Method for extracting aluminum oxide from fly ash by acid-base combination method

By using anhydrous sodium carbonate activation and acid-leaching alkali extraction processes in fly ash, the problems of low carbonization efficiency and high production cost in traditional acid-base combined methods are solved, and the efficient extraction of alumina is achieved and the leaching of aluminum is improved. The purity of alumina meets industrial standards.

CN118954556APending Publication Date: 2024-11-15NINGXIA UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411020356.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The traditional acid-base combined process of extracting alumina from fly ash has low efficiency, high production cost, large carbon emissions, and complex process parameter adjustment, making it difficult to meet the requirements of industrial applications.

Method used

The fly ash is activated by low-cost anhydrous sodium carbonate as alkaline ingredients, and combined with the process flow of acid leaching, alkali extraction and acid analysis, and optimize the ash alkali ingredients ratio, acid leaching and alkali extract types and Under experimental conditions, an efficient alumina extraction process was formed, replacing the CO2 carbonization process, and improving the leachate of aluminum and the purity of alumina.

Benefits of technology

The efficient extraction of alumina in fly ash was achieved, the leaching rate of aluminum reached 97.4%, and the content of alumina products reached 98.62%, which comply with national level 3 and above standards, reducing production costs and carbon emissions, and simplifying the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954556A_ABST
    Figure CN118954556A_ABST
Patent Text Reader

Abstract

The invention discloses a method for extracting aluminum oxide from fly ash by an acid-base combination method, which comprises the following steps of: firstly, crushing a fly ash raw material by using a crusher, mixing and calcining the crushed fly ash raw material and an alkaline ingredient according to a certain proportion to obtain an activated blocky solid, crushing the activated blocky solid, performing acid leaching, fully stirring until the solid is dissolved, performing suction filtration for multiple times, and recovering and clarifying an acid leaching solution; dropwise adding an alkaline solution into the pickle liquor, adjusting the pH value to 6.5-7.0 so that iron ions and aluminum ions completely form precipitates at the moment, and recovering the precipitates through suction filtration for multiple times; dissolving the precipitate with an alkaline solution, adjusting the pH value to 12.5-14.0, carrying out suction filtration for multiple times, and recovering clear filtrate; dropwise adding a certain amount of acid solution into the clarified filtrate to form white emulsion, and recycling white aluminum hydroxide precipitate through multiple times of suction filtration; in conclusion, the process for extracting the aluminum oxide by utilizing the improved acid-base combination method is one of effective ways for realizing harmlessness, reduction and recycling of the fly ash, and has great benefits for environmental pollution improvement, energy conservation and efficiency improvement in the thermal power industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of mineral processing and metallurgy, and in particular relates to a method for extracting aluminum oxide by using fly ash acid-base combined method. Background Art

[0002] my country's annual fly ash production is expected to reach 620 million tons, ranking first in the world. Its production is increasing year by year, which has brought great pressure to the environment. The power industry is the main source of fly ash. Usually, 1 ton of fly ash is produced for every 2 tons of coal consumed. It not only occupies a large amount of land resources, but also causes the harmful elements in fly ash to pollute the soil and groundwater due to rainwater erosion. The fly ash dust will also cause the surrounding air to be polluted, seriously affecting people's respiratory health. Therefore, it is urgent to make fly ash harmless, reduce its volume and make it a resource.

[0003] The formation process of fly ash is as follows: Fly ash is the waste product after coal combustion. Coal is first ground into fine coal powder in the power plant, and then sprayed into the combustion furnace for suspended combustion, producing high-temperature flue gas with a large amount of combustion residues. The flue gas is discharged after dust removal and purification, and the combustion residues settle to form fly ash.

[0004] The composition of fly ash varies with the type of coal, and mainly contains complex oxide mineral phases such as silicon, aluminum, iron and calcium, as well as incompletely burned carbon. In addition, it also contains a small amount of inorganic trace elements such as phosphorus, sulfur and chlorine, which has potential recycling value. In particular, high-aluminum fly ash, whose aluminum content is as high as more than 30%, can effectively replace bauxite, the raw material for smelting aluminum. Therefore, the technology of extracting alumina from fly ash is one of the key technologies to improve the comprehensive utilization rate of fly ash and the economic benefits of the power industry, and has received widespread attention at home and abroad.

[0005] There are many methods to extract alumina from high-alumina fly ash, mainly sintering method, acid method, acid-base combined method, etc. The sintering method mainly includes limestone sintering method, soda lime sintering method and sodium carbonate roasting method. The sintering method generally has a roasting temperature of up to 1200°C, and the leaching rate of aluminum in fly ash and the purity of alumina can reach more than 80%. However, the sintering method has obvious disadvantages, such as too high sintering temperature, complex process and the generation of a large amount of waste slag. The acid method mainly includes sulfuric acid leaching method, ammonium fluoride dissolution method and ammonium aluminum sulfate method. The recovery rate of aluminum in fly ash can reach more than 90% by acid leaching method. The acid-base combined method is to first mix the alkali and fly ash in a certain proportion and roast them, then use acid to dissolve and activate the clinker to obtain calcium-containing silica gel and aluminum-containing filtrate. When an alkaline solution is added to the filtrate to adjust the pH to a certain value, a sodium aluminate solution can be formed, and then CO2 gas is introduced into the sodium aluminate solution for carbonization to precipitate Al(OH)3. After calcination, Al2O3 products can be obtained. The alumina leaching rate using this method can reach 90%, and the alumina content can reach more than 87%. However, the traditional acid-base combined method for aluminum extraction has complex process parameters to adjust, and there is room for improvement in both the alumina leaching rate and the purity of the alumina product. In addition, the traditional acid-base combined method uses CO2 gas carbonization, which has low reaction efficiency and produces a large amount of CO2 waste gas. It neither meets the requirements of the national carbon emission policy nor meets the industrial assessment standards.

[0006] The present invention is mainly improved on the basis of the acid-base combined method. First, low-cost anhydrous sodium carbonate is used as an alkaline ingredient to activate fly ash, and then "acid leaching" and "alkaline extraction" and other steps are adopted. After the alkaline extraction, the "acid precipitation" method is introduced, that is, a trace amount of acid solution is used to quickly form aluminum hydroxide precipitation from the sodium aluminate solution, thereby shortening the aluminum precipitation time, greatly improving production efficiency and saving costs. This link can effectively replace the CO2 carbonization process. The present invention also forms a series of implementation cases suitable for aluminum extraction from fly ash by optimizing the experimental conditions such as the ash-alkali ingredient ratio, the type of acid leaching solution and the type of alkaline extraction solution, providing necessary experimental data for the industrial application of the fly ash aluminum extraction process.

[0007] The main chemical reaction equations involved in each step of the process are:

[0008] The chemical reaction formulas involved in step 2 are:

[0009] Al6Si2O 13 +3Na2CO3=2NaAlSiO4+4NaAlO2+3CO2↑

[0010] SiO2+Na2CO3=Na2SiO3+CO2↑

[0011] Al2O3+Na2CO3=2NaAlO2+CO2↑

[0012] The chemical reaction formulas involved in step three are:

[0013] NaAlSiO4+4HCl=NaCl+AlCl3+H2SiO3↓+H2O

[0014] The chemical reaction formulas involved in step 4 are:

[0015] FeCl3+3NaOH=3NaCl+Fe(OH)3↓

[0016] AlCl3+3NaOH=3NaCl+Al(OH)3↓

[0017] The chemical reaction formulas involved in step 5 are:

[0018] Al(OH)3+NaOH=NaAlO2+2H2O

[0019] The chemical reaction formulas involved in step six are:

[0020] NaAlO2+HCl+H2O=Al(OH)3↓+NaCl

[0021] In summary, the present invention provides a method of extracting alumina from fly ash using fly ash as raw material, using sodium carbonate activation and combining an acid-base combined method. The process is simple and the production cost is low. It is of great significance to the recycling of fly ash resources and the protection of the local ecological environment. Summary of the invention

