SiO2 particles and absolute ethyl alcohol to obtain the magnetic microcilia. And drying to obtain the super-hydrophobic magnetic microcilia array. The preparation method has the advantages of being environmentally friendly, simple in preparation process and low in cost, the surface micro-nano structure enables the array to reach a stable Cassie state, an air layer can be formed in water, the super-hydrophobic effect is achieved, the cilia structure of the array can reduce adhesion sites of algae, mussels and other fouling organisms in the ocean, and the service life of the array is prolonged. The air layer and the array cilium-shaped structure cooperate to realize the antifouling and resistance-reducing functions in the navigation process of the navigation body, so that the energy consumption is reduced, and the economic loss is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of surface anti-fouling and drag reduction, and specifically relates to a method for preparing a super-hydrophobic anti-fouling and drag-reducing ciliary array surface. Background Art

[0002] When surface ships, submarines and marine vessels sail in the ocean, they face the problems of biofouling and underwater friction resistance due to their interaction with the flow of seawater, which leads to reduced speed and range, or even surface damage. Therefore, exploring new methods of anti-fouling and drag reduction has important engineering significance for reducing the harm of biofouling and reducing the energy consumption of surface friction resistance.

[0003] Due to its special surface wetting characteristics, superhydrophobic surfaces have great application prospects in the development of antifouling and drag-reducing surfaces. Specific micro-nano structures such as T-shaped, conical, columnar, mushroom-shaped, etc. are constructed on the surface, and the upward Laplace force can be used to stabilize the droplets in the Cassie state with an air layer, so that low surface energy liquids can also not wet on its surface. For example, the claw structure prepared by 3D printing, the T-shaped nanocolumn concave angle structure array processed by reactive ion etching, and the superhydrophobic microciliary structure obtained by fluorination treatment of the surface by template method can achieve antifouling, superoleophobic, superhydrophobic and other functions. However, these methods are costly, the preparation process is complicated, and some involve fluorine-containing chemicals, which limits the actual marine application of such methods. In engineering, there is an urgent need to develop a low-cost, superhydrophobic surface preparation method with excellent superhydrophobic properties and antifouling and drag-reducing capabilities. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a super-hydrophobic antifouling and drag-reducing ciliary surface which is environmentally friendly, has a simple preparation process and is low-cost.

[0005] The process involved in the present invention is: under the action of static and dynamic magnetic fields, a magnetic solution of polydimethylsiloxane (PDMS) prepolymer and carbonyl iron powder is evenly mixed and cast on a microporous mold to prepare a magnetic microciliary array; due to the action of the micropores and the magnetic field, the magnetic mixed solution is spontaneously arranged along the direction of the micropores and the magnetic field to form an ordered conical ciliary array; then, the surface is immersed in a mixed solution of hexadecyltrimethoxysilane-modified SiO2 particles and anhydrous ethanol, and a super-hydrophobic magnetic microciliary array surface is obtained after drying; a micro / nano hierarchical structure is formed on the super-hydrophobic magnetic microciliary array surface.

[0006] The present invention specifically comprises the following steps:

[0007] 1. Preparation of superhydrophobic SiO2

[0008] Disperse 2-5 g SiO2 in a beaker containing 200-500 mL deionized water and anhydrous ethanol (v / v: 1 / 3-1 / 5), ultrasonicate for 30-50 min, add 1-3 mL hexadecyltrimethoxysilane to the mixed suspension, then magnetically stir the suspension in a water bath at 80-100° C. for 1-1.5 h, separate the modified SiO2 with a high-speed centrifuge, wash the obtained powder with anhydrous ethanol for 3-5 times, and dry at 60-80° C. for 10-15 h.

[0009] 2. Preparation of Microwell Array Substrate

[0010] A laser marking machine was used to process a regularly arranged micropore array with a diameter of 300-800 μm, a depth of 290-320 μm, and a spacing of 100-300 μm on the substrate. The substrate was treated 12-15 times with parameters of an average current of 8 A-10 A, a repetition frequency of 20-30 kHz, and a scanning speed of 200-260 mm / s, and the micropore array substrate was ultrasonically cleaned with anhydrous ethanol for 5-10 minutes.