[0022] The present invention adopts the process flow of sodium carbonate activation + acid-base combined method to efficiently extract aluminum oxide from fly ash. A method for extracting aluminum oxide from fly ash by acid-base combined method is characterized by comprising the following steps:

[0023] Step 1, crush the fly ash raw material and sieve it through a sieve with a mesh size of 200 or more, collect the fly ash S0 component that passes through the sieve, weigh 20.0 to 20.01 g for later use;

[0024] Step 2, the fly ash S0 is mixed with the alkaline ingredients, ground evenly, calcined to obtain clinker, and then crushed, passed through a sieve with mesh size of 200 or more, and the components passing through the sieve are collected to obtain activated powder clinker S1;

[0025] Step 3: pour the acid solution into a container, add the powdered clinker S1 into the acid solution under heating conditions of 80-81° C. and stir until S1 is completely dissolved, and then gradually form floccules, continue heating and stirring for 4-5 hours until a colloid F1 with a uniform texture is formed, and the filtrate L1 obtained by multiple filtration of the colloid F1 is a clear solution; this step requires the recovery of the filtrate L1;

[0026] Step 4: add the alkaline solution to L1 under heating and stirring conditions at 80-81°C to gradually obtain floccules F2, stop adding when the pH is adjusted to 6.5-7.0, filter the floccules F2 multiple times to obtain a cream-like precipitate S3, and obtain a primary alkali extraction filtrate L2; this step requires the recovery of the precipitate S3;

[0027] Step 5, first dissolving the precipitate S3 in 200-300 mL of water, then continuing to drop an alkali solution into S3 under heating conditions of 80-81° C. to form a flocculant F3, stopping the dropwise addition when the pH is adjusted to 12.5-14.0, continuing heating and stirring for 30-40 min, and then filtering the flocculant F3 multiple times to obtain a secondary alkali extraction filtrate L3, and recovering the filtrate L3;

[0028] Step six, add the acid solution described in step two to the filtrate L3 while stirring, gradually forming floccules F4, stop adding when the pH is adjusted to 9.5-10.0, continue heating and stirring for 1.0-1.1h; filter the floccules F4 several times, and place the white precipitate S5 obtained by filtration in an oven to dry, then crush it through a sieve with a mesh size of 60 or above, collect the components passing through the sieve, and then place it in a muffle furnace for calcination to obtain a white powder solid S6.

[0029] The fly ash raw material comes from the Guodian Shizuishan Power Plant. According to the X-ray diffraction fluorescence spectrum detection, the chemical components of the obtained fly ash are as follows: Al2O3 content is 28.40-28.401wt.%; SiO2 content is 44.86-44.861wt.%; Fe2O3 content is 7.38-7.381wt.%; CaO content is 7.11-7.111wt.%; SO3 content is 4.76-4.761wt.%; MgO content is 1.70-1.701wt.%; TiO2 content is 1.49-1.491wt.%; K2O content is 1.47-1.471wt.%; Na2O content is 1.05-1.051wt.%; C The content of l is 0.791~0.792wt.%; the content of P2O5 is 0.301~0.302wt.%; the content of ZrO2 is 0.137~0.138wt.%; the content of SrO is 0.130~0.131wt.%; the content of MnO is 0.092~0.093wt.%; the content of BaO is 0.055~0.056wt.%; the content of ZnO is 0.047~0.048wt.%; the content of V2O5 is 0.032~0.033wt.%; the content of PbO is 0.023~0.024wt.%; the content of CeO2 is 0.022~0.023wt.%; the content of other chemical components is 0.131wt.%. (Other components include one or more of Cr2O3, Y2O3, MoO3, CuO, NiO, As2O3, Ga2O3, Rb2O, Nd2O3, Co3O4, Nb2O, Bi2O3, Au, SeO2, GeO2, and Br).

[0030] In the step 2, the weight ratio of fly ash to alkaline ingredients is 1:(1.0-1.5) (preferably in the range of 1:(1.05-1.45));

[0031] The alkaline ingredients are one or more of sodium carbonate or sodium bicarbonate;

[0032] In the step 2, the fly ash is mixed with the alkaline ingredients and then placed in a muffle furnace for calcination at a temperature of 830 to 832° C. for a calcination time of 3.0 to 3.05 hours.

[0033] In the steps 3 to 5, the “multiple filtrations” refer to filtration with water at least twice, with the amount of water used each time being 950-1050 mL;

[0034] In the step six, the "multiple filtrations" refer to filtering with water and ethanol at least twice in sequence, with the amount of water or ethanol used each time being 950-1050 mL.

[0035] In the step 3, the acid solution is 6.45-6.47 mol / L HCl solution, HNO3 solution, H2SO4 solution, oxalic acid, or citric acid;

[0036] The preparation method of 6.45-6.47 mol / L HCl solution is as follows: take 537-538 mL of 36-38% HCl solution and dilute it to 1000 mL with deionized water;

[0037] The method for preparing the 6.45-6.47 mol / L HNO3 solution is as follows: take 448-449 mL of a 65-68% HNO3 solution and dilute it to 1000 mL with deionized water;

[0038] The preparation method of the 6.45-6.47 mol / L H2SO4 solution is as follows: take 350-351 mL of 95-98% H2SO4 solution and dilute it to 1000 mL with deionized water.

[0039] The preparation method of the 6.45-6.47 mol / L oxalic acid (molecular formula: H2C2O4) solution is as follows: take 813.16-815.68 g of oxalic acid dihydrate solid and dilute it to 1000 mL with deionized water.

[0040] The preparation method of the 6.45-6.47 mol / L citric acid (molecular formula: C6H8O7) solution is as follows: take 1354.76-1358.96 g of citric acid monohydrate solid and dilute it to 1000 mL with deionized water.

[0041] In the step 3, the white colloidal precipitate S2 obtained by suction filtration needs to be dried, taken out and crushed, and then passed through a sieve with a mesh size of 200 or more, and the components passing through the sieve are collected and then placed in a muffle furnace for calcination;

[0042] The drying temperature of the colloidal precipitate S2 is 60-61° C., and the drying time is 12-24 hours;

[0043] In the step 3, the S4 is placed in a muffle furnace and calcined at a constant temperature of 650-652° C. for 6.0-6.05 h;

[0044] In the step 5, at the same time, the reddish brown precipitate S4 is obtained by suction filtration, dried, and then placed in a muffle furnace for calcination;

[0045] In the step 5, the S4 is placed in an oven at a drying temperature of 80 to 81° C. for 24 to 25 hours;

[0046] In the step 5, the S4 is placed in a muffle furnace and calcined at a constant temperature of 650-652° C. for 6.0-6.05 h.

[0047] In the step 4, the alkaline solution is one or more of the following four types;

[0048] The NaOH solution is prepared as follows: weigh 159.9-160.1 g of NaOH solid and dilute it to 500 mL with deionized water to prepare a NaOH solution with a concentration of 7.99-8.01 mol / L;

[0049] The KOH solution is prepared as follows: weigh 224.5-224.8 g of KOH solid and dilute it to 500 mL with deionized water to prepare a KOH solution with a concentration of 7.99-8.01 mol / L;

[0050] The preparation method of NH3·H2O solution is as follows: 374-375 mL of 25-28% ammonia water is measured and diluted to 500 mL with deionized water, and the preparation concentration is 9.99-10.1 mol / L;

[0051] The preparation method of NH4HCO3 solution is as follows: weigh 394.9-395.1 g of NH4HCO3 solid and dilute it to 500 mL with deionized water to prepare NH4HCO3 solution with a concentration of 9.99-10.1 mol / L.

[0052] The preparation method of (NH4)2CO3 solution is as follows: weigh 784.9-793.5g (NH4)2CO3 solid and dilute it to 500mL with deionized water to prepare (NH4)2CO3 solution with a concentration of 9.99-10.1mol / L.

[0053] In the step 4, the time of adding the alkaline solution to L1 is controlled within 5 to 7 minutes; the cream-like precipitate S3 mainly contains aluminum and iron hydroxides;

[0054] In the step 5, the L3 transparent solution is mainly a solution of sodium aluminate, which is because aluminum hydroxide dissolves under strong alkaline conditions;

[0055] In the step 5, the reddish brown precipitate S4 is mainly iron hydroxide that has not dissolved under excessive alkaline conditions. The purpose of step 5 is to remove iron;

[0056] In step 6, the flocculent F4 is filtered multiple times to obtain a colorless and transparent filtrate L4, and a silver nitrate solution is used to detect whether the filtrate L4 contains Cl - ; The concentration of silver nitrate solution is 1.0~1.05mol / L.

[0057] In the step six, the S5 is placed in an oven at a drying temperature of 120-121° C. and a drying time of 24-25 hours; in the step six, the calcination conditions of the precipitated S5 in the muffle furnace are: first calcining at 230-232° C. for 60-62 minutes, and then calcining at 830-832° C. for 360-362 minutes.

[0058] In the steps 2, 3, 5 and 6, the heating rate of the muffle furnace during calcination is 5.0-5.05° C. / min.

[0059] The specific content is: sodium carbonate is used as the alkaline ingredient, and the alumina product is obtained by changing the alkaline material ratio (1:1 and 1:1.5), the type of acid (hydrochloric acid, sulfuric acid and nitric acid) and the type of alkali (NaOH, NH3·H2O and NH4HCO3). The effect of the process is measured by the aluminum leaching rate and the content of alumina. Preferably, the fly ash and sodium carbonate mass ratio is 1:1.5, the roasting temperature is 830℃, the roasting time is 3h, leaching is carried out with 6.45mol / L HCl, and alkaline extraction is carried out with NaOH solution. The aluminum leaching rate of the fly ash finally obtained can reach 97.4%, and the content of the alumina product reaches 98.62%, reaching the national Al2O3 standard of level 3 and above (GB / T 24487-2022). This experiment optimizes the alkaline ratio and the experimental conditions of the acid-base combined method on the basis of the traditional acid-base combined method, and improves the acid extraction technology, aiming to increase the leaching rate and purity of alumina.

[0060] The purpose of the present invention can be achieved through the following technical solutions:

[0061] A method for extracting aluminum oxide from fly ash by an acid-base combined method comprises the following steps:

[0062] Step 1, pretreatment of fly ash raw materials, the steps are:

[0063] First, weigh a certain amount of fly ash S0, crush it with a crusher for 10 seconds, sieve it through 200 mesh or more, and weigh about 20.0-20.01g for later use;

[0064] Step 2, mixing and calcining fly ash and alkaline ingredients, comprising:

[0065] 1) Mix the fly ash SO and alkaline ingredients in a certain mass ratio and grind them evenly with a mortar;

[0066] 2) placing it in a muffle furnace for calcination at a certain temperature to obtain a yellow-green solid clinker, then crushing and mixing it evenly with a pulverizer, and sieving it to a size of more than 200 meshes to obtain a solid clinker S1;

[0067] Step three, acid leaching the activated clinker, comprising:

[0068] 1) Pour an acid solution of a certain concentration into a beaker, and under heating conditions of 80-81°C, slowly sprinkle S1 into the acid solution and stir rapidly until S1 is completely dissolved and gradually forms an orange flocculent F1. Continue heating and stirring for 4-5 hours to form a uniform colloid.

[0069] 2) The filtrate L1 obtained by multiple suction filtration of the flocculent F1 is a light yellow clear solution. At the same time, the white colloidal precipitate S2 is dried in an oven, taken out and ground into a size of more than 200 meshes using a mortar;

[0070] 3) calcining S2 in a muffle furnace and recovering the filtrate L1;

[0071] Step 4, performing an alkali extraction on the aluminum-containing filtrate, the steps comprising:

[0072] 1) Add a certain concentration of NaOH solution to L1 under heating and stirring conditions at 80-81°C to gradually obtain flocculent F2. Stop adding when the pH is adjusted to 6.5-7.0;

[0073] 2) The flocculent F2 is filtered for multiple times to obtain a light orange cream-like precipitate S3, and a primary alkali extraction filtrate L2 is obtained, which is colorless and transparent. When the pH is adjusted to 6.5-7.0, the dripping is stopped, and the flocculent F2 is filtered for multiple times to obtain a cream-like precipitate S3, and a primary alkali extraction filtrate L2 is obtained; this step requires the recovery of the precipitate S3;

[0074] Step 5, performing secondary alkaline extraction on the aluminum-containing precipitate, the steps comprising:

[0075] 1) Dissolve S3 with 200-300 mL of deionized water, then continue to drop NaOH solution into S3 under heating conditions of 80-81°C, gradually forming reddish-brown flocculent F3. Stop dropping when the pH is adjusted to 12.5-14.0, and continue heating and stirring for 30-40 min;

[0076] 2) The flocculent F3 is filtered for multiple times to obtain a secondary alkali extraction filtrate L3 which is colorless and transparent, and the filtrate L3 is recovered. Meanwhile, the obtained reddish brown precipitate S4 is dried in an oven and then calcined in a muffle furnace.

[0077] Step six, acid precipitation of the sodium aluminate solution, comprising:

[0078] 1) Slowly add an acid solution of a certain concentration to the clear L3 solution, stirring while adding, and gradually form a milky white flocculent F4. When the pH is adjusted to 9.5-10.0, stop adding and continue heating and stirring for 1.0-1.1h;

[0079] 2) The flocculent F4 is filtered several times to obtain a colorless and transparent filtrate L4, and a silver nitrate solution is used to detect whether the filtrate L4 contains Cl - ;

[0080] 3) The white precipitate S5 obtained by filtration is placed in an oven to dry, the dried S5 is ground and sieved to 60 mesh in a grinder, and then placed in a muffle furnace for calcination, and then ground again to obtain a white powder solid S6.

[0081] The fly ash raw material comes from the Guodian Shizuishan Power Plant. According to the X-ray diffraction fluorescence spectrum detection, the chemical components of the obtained fly ash are as follows: Al2O3 content is 28.40-28.401wt.%; SiO2 content is 44.86-44.861wt.%; Fe2O3 content is 7.38-7.381wt.%; CaO content is 7.11-7.111wt.%; SO3 content is 4.76-4.761wt.%; MgO content is 1.70-1.701wt.%; TiO2 content is 1.49-1.491wt.%; K2O content is 1.47-1.471wt.%; Na2O content is 1.05-1.051wt.%; C The content of l is 0.791~0.792wt.%; the content of P2O5 is 0.301~0.302wt.%; the content of ZrO2 is 0.137~0.138wt.%; the content of SrO is 0.130~0.131wt.%; the content of MnO is 0.092~0.093wt.%; the content of BaO is 0.055~0.056wt.%; the content of ZnO is 0.047~0.048wt.%; the content of V2O5 is 0.032~0.033wt.%; the content of PbO is 0.023~0.024wt.%; the content of CeO2 is 0.022~0.023wt.%; the content of other chemical components is 0.131wt.%. (Other components include one or more of Cr2O3, Y2O3, MoO3, CuO, NiO, As2O3, Ga2O3, Rb2O, Nd2O3, Co3O4, Nb2O, Bi2O3, Au, SeO2, GeO2, and Br).

[0082] Furthermore, the weight ratio of fly ash to alkaline ingredients in step one is 1:(1.0-1.5) (preferably in the range of 1:(1.05-1.45)).

[0083] Furthermore, the fly ash in step 2 is mixed with the alkaline ingredients and then placed in a muffle furnace for calcination at a temperature of 830 to 832° C. for a calcination time of 3.0 to 3.05 hours.

[0084] Furthermore, the "multiple filtrations" in steps three to six refer to filtration with deionized water at least twice, with the amount of water used each time being 950-1050 mL.