[0011] 3. Preparation of Magnetic Cilia Arrays

[0012] The PDMS precursor, curing agent and magnetic powder are mixed in a weight ratio of 10:1:10 to 8:0.5:8, 0.5 to 0.8 g of the magnetic mixture is poured on the substrate and vacuumed for 2 to 6 minutes to remove bubbles and fill the microwell array, spin-coated at a speed of 200 to 300 rpm for 36 to 54 seconds, and then ultrasonically treated for 5 to 10 minutes. Finally, the bottom surface of the microwell array substrate is placed vertically on a permanent magnet, and a static magnetic field is applied and maintained for 10 to 15 seconds, which can attract magnetic particles to fill the array holes and generate tiny cilia in the outer area of ​​the microwells. The permanent magnet periodically moves back and forth and left and right close to the substrate, and an oscillating magnetic field is applied about 25 to 35 times to further induce the tiny cilia floating outside the hole to move to the cavity and converge into a complete cilia array structure. The prepared magnetic cilia array is kept close to the permanent magnet and placed in a drying oven, and cured at 70° to 80°C for 50 to 100 minutes.

[0013] 4. Preparation of Superhydrophobic Fluorine-free Magnetic Cilia Array

[0014] Dissolve 0.5-0.8 g of modified SiO2 powder in anhydrous ethanol (50-80 mL) and ultrasonically treat for 10-15 min to mix it evenly. Then immerse the magnetic ciliary array in the above mixed suspension for 2-5 min, take it out and dry it at room temperature for 2-3 h to obtain a superhydrophobic magnetic microciliary array with a height of 500-2000 μm.

[0015] The SiO2 particle size in step 1 is 10 to 60 nm.

[0016] The microwell array substrate in step 2 can be made of materials such as glass, magnesium alloy, silicon and polytetrafluoroethylene.

[0017] The magnetic powder in step 3 can be iron powder, cobalt powder, nickel powder, etc., with a particle size of 1 to 10 μm, and the permanent magnet is a neodymium iron boron magnet.

[0018] The preparation of the super-hydrophobic anti-fouling and drag-reducing magnetic ciliary array by the present invention involves a multi-scale "millimeter-micrometer-nanometer" hierarchical structure. The surface can capture the air layer to achieve the Cassie state and realize the super-hydrophobic property. In addition, the ciliary structure of the array can reduce the adhesion sites of fouling organisms such as algae and mussels in the ocean. The synergistic effect of the ciliary structure of the array and super-hydrophobicity better achieves the purpose of anti-fouling and drag reduction.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention uses a laser marker to prepare a super-hydrophobic anti-fouling and drag-reducing surface on a polymer surface, which has the characteristics of environmental protection, simple preparation process, short preparation process time and low cost. By adjusting the ratio of polymer and carbonyl iron powder, the quality and rotation speed of spin coating, the scanning parameters of the laser marker, etc., the conical ciliary arrays with different aspect ratios and arrangements can be controllably obtained, so that the anti-fouling and drag-reducing performance can be optimized to obtain the best parameters. In addition, when the super-hydrophobic anti-fouling and drag-reducing ciliary array is immersed in water, an air layer can be formed on the surface, and a silver mirror phenomenon occurs. On the one hand, it can greatly reduce the contact area between seawater and the solid surface, change the wall boundary layer flow field structure, reduce the wall shear stress, and thus reduce the friction resistance of the moving solid wall. On the other hand, it can hinder the contact between fouling organisms in seawater and the solid surface, so as to reduce biological attachment. The super-hydrophobic magnetic ciliary array preparation method can be used for any substrate, such as glass, magnesium alloy, silicon and polytetrafluoroethylene. The prepared super-hydrophobic ciliary array has the functions of drag reduction and anti-fouling, so that the ship can achieve energy reduction and optimal drag reduction effect under full working condition operation. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of the preparation process of the magnetic ciliary array of the present invention;

[0022] Figure 2 This is a top view of the magnetic ciliary array involved in the present invention;

[0023] Figure 3 This is a side view of the superhydrophobic magnetic ciliary array involved in the present invention. DETAILED DESCRIPTION

[0024] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments.