[0085] Furthermore, the preparation method of the 6.45mol / L HCl solution in step 3 is: take 537mL of 36-38% HCl solution and dilute it to 1000mL with deionized water. The preparation method of the 6.45mol / L HNO3 solution is: take 448mL of 65-68% HNO3 solution and dilute it to 1000mL with deionized water. The preparation method of the 6.45mol / L H2SO4 solution is: take 350mL of 95-98% H2SO4 solution and dilute it to 1000mL with deionized water.

[0086] Furthermore, the drying temperature of the colloidal precipitate S2 in step 3 in the oven is 60-61° C., and the drying time is 12-24 hours.

[0087] Furthermore, the heating rates of the muffle furnaces in steps 2 to 6 are

[0088] 5.0~5.05℃ / min.

[0089] Furthermore, the L1 filtrate in step 3 mainly contains Al 3+ , Fe 3+ Plasma.

[0090] Furthermore, the solid after calcining S2 in step three mainly contains substances such as silicic acid, sodium silicate and calcium silicate.

[0091] Furthermore, S2 and S5 in step three and step six are placed in a muffle furnace for constant temperature calcination at 650-652° C., and the calcination time is 6-6.05 h.

[0092] In the step 3, the acid solution is 6.45-6.47 mol / L HCl solution, HNO3 solution, H2SO4 solution, oxalic acid, or citric acid;

[0093] The preparation method of 6.45-6.47 mol / L HCl solution is as follows: take 537-538 mL of 36-38% HCl solution and dilute it to 1000 mL with deionized water;

[0094] The method for preparing the 6.45-6.47 mol / L HNO3 solution is as follows: take 448-449 mL of a 65-68% HNO3 solution and dilute it to 1000 mL with deionized water;

[0095] The preparation method of the 6.45-6.47 mol / L H2SO4 solution is as follows: take 350-351 mL of 95-98% H2SO4 solution and dilute it to 1000 mL with deionized water.

[0096] The preparation method of the 6.45-6.47 mol / L oxalic acid (molecular formula: H2C2O4) solution is as follows: take 813.16-815.68 g of oxalic acid dihydrate solid and dilute it to 1000 mL with deionized water.

[0097] The preparation method of the 6.45-6.47 mol / L citric acid (molecular formula: C6H8O7) solution is as follows: take 1354.76-1358.96 g of citric acid monohydrate solid and dilute it to 1000 mL with deionized water.

[0098] Furthermore,

[0099] In the step 4, the alkaline solution is one or more of the following four types;

[0100] The NaOH solution is prepared as follows: weigh 159.9-160.1 g of NaOH solid and dilute it to 500 mL with deionized water to prepare a NaOH solution with a concentration of 7.99-8.01 mol / L;

[0101] The KOH solution is prepared as follows: weigh 224.5-224.8 g of KOH solid and dilute it to 500 mL with deionized water to prepare a KOH solution with a concentration of 7.99-8.01 mol / L;

[0102] The preparation method of NH3·H2O solution is as follows: 374-375 mL of 25-28% ammonia water is measured and diluted to 500 mL with deionized water, and the preparation concentration is 9.99-10.1 mol / L;

[0103] The preparation method of NH4HCO3 solution is as follows: weigh 394.9-395.1 g of NH4HCO3 solid and dilute it to 500 mL with deionized water to prepare NH4HCO3 solution with a concentration of 9.99-10.1 mol / L.

[0104] The preparation method of (NH4)2CO3 solution is as follows: weigh 784.9-793.5g (NH4)2CO3 solid and dilute it to 500mL with deionized water to prepare (NH4)2CO3 solution with a concentration of 9.99-10.1mol / L.

[0105] In the step 4, the time of adding the alkaline solution to L1 is controlled within 5 to 7 minutes; the cream-like precipitate S3 mainly contains aluminum and iron hydroxides;

[0106] Furthermore, the L3 transparent solution in step 5 is mainly a sodium aluminate solution, which is formed by the dissolution of aluminum hydroxide under strong alkaline conditions.

[0107] Furthermore, the reddish-brown precipitate S4 in step 5 is mainly iron hydroxide that does not dissolve under excessive alkaline conditions.

[0108] Furthermore, in step 5, S4 is placed in an oven at a drying temperature of 80-81° C. and a drying time of 24-25 hours.

[0109] Furthermore, in step 6, S5 is placed in an oven at a drying temperature of 120-121° C. and a drying time of 24-25 hours.

[0110] Furthermore, the concentration of the silver nitrate solution in step six is ​​1.0-1.05 mol / L.

[0111] Furthermore, the calcination conditions of the precipitate S5 in the muffle furnace in the step six are: first calcining at 230-232°C for 60-62 min, and then calcining at 830-832°C for 360-362 min. In the steps two, three, five and six, the heating rate of the muffle furnace to calcination is 5.0-5.05°C / min.

[0112] By applying the technical solution of the present invention, fly ash is first activated by sodium carbonate to destroy the spherical solid solution structure of fly ash, so that the insoluble phase in fly ash is transformed into a soluble phase. Then, the activated fly ash is subjected to the "121" mode of "1 acid leaching-2 alkali extraction-1 acid precipitation" by the "acid-base combined method" to successively remove impurities and purify the fly ash, and finally the "leaching rate of aluminum in fly ash" and "product purity of alumina" are used as dual indicators to measure the test effect of the process. Among them, "the product purity of alumina" refers to the chemical composition analysis results of the alumina product (the mass percentage obtained from the X-ray fluorescence spectrometry analysis results, wt.%), and the grade of the alumina product extracted by the process is determined according to the four grades divided by the national standard for alumina (GB / T 24487-2022) (first-grade alumina: containing Al2O3 ≥ 98.6%; second-grade alumina: containing Al2O3 ≥ 98.4%; third-grade alumina: containing Al2O3 ≥ 98.3%; fourth-grade alumina: containing Al2O3 ≥ 98.2%). The fly ash aluminum extraction process of the present invention is simple and easy to operate. The aluminum leaching rate can reach more than 90%, and the purity of the alumina product is more than 98.2%, which meets the fourth grade and above of the national standard for alumina (GB / T 24487-2022).

[0113] The technology of extracting alumina from fly ash of the present invention can realize the high added value recycling of fly ash, a large solid waste of thermal power plants, on a large scale, reduce the pollution of fly ash to the environment, and help improve the level of resource utilization and high value utilization of solid waste in my country. More importantly, fly ash, as a potential aluminum resource, has the potential to replace traditional bauxite to alleviate the problem of bauxite resource shortage in my country. In summary, the process of extracting alumina using the acid-base combined method is one of the effective ways to achieve the harmlessness, reduction and resource utilization of fly ash, which is of great benefit to environmental protection and energy saving and efficiency improvement in the thermal power industry.

[0114] Beneficial effects of the present invention:

[0115] 1. Activate fly ash with sodium carbonate to destroy the spherical solid solution structure of fly ash and transform the insoluble phase in fly ash into soluble phase.

[0116] 2. The "121" innovative model of "1 acid leaching-2 alkali extraction-1 acid precipitation" greatly improves the efficiency of aluminum extraction from fly ash. Acid leaching under 80℃ heating and stirring conditions can dissolve hard and insoluble mineral phases such as mullite (Note: Mullite is a mineral composed of aluminum silicate, with a chemical formula of 3Al2O3·2SiO2 or 2Al2O3·SiO2, which belongs to aluminum silicate minerals) in activated fly ash to facilitate the dissolution of aluminum ions.

[0117] 3. The first of the two alkaline extractions is to form aluminum-iron precipitation by strictly controlling the pH value. The second alkaline extraction also requires strict control of the pH value to dissolve aluminum ions, thereby separating the aluminum-iron precipitate. This process requires precise pH control, and a pH meter and pH test paper are used for joint monitoring during the process.

[0118] 4. The aluminum ions in the solution are recovered and precipitated through the "acid extraction" method, which replaces the traditional CO2 carbonization process, saves time and cost, and is also conducive to reducing carbon emissions.

[0119] 5. The optimized acid-base combined method for extracting aluminum from fly ash of the present invention (process conditions: ash-base mass ratio = 1:1.5, hydrochloric acid solution is used as the acid extraction solution, and NaOH solution is used as the alkaline extraction solution, and the type of acid precipitation solution is consistent with the acid extraction solution) is superior to the aluminum extraction effect of using sulfuric acid, nitric acid as the acid extraction solution, and ammonia water and ammonium carbonate solution as the alkaline extraction solution.

[0120] 6. All embodiments of the present invention for extracting aluminum from fly ash by the acid-base combined method are superior to the two comparative examples of not using sodium carbonate activated calcination and using CO2 carbonization process in the acid extraction step.

[0121] 7. The acid-base combined method of the present invention is simple, low-cost and has excellent aluminum extraction effect. Through the study of aluminum extraction technology, the acid-base combined method of sodium carbonate activation combined with "121" has the best effect on aluminum extraction from fly ash. BRIEF DESCRIPTION OF THE DRAWINGS

[0122] The present invention will be further described below in conjunction with the accompanying drawings.

[0123] Figure 1 It is a process flow chart of extracting alumina from fly ash by the acid-base combined method, corresponding to Examples 1-10.

[0124] The acid solution may be 6.45 mol / L hydrochloric acid, sulfuric acid, nitric acid, oxalic acid or citric acid solution; the alkaline solution may be 8 mol / L NaOH solution or KOH solution, or 10 mol / L ammonia solution, ammonium bicarbonate or ammonium carbonate solution.

[0125] Figure 2 This is a scanning electron microscope (SEM) image of fly ash raw material, the left image is 5μm, and the right image is 1μm. The morphology of fly ash after being crushed by a grinding machine is basically spherical, with uneven ball diameters ranging from about 1 to 5μm, and a flaky structure on the surface.

[0126] Figure 3 This is the energy spectrum analysis (EDS) diagram of fly ash raw material. From the energy spectrum analysis of the original fly ash, it can be seen that the fly ash contains elements such as Al, Fe, Si, Mg and Ca, and the elements are evenly distributed to form a solid solution structure.

[0127] Figure 4 This is a scanning electron microscope (SEM) image of fly ash after activation with sodium carbonate (i.e., the end of step 2 in the task book), the left image is 2μm, and the right image is 200nm. After the fly ash is activated by sodium carbonate at high temperature, the spherical solid solution structure is destroyed, and aluminosilicates are precipitated on the surface, presenting a loose and porous structure, which corresponds to Example 1.

[0128] Figure 5 This is a scanning electron microscope (SEM) image of alumina extracted from fly ash (i.e., the end of step six in the task book), corresponding to Example 1, and a SEM comparison image of commercial γ-Al2O3 (Figure a) and alumina extracted according to Example 1 (Figure b).

[0129] Figure 6 This is a diagram of the solid phase evolution during the experimental process of extracting alumina from fly ash. From fly ash S0 to aluminum hydroxide precipitate S5, the morphology and color of the solid are changing.

[0130] Figure 7The X-ray diffraction (XRD) comparison diagram of fly ash raw material and extracted alumina Al2O3-1 (extracted according to Example 1). From the XRD diffraction peaks of fly ash and alumina products, fly ash has a complex multi-metallic mineral phase, and its specific crystal structure cannot be determined. The alumina product Al2O3-1 extracted from fly ash by the present invention has a specific cubic phase crystal form, and the diffraction peak is obvious, which is very consistent with the XRD standard card (γ-Al2O3 PDF#10-0425), and has 111, 220, 311, 222, 400, 511 and 440 crystal planes in the 2θ range of 15 to 80°.

[0131] Figure 8 The X-ray diffraction (XRD) comparison diagram of the extracted alumina products Al2O3-1 (extracted according to Example 1), Al2O3-2 (extracted according to Example 2) and commercial γ-Al2O3. The alumina products extracted from fly ash using the process of the present invention are basically consistent with the crystal form of commercial alumina. Figure 8 It also shows that the use of different alkali ratios has little effect on the purity of the final extracted alumina product. DETAILED DESCRIPTION

[0132] It should be noted that, in the absence of conflict, the embodiments, features in the embodiments, and comparative examples in the present application may be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with examples.

[0133] As described in the background technology of the present invention, the existing technology has the problems of large carbon emission and environmental pollution in the CO2 carbonization process for extracting aluminum oxide from fly ash, and the process parameters of the acid-base combined method are not precise, the process is difficult to control, and the production cost is high. The present invention discloses a process for extracting aluminum oxide from fly ash by the acid-base combined method. The method mainly includes key steps such as "acid leaching", "primary alkali extraction", "secondary alkali extraction" and "acid precipitation". First, the fly ash raw material is crushed by a crusher, mixed with alkaline ingredients in a certain proportion and calcined to obtain an activated block solid, which is then crushed and acid-leached, fully stirred until dissolved, and filtered multiple times to recover a clear acid leaching solution. Then, the alkaline solution is added dropwise to the above-mentioned acid leaching solution, and the pH is adjusted to 6.5-7.0. At this time, the iron ions and aluminum ions completely form a precipitate, and the precipitate is recovered after multiple filtrations. The above-mentioned precipitate is dissolved with an alkaline solution, and the pH is adjusted to 12.5-14.0. After multiple filtrations, a clear filtrate is recovered. A certain amount of acid solution is added to the above clear filtrate to form a white emulsion, which is filtered several times to obtain a white aluminum hydroxide precipitate. The above aluminum hydroxide precipitate is dried and calcined at high temperature to form an aluminum oxide product.

[0134] Embodiment 1:

[0135] A method for extracting aluminum oxide from fly ash by an acid-base combined method comprises the following steps:

[0136] Step 1: First, the fly ash raw material is crushed by a pulverizer, passed through a 200-mesh sieve, and the fly ash S0 component passing through the sieve is collected and weighed 20.0 g for later use;

[0137] Step 2: Mix the fly ash S0 and anhydrous sodium carbonate in a mass ratio of 1:1, grind them evenly with a mortar, and calcine them in a muffle furnace at 830° C. for 3 hours to obtain a yellow-green solid clinker, then crush and mix them evenly with a grinder, pass through a 200-mesh sieve, collect the components passing through the sieve, and obtain solid clinker S1;

[0138] Step 3: Pour 400 mL of 6.45 mol / L hydrochloric acid solution into a beaker. Under heating conditions of 80°C, slowly sprinkle the solid clinker S1 into the hydrochloric acid solution and stir rapidly until S1 is completely dissolved and gradually forms orange floccules. Continue heating and stirring for 4 hours to form a uniform colloid F1. Wash the colloid F1 with deionized water three times, each washing volume is 1000 mL. The filtrate L1 obtained is a light yellow clear solution, and the filtrate L1 is recovered. At the same time, the white colloidal precipitate S2 is dried in an oven at 60°C overnight (12 hours), taken out and ground with a mortar, passed through a 200-mesh sieve, collected the components passing through the sieve, and S2 was calcined at 650°C in a muffle furnace for 6 hours; the L1 filtrate mainly contains Al 3+ , Fe 3+ The solid after calcination of S2 mainly contains silicic acid, sodium silicate and calcium silicate, and the purpose of step three is to remove calcium and silicon.

[0139] Step 4: add 8.0 mol / L NaOH solution to L1 under heating and stirring at 80°C to gradually obtain flocculent F2. Stop adding when the pH is adjusted to 6.6, and then wash the solution containing flocculent F2 with deionized water three times, each washing volume is 1000 mL, to obtain a light orange cream precipitate S3, and obtain a primary alkali extraction filtrate L2 in a colorless and transparent state, and recover the precipitate S3;

[0140] Step 5: Dissolve the precipitate S3 with 200 mL of deionized water, then continue to drip 8.0 mol / L NaOH solution into the precipitate S3 under heating conditions at 80°C, gradually forming a reddish brown flocculent F3, stop dripping when the pH is adjusted to 12.5-14.0 (here 13.0), continue heating and stirring for 30 minutes, then wash the flocculent F3 with deionized water three times, each washing amount is 1000 mL, obtain a secondary alkaline extract L3 in a colorless and transparent state, and recover the filtrate L3. At the same time, the obtained reddish brown precipitate S4 is dried in an oven at 80°C for 24 hours, and then placed in a muffle furnace at 650°C for calcination for 6 hours.