[0025] The specific steps of the present invention are as follows:

[0026] 1. Preparation of superhydrophobic SiO2

[0027] 5g SiO2 was dispersed in a beaker containing 500mL deionized water and anhydrous ethanol (v / v: 1 / 3) and ultrasonicated for 50min. 2.5mL hexadecyltrimethoxysilane was added to the mixed suspension, and then the suspension was magnetically stirred in a water bath at 80℃ for 1.5h. The modified SiO2 was separated by a high-speed centrifuge, and the obtained powder was washed 3 times with anhydrous ethanol and dried at 60℃ for 15h.

[0028] 2. Preparation of Microwell Array Substrate

[0029] A micropore array with a diameter of 600 μm, a depth of 290 μm, and a spacing of 150 μm was processed on the substrate using an ultraviolet laser marking machine. The substrate was treated 15 times with parameters of an average current of 8 A, a repetition frequency of 20 kHz, and a scanning speed of 200 mm / s, and the micropore array substrate was ultrasonically cleaned with anhydrous ethanol for 15 minutes.

[0030] 3. Preparation of Magnetic Cilia Arrays

[0031] The steps for preparing magnetic ciliary arrays are as follows: Figure 1 As shown, PDMS precursor, curing agent and magnetic powder are mixed in a weight ratio of 10:1:10, 0.5g of the magnetic mixture is spin-coated on the microwell array substrate at a speed of 300rpm for 54s, and vacuumed for 2min to remove bubbles and fill the microwell array. The sample is then ultrasonically treated for 10min to make the surface flat and smooth. Finally, the bottom surface of the microwell array substrate is placed vertically on a permanent magnet, and a static magnetic field is applied and maintained for 10s, which can attract magnetic particles to fill the array holes and produce tiny cilia in the outer area of ​​the microwells. The permanent magnet periodically moves back and forth and left and right close to the substrate, and an oscillating magnetic field is applied about 25 times to further induce the tiny cilia floating outside the hole to move to the cavity and converge into a complete ciliary structure. The prepared magnetic ciliary array is kept close to the permanent magnet and placed in a drying oven, and cured at 70°C for 90min.

[0032] 4. Preparation of Superhydrophobic Fluorine-free Magnetic Cilia Array

[0033] 0.8 g of modified SiO2 powder was dissolved in anhydrous ethanol (80 mL) and ultrasonically treated for 15 min to mix it evenly. Then the magnetic cilia were immersed in the above mixed suspension for 2 min, taken out and dried at room temperature for 3 h to obtain a superhydrophobic magnetic microciliary array with a height of 1980 μm.

[0034] The SiO2 particle size in step 1 is 20 nm.

[0035] The microwell array substrate material in step 2 is PDMS, with a size of 1.3 mm×2.8 mm and an arrangement of 18×36.

[0036] The magnetic powder in step 3 is carbonyl iron powder with a particle size of 6 μm, and the permanent magnet is a neodymium iron boron magnet with a specification of 51×25×13 mm. 3 , the magnetic field strength is 350mT.

[0037] The wettability test was carried out on the surface of the prepared superhydrophobic antifouling and drag reducing ciliary array, and a contact angle meter was used to measure the impact of a 10μm droplet on the surface of the superhydrophobic antifouling and drag reducing ciliary array. The average rolling angle of the test three times was 3.5°, indicating that the superhydrophobic antifouling and drag reducing ciliary array has a smaller rolling angle; when the hydrophobic antifouling and drag reducing ciliary array is placed in water, it can be clearly seen that there is a layer of silvery-white light film on the surface of the ciliary array, which is the air layer captured by the superhydrophobic antifouling and drag reducing ciliary array underwater. In addition, if a 10μL droplet is used to impact the array, the droplets on the surface rebound and no droplets remain, indicating that the superhydrophobic antifouling and drag reducing ciliary array has good superhydrophobic properties.