[0141] Step 6: Slowly add 6.45 mol / L hydrochloric acid solution to the clarified filtrate L3, stirring while adding, gradually forming a milky white flocculent F4. When the pH is adjusted to 9.5-10.0 (here 9.8), stop adding, and continue heating and stirring for 1.0-1.1 h (here 1.1 h). The flocculent F4 is filtered 6 times, washed with deionized water three times and washed with ethanol three times, each washing (water or ethanol) is 1000 mL, and finally the washing liquid L4 is colorless and transparent, and the filtrate L4 is tested for Cl with a 1.0 mol / L silver nitrate solution. - (Confirm that there is no Cl - ). At the same time, the white precipitate S5 obtained by filtration was placed in an oven at 120°C and dried for 24 hours. The dried precipitate S5 was ground in a grinder and passed through a 60-mesh sieve. The components passing through the sieve were collected and then placed in a muffle furnace and calcined at 230°C for 1 hour. The temperature was then raised to 830°C and calcined for 6 hours. After cooling to room temperature, the white powder solid S6 was ground again and was the obtained alumina product, named Al2O3-1.

[0142] Embodiment 2:

[0143] Specifically, the difference from Example 1 is that the fly ash S0 described in step 2 of Example 1 is mixed with anhydrous sodium carbonate in a mass ratio of 1:1.5, and the other steps remain unchanged (the rest of the process and conditions are the same as Example 1), and finally a white powder solid S6 is obtained, named Al2O3-2.

[0144] Embodiment 3:

[0145] Specifically, the difference from Example 1 is that the hydrochloric acid solution described in step three and step six in Example 1 is replaced with a 6.45 mol / L nitric acid solution, and the other steps remain unchanged (the rest of the process and conditions are the same as Example 1), and finally a white powder solid S6 is obtained, named Al2O3-3.

[0146] Embodiment 4:

[0147] Specifically, the difference from Example 1 is that the hydrochloric acid solution described in step three and step six in Example 1 is replaced with a 6.45 mol / L sulfuric acid solution, and the other steps remain unchanged (the rest of the process and conditions are the same as Example 1), and finally a white powder solid S6 is obtained, named Al2O3-4.

[0148] Embodiment 5:

[0149] Specifically, the difference from Example 1 is that the hydrochloric acid solution described in step three and step six in Example 1 is replaced with a 6.45 mol / L oxalic acid solution, and the other steps remain unchanged (the rest of the process and conditions are the same as Example 1), and finally a white powder solid S6 is obtained, named Al2O3-5.

[0150] Embodiment 6:

[0151] Specifically, the difference from Example 1 is that the hydrochloric acid solution described in step three and step six in Example 1 is replaced with a 6.45 mol / L citric acid solution, and the other steps remain unchanged (the rest of the process and conditions are the same as Example 1), and finally a white powder solid S6 is obtained, named Al2O3-6.

[0152] Embodiment 7:

[0153] Specifically, the difference from Example 1 is that the sodium hydroxide solution described in step 4 and step 5 in Example 1 is replaced with 8 mol / L potassium hydroxide solution, and the other steps remain unchanged (the rest of the process and conditions are the same as Example 1), and finally a white powder solid S6 is obtained, named Al2O3-7.

[0154] Embodiment 8:

[0155] Specifically, the difference from Example 1 is that the sodium hydroxide solution described in step 4 and step 5 in Example 1 is replaced with a 10 mol / L ammonia solution, and the other steps remain unchanged (the rest of the process and conditions are the same as Example 1), and finally a white powder solid S6 is obtained, named Al2O3-8.

[0156] Embodiment 9:

[0157] Specifically, the difference from Example 1 is that the sodium hydroxide solution described in step 4 and step 5 in Example 1 is replaced with a 10 mol / L ammonium bicarbonate solution, and the other steps remain unchanged (the rest of the process and conditions are the same as Example 1), and finally a white powder solid S6 is obtained, named Al2O3-9.

[0158] Embodiment 10:

[0159] Specifically, the difference from Example 1 is that the sodium hydroxide solution described in step 4 and step 5 in Example 1 is replaced with a 10 mol / L ammonium carbonate solution, and the other steps remain unchanged (the rest of the process and conditions are the same as in Example 1), and finally a white powder solid S6 is obtained, named Al2O3-10. Comparative Example 1:

[0160] Alumina was extracted from fly ash using the same steps as step 1, step 3 to step 6 in Example 1, but the difference from Example 1 was that the step of activating fly ash with sodium carbonate was missing (no step 2, fly ash S0 was used instead of solid clinker S1 for step 3, and the rest of the process and conditions were the same as Example 1). Finally, a white powder was obtained, named Al2O3-A.

[0161] Comparative Example 2:

[0162] Step 1 in Example 1 was discarded, and step 6 was replaced by introducing CO2 gas into the sodium aluminate solution for carbonization until the pH value of the solution reached 8.0 and then the aeration was stopped to obtain aluminum hydroxide precipitate. The precipitate was repeatedly filtered and washed (the rest of the process and conditions were the same as in Example 1), and the filtrate was tested with silver nitrate solution to see if it contained Cl - The precipitate was dried and ground to pass through a 60-mesh sieve, and the components passing through the sieve were collected and then placed in a muffle furnace and calcined at 230°C for 1 hour, and then continued to be heated to 830°C and calcined for 6 hours. After cooling, it was ground again to obtain a white powder solid, named Al2O3-B.

[0163] Comparative Example 3:

[0164] Step 1 in Example 1 was discarded, and the hydrochloric acid solution described in Steps 3 and 6 was replaced with a 6.45 mol / L sulfuric acid solution. In addition, Step 6 in Example 1 was replaced by introducing CO2 gas into the sodium aluminate solution for carbonization until the pH value of the solution reached 8.0 and the aeration was stopped to obtain aluminum hydroxide precipitate, which was repeatedly filtered and washed (the rest of the process and conditions were the same as in Example 1), and the filtrate was tested with a silver nitrate solution to see if it contained Cl - The precipitate was dried and ground to pass through a 60-mesh sieve, and the components passing through the sieve were collected and then placed in a muffle furnace and calcined at 230°C for 1 hour, and then continued to be heated to 830°C and calcined for 6 hours. After cooling, it was ground again to obtain a white powder solid, named Al2O3-C.

[0165] Comparative Example 4:

[0166] Step 1 in Example 1 was discarded, and the sodium hydroxide solution described in Steps 4 and 5 was replaced with a 10 mol / L ammonium bicarbonate solution. In addition, Step 6 in Example 1 was replaced by introducing CO2 gas into the sodium aluminate solution for carbonization until the pH value of the solution reached 8.0 and the aeration was stopped to obtain aluminum hydroxide precipitate, which was repeatedly filtered and washed (the rest of the process and conditions were the same as in Example 1), and the filtrate was tested with a silver nitrate solution to see if it contained Cl - The precipitate was dried and ground to pass through a 60-mesh sieve, and the components passing through the sieve were collected and then placed in a muffle furnace and calcined at 230°C for 1 hour, and then continued to be heated to 830°C and calcined for 6 hours. After cooling, it was ground again to obtain a white powder solid, named Al2O3-D.

[0167] Comparative Example 5:

[0168] Step 1 in Example 1 was discarded, and the sodium hydroxide solution described in Steps 4 and 5 was replaced with a 10 mol / L ammonia solution. In addition, Step 6 in Example 1 was replaced by introducing CO2 gas into the sodium aluminate solution for carbonization until the pH value of the solution reached 8.0 and the aeration was stopped to obtain aluminum hydroxide precipitate, which was repeatedly filtered and washed (the rest of the process and conditions were the same as in Example 1), and the filtrate was tested with a silver nitrate solution to see if it contained Cl - The precipitate was dried and ground to pass through a 60-mesh sieve, and the components passing through the sieve were collected and then placed in a muffle furnace and calcined at 230°C for 1 hour, and then continued to be heated to 830°C and calcined for 6 hours. After cooling, it was ground again to obtain a white powder solid, named Al2O3-E.

[0169] Compare Examples 1-10 with Comparative Examples 1-5.

[0170] The calculation formula of alumina leaching rate (T) is:

[0171]

[0172] The aluminum content of the aluminum oxide of the present invention can be determined based on data from X-ray fluorescence spectrometry (XRF).

[0173] Please refer to the national standard (GB / T 24487-2022) for details.

[0174] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0175] The oxide composition table of fly ash is shown in Table 1 (data from X-ray fluorescence spectroscopy (XRF)), which serves as the initial data of the oxides contained in the fly ash before aluminum extraction.

[0176] Table 2 is the test scheme of six embodiments of the present invention and two comparative examples.

[0177] Table 3 is a comparison chart of the leaching rate (T) of aluminum in fly ash and the product purity of aluminum oxide in six embodiments and two comparative examples (data from X-ray fluorescence spectroscopy (XRF)). According to the aluminum oxide analysis and calculation method specified in the national standard GB / T24487-2022, the grade of the aluminum oxide products prepared from fly ash as raw material in the present invention is grade three or above. Compared with the comparative examples, the aluminum extraction process of the present invention has a great advantage in product effect.

[0178] Table 1 Chemical composition of fly ash

[0179]

[0180] Table 2 Experimental scheme of six embodiments and two comparative examples

[0181]

[0182]

[0183] Table 3 Alumina product purity, aluminum leaching rate in fly ash and product grade

[0184]

[0185] The purity of the alumina product obtained by the method of Example 1 reaches 98.31%, and the leaching rate T of aluminum in fly ash reaches 93.5%. According to the national standard GB / T 24487-2022 for alumina, the alumina product belongs to grade three.

[0186] By the method of Example 2, the purity of the alumina product reaches 98.62%, and the leaching rate T of aluminum in fly ash reaches 95.4%. According to the national standard GB / T 24487-2022 for alumina, the alumina product belongs to Grade 1.

[0187] By the method of Example 3, the purity of the alumina product reaches 98.57%, and the leaching rate T of aluminum in fly ash reaches 94.2%. According to the national standard GB / T 24487-2022 for alumina, the alumina product belongs to Grade II.

[0188] By the method of Example 4, the purity of the alumina product reaches 98.44%, and the leaching rate T of aluminum in fly ash reaches 93.6%. According to the national standard GB / T 24487-2022 for alumina, the alumina product belongs to Grade II.

[0189] By the method of Example 5, the purity of the alumina product reaches 98.27%, and the leaching rate T of aluminum in fly ash reaches 93.3%. According to the national standard GB / T 24487-2022 for alumina, the alumina product belongs to grade IV.

[0190] By the method of Example 6, the purity of the alumina product reaches 98.22%, and the leaching rate T of aluminum in fly ash reaches 92.7%. According to the national standard GB / T 24487-2022 for alumina, the alumina product belongs to grade IV.

[0191] By the method of Example 7, the purity of the alumina product reaches 98.20%, and the leaching rate T of aluminum in fly ash reaches 91.1%. According to the national standard GB / T 24487-2022 for alumina, the alumina product belongs to grade IV.

[0192] By the method of Example 8, the purity of the alumina product reaches 98.29%, and the leaching rate T of aluminum in fly ash reaches 92.6%. According to the national standard GB / T 24487-2022 for alumina, the alumina product belongs to grade IV.

[0193] By the method of Example 9, the purity of the alumina product reaches 98.28%, and the leaching rate T of aluminum in fly ash reaches 93.2%. According to the national standard GB / T 24487-2022 for alumina, the alumina product belongs to grade IV.

[0194] By the method of Example 10, the purity of the alumina product reaches 98.27%, and the leaching rate T of aluminum in fly ash reaches 92.4%. According to the national standard GB / T 24487-2022 for alumina, the alumina product belongs to grade IV.

[0195] By using the method of comparative example 1, the product purity of alumina reaches 78.23%, and the leaching rate T of aluminum in fly ash reaches 48.1%. According to the national standard GB / T 24487-2022 for alumina, the alumina product is non-grade.

[0196] By using the method of Comparative Example 2, the purity of alumina products reaches 83.29%, and the leaching rate T of aluminum in fly ash reaches 57.6%. According to the national standard GB / T 24487-2022 for alumina, the alumina products are non-grade.

[0197] By using the method of comparative example 3, the purity of alumina products reaches 80.34%, and the leaching rate T of aluminum in fly ash reaches 62.1%. According to the national standard GB / T 24487-2022 for alumina, the alumina products are non-grade.

[0198] By using the method of Comparative Example 4, the purity of alumina products reaches 81.54%, and the leaching rate T of aluminum in fly ash reaches 50.4%. According to the national standard GB / T 24487-2022 for alumina, the alumina products are non-grade.

[0199] By using the method of comparative example 5, the purity of alumina products reaches 80.86%, and the leaching rate T of aluminum in fly ash reaches 60.3%. According to the national standard GB / T 24487-2022 for alumina, the alumina products are non-grade.

[0200] The invention discloses a method for extracting aluminum oxide from fly ash by an acid-base combined method. First, fly ash raw materials are crushed by a crusher, mixed with alkaline ingredients in a certain proportion and calcined to obtain an activated block solid, which is then crushed and acid-leached, fully stirred until dissolved, and filtered multiple times to recover a clarified acid leaching liquid. Then, an alkaline solution is dripped into the acid leaching liquid, and the pH is adjusted to 6.5-7.0. At this time, iron ions and aluminum ions completely form a precipitate, and the precipitate is recovered after multiple filtrations. The precipitate is dissolved by an alkaline solution, and the pH is adjusted to 12.5-14.0. The clarified filtrate is recovered after multiple filtrations. A certain amount of acid solution is dripped into the clarified filtrate to form a white emulsion, and white aluminum hydroxide precipitate is recovered after multiple filtrations. The aluminum hydroxide precipitate is dried and then calcined at high temperature to form an aluminum oxide product.

[0201] The fly ash aluminum extraction process of the present invention has a simple process and is easy to operate. It can realize the high-value-added recycling of fly ash, a large solid waste of thermal power plants, and reduce the pollution of fly ash to the environment, which is conducive to improving the level of solid waste resource utilization and high-value utilization in my country. More importantly, fly ash, as a potential aluminum resource, has the advantage of being able to replace traditional bauxite, in order to alleviate the problem of bauxite resource shortage in my country. In summary, the use of an improved acid-base combined method to extract alumina is one of the effective ways to achieve the harmlessness, reduction and resource utilization of fly ash, which is of great benefit to the environmental pollution control and energy saving and efficiency improvement of the thermal power industry.