Claims

1. A method for preparing a super-hydrophobic anti-fouling and drag-reducing cilia array surface, characterized in that The following steps are involved: 1.1 Preparation of superhydrophobic SiO2 Disperse 2-5 g SiO2 in a beaker containing 200-500 mL deionized water and anhydrous ethanol (v / v: 1 / 3-1 / 5), ultrasonicate for 30-50 min, add 1-3 mL hexadecyltrimethoxysilane to the mixed suspension, then stir the suspension magnetically in a water bath at 80-100° C. for 1-1.5 h, separate the modified SiO2 with a high-speed centrifuge, wash the obtained powder with anhydrous ethanol for 3-5 times, and dry at 60-80° C. for 10-15 h; 1.2 Preparation of microwell array substrate A laser marking machine was used to process a regularly arranged micro-hole array with a diameter of 300-800 μm, a depth of 290-330 μm, and a spacing of 100-300 μm on the substrate, wherein the substrate was processed 12-15 times with an average current of 8 A-10 A, a repetition frequency of 20-30 kHz, and a scanning speed of 200-260 mm / s, and the micro-hole array substrate was ultrasonically cleaned with anhydrous ethanol for 5-10 minutes; 1.3 Preparation of magnetic ciliary arrays The PDMS precursor, curing agent and magnetic powder are mixed in a weight ratio of 10:1:10 to 8:0.5:8, 0.5 to 0.8 g of the magnetic mixture is poured on the substrate and vacuumed for 2 to 6 minutes to remove bubbles and fill the microwell array, and the mixture is spin-coated at a speed of 200 to 300 rpm for 36 to 54 seconds, followed by ultrasonic treatment for 5 to 10 minutes. Finally, the bottom surface of the microwell array substrate is placed vertically on a permanent magnet, and a static magnetic field is applied and maintained for 10 to 15 seconds, which can attract magnetic particles to fill the array holes and generate tiny cilia in the outer area of ​​the microwells. The permanent magnet periodically moves back and forth and left and right close to the substrate, and an oscillating magnetic field is applied about 25 to 35 times to further induce the tiny cilia floating outside the hole to move to the cavity and converge into a complete cilia array structure. The prepared magnetic cilia array is kept close to the permanent magnet and placed in a drying oven, and cured at 70° to 80° C. for 50 to 100 minutes. 1.4 Preparation of superhydrophobic fluorine-free magnetic ciliary arrays Dissolve 0.5-0.8 g of modified SiO2 powder in anhydrous ethanol (50-80 mL) and ultrasonically treat for 10-15 min to mix it evenly. Then immerse the magnetic ciliary array in the above mixed suspension for 2-5 min, take it out and dry it at room temperature for 2-3 h to obtain a superhydrophobic magnetic microciliary array with a height of 500-2000 μm.

2. The method for preparing the super-hydrophobic anti-fouling and drag-reducing ciliary array surface according to claim 1, characterized in that: The SiO2 particle size in step 1.1 is 10 to 60 nm.

3. The method for preparing the super-hydrophobic anti-fouling and drag-reducing ciliary array surface according to claim 1, characterized in that: The microwell array substrate in step 2 can be made of materials such as glass, magnesium alloy, silicon and polytetrafluoroethylene.

4. The method for preparing the super-hydrophobic anti-fouling and drag-reducing ciliary array surface according to claim 1, characterized in that: The magnetic powder in step 1.3 can be iron powder, cobalt powder, nickel powder, etc., with a particle size of 1 to 10 μm, and the permanent magnet is a neodymium iron boron magnet.

Citation Information

Cited By

  • Method for improving stability of underwater streamline cavity

    CN119929058A