Claims

1. A method for extracting aluminum oxide from fly ash by an acid-base combined method, characterized in that: The following steps are involved: Step 1, crush the fly ash raw material and sieve it through a sieve with a mesh size of 200 or more, collect the fly ash S0 component that passes through the sieve, weigh 20.0 to 20.01 g for later use; Step 2, the fly ash S0 is mixed with the alkaline ingredients, ground evenly, calcined to obtain clinker, and then crushed, passed through a sieve with mesh size of 200 or more, and the components passing through the sieve are collected to obtain activated powder clinker S1; Step 3: pour the acid solution into a container, add the powdered clinker S1 into the acid solution under heating conditions of 80-81° C. and stir until S1 is completely dissolved, and then gradually form floccules, continue heating and stirring for 4-5 hours until a colloid F1 with a uniform texture is formed, and the filtrate L1 obtained by multiple filtration of the colloid F1 is a clear solution; this step requires the recovery of the filtrate L1; Step 4: add the alkaline solution to L1 under heating and stirring conditions at 80-81°C to gradually obtain floccules F2, stop adding when the pH is adjusted to 6.5-7.0, filter the floccules F2 multiple times to obtain a cream-like precipitate S3, and obtain a primary alkali extraction filtrate L2; this step requires the recovery of the precipitate S3; Step 5, first dissolving the precipitate S3 in 200-300 mL of water, then continuing to drop an alkali solution into S3 under heating conditions of 80-81° C. to form a flocculant F3, stopping the dropwise addition when the pH is adjusted to 12.5-14.0, continuing heating and stirring for 30-40 min, and then filtering the flocculant F3 multiple times to obtain a secondary alkali extraction filtrate L3, and recovering the filtrate L3; Step six, add the acid solution described in step two to the filtrate L3 while stirring, gradually forming floccules F4, stop adding when the pH is adjusted to 9.5-10.0, continue heating and stirring for 1.0-1.1h; filter the floccules F4 several times, and place the white precipitate S5 obtained by filtration in an oven to dry, then crush it through a sieve with a mesh size of 60 or above, collect the components passing through the sieve, and then place it in a muffle furnace for calcination to obtain a white powder solid S6.

2. The method according to claim 1, characterized in that The fly ash raw material comes from the Guodian Shizuishan Power Plant. According to the X-ray diffraction fluorescence spectrum detection, the chemical components of the obtained fly ash are as follows: Al2O3 content is 28.40-28.401wt.%; SiO2 content is 44.86-44.861wt.%; Fe2O3 content is 7.38-7.381wt.%; CaO content is 7.11-7.111wt.%; SO3 content is 4.76-4.761wt.%; MgO content is 1.70-1.701wt.%; TiO2 content is 1.49-1.491wt.%; K2O content is 1.47-1.471wt.%; Na2O content is 1.05-1.051wt.%; C The content of l is 0.791~0.792wt.%; the content of P2O5 is 0.301~0.302wt.%; the content of ZrO2 is 0.137~0.138wt.%; the content of SrO is 0.130~0.131wt.%; the content of MnO is 0.092~0.093wt.%; the content of BaO is 0.055~0.056wt.%; the content of ZnO is 0.047~0.048wt.%; the content of V2O5 is 0.032~0.033wt.%; the content of PbO is 0.023~0.024wt.%; the content of CeO2 is 0.022~0.023wt.%; the content of other chemical components is 0.131wt.%. (Other components include one or more of Cr2O3, Y2O3, MoO3, CuO, NiO, As2O3, Ga2O3, Rb2O, Nd2O3, Co3O4, Nb2O, Bi2O3, Au, SeO2, GeO2, and Br).

3. The method according to claim 1, characterized in that: In the step 2, the weight ratio of fly ash to alkaline ingredients is 1:(1.0-1.5) (preferably in the range of 1:(1.05-1.45)); The alkaline ingredients are one or more of sodium carbonate or sodium bicarbonate; In the step 2, the fly ash is mixed with the alkaline ingredients and then placed in a muffle furnace for calcination at a temperature of 830 to 832° C. for a calcination time of 3.0 to 3.05 hours.

4. The method according to claim 1 or 3, characterized in that: In the steps 3 to 5, the "multiple filtrations" refer to filtration with water at least twice, with the amount of water used each time being 950-1050 mL; In step six, the "multiple filtrations" refer to filtering with water and ethanol at least twice in sequence, with the amount of water or ethanol used each time being 950-1050 mL.

5. The method according to claim 1, characterized in that In the step 3, the acid solution is 6.45-6.47 mol / L HCl solution, HNO3 solution, H2SO4 solution, oxalic acid, or citric acid; The preparation method of 6.45-6.47 mol / L HCl solution is as follows: take 537-538 mL of 36-38% HCl solution and dilute it to 1000 mL with deionized water; The method for preparing the 6.45-6.47 mol / L HNO3 solution is as follows: take 448-449 mL of a 65-68% HNO3 solution and dilute it to 1000 mL with deionized water; The preparation method of the 6.45-6.47 mol / L H2SO4 solution is as follows: take 350-351 mL of 95-98% H2SO4 solution and dilute it to 1000 mL with deionized water. The preparation method of the 6.45-6.47 mol / L oxalic acid (molecular formula: H2C2O4) solution is as follows: take 813.16-815.68 g of oxalic acid dihydrate solid and dilute it to 1000 mL with deionized water. The preparation method of the 6.45-6.47 mol / L citric acid (molecular formula: C6H8O7) solution is as follows: take 1354.76-1358.96 g of citric acid monohydrate solid and dilute it to 1000 mL with deionized water.

6. The method according to claim 1, characterized in that In the step 3, the white colloidal precipitate S2 obtained by suction filtration needs to be dried, taken out and crushed, and then passed through a sieve with a mesh size of 200 or more, and the components passing through the sieve are collected and then placed in a muffle furnace for calcination; The drying temperature of the colloidal precipitate S2 is 60-61° C., and the drying time is 12-24 hours; In the step 3, the S4 is placed in a muffle furnace and calcined at a constant temperature of 650-652° C. for 6.0-6.05 h; In the step 5, at the same time, the reddish brown precipitate S4 is obtained by suction filtration, and after drying, it is placed in a muffle furnace for calcination; In the step 5, the S4 is placed in an oven at a drying temperature of 80 to 81° C. for 24 to 25 hours; In the step 5, the S4 is placed in a muffle furnace and calcined at a constant temperature of 650-652° C. for 6.0-6.05 h.

7. The method according to claim 1, characterized in that In the step 4, the alkaline solution is one or more of the following four types; The NaOH solution is prepared as follows: weigh 159.9-160.1 g of NaOH solid and dilute it to 500 mL with deionized water to prepare a NaOH solution with a concentration of 7.99-8.01 mol / L; The KOH solution is prepared as follows: weigh 224.5-224.8 g of KOH solid and dilute it to 500 mL with deionized water to prepare a KOH solution with a concentration of 7.99-8.01 mol / L; The preparation method of NH3·H2O solution is as follows: 374-375 mL of 25-28% ammonia water is measured and diluted to 500 mL with deionized water, and the preparation concentration is 9.99-10.1 mol / L; The preparation method of NH4HCO3 solution is as follows: weigh 394.9-395.1 g of NH4HCO3 solid and dilute it to 500 mL with deionized water to prepare NH4HCO3 solution with a concentration of 9.99-10.1 mol / L. The preparation method of (NH4)2CO3 solution is as follows: weigh 784.9-793.5g (NH4)2CO3 solid and dilute it to 500mL with deionized water to prepare (NH4)2CO3 solution with a concentration of 9.99-10.1mol / L.

8. The method according to claim 1, characterized in that In the step 4, the time of adding the alkaline solution to L1 is controlled within 5 to 7 minutes; the cream-like precipitate S3 mainly contains aluminum and iron hydroxides; In the step 5, the L3 transparent solution is mainly a solution of sodium aluminate, which is because aluminum hydroxide dissolves under strong alkaline conditions; In the step 5, the reddish brown precipitate S4 is mainly iron hydroxide that has not dissolved under excessive alkaline conditions. The purpose of step 5 is to remove iron; In step 6, the flocculent F4 is filtered multiple times to obtain a colorless and transparent filtrate L4, and a silver nitrate solution is used to detect whether the filtrate L4 contains Cl - ; The concentration of silver nitrate solution is 1.0~1.05mol / L.

9. The method according to claim 1, characterized in that: In the step six, the S5 is placed in an oven at a drying temperature of 120-121° C. and a drying time of 24-25 hours; in the step six, the calcination conditions of the precipitated S5 in the muffle furnace are: first calcining at 230-232° C. for 60-62 minutes, and then calcining at 830-832° C. for 360-362 minutes.

10. The method according to claim 1, 3, 6 or 9, characterized in that In the steps 2, 3, 5 and 6, the heating rate of the muffle furnace during calcination is 5.0-5.05° C. / min.