Method for preparing alpha-Al2O3 based on meta-aluminate

By calcining aluminates in a chlorine-containing organic atmosphere, highly crystalline α-Al2O3 was prepared at low temperature, solving the problems of high energy consumption and complex preparation in high-temperature calcination, and obtaining α-Al2O3 products with uniform particle size.

CN118954558AInactive Publication Date: 2024-11-15SHENZHEN BAINA CORE MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411185654.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The preparation of α-Al2O3 in the existing technology requires high-temperature calcination (usually above 1200℃), which consumes a lot of energy, and the preparation process is complicated, with large grain size and difficult morphology control.

Method used

Using aluminates as raw materials, calcination is carried out in a chlorine-containing organic atmosphere. The metal cations are separated by the volatilization of chloride salts. Then, impurities are removed by washing to obtain highly crystalline α-Al2O3.

Benefits of technology

Pure-phase α-Al2O3 was prepared at a relatively low temperature (650–1000℃), which simplified the preparation process, saved energy, and yielded α-Al2O3 products with uniform particle size and good dispersibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954558A_ABST
    Figure CN118954558A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing alpha-Al2O3 based on meta-aluminate, and belongs to the technical field of metal oxide material preparation. The method comprises the following steps of: calcining meta-aluminate serving as a raw material in a protective atmosphere containing chlorine-containing organic matters, and washing to obtain alpha-Al2O3; according to the technical scheme, alpha-Al2O3 can be obtained at the low calcination temperature (650-1000 DEG C), pure-phase alpha-Al2O3 can be obtained at the calcination temperature of 770-1000 DEG C, the calcination temperature of traditional alpha-Al2O3 preparation is greatly reduced, the preparation method is simple and convenient, only one-time calcination, one-time acid pickling and two-time washing are needed, the manufacturing time and cost can be saved, the obtained alpha-Al2O3 particles are uniform in size, and the preparation method is suitable for industrial production. The dispersity is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal oxide material preparation, and specifically relates to a method for preparing α-Al2O3 based on metaaluminate. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] α-Al2O3 has the characteristics of high melting point, high hardness, good wear resistance, high mechanical strength, good electrical insulation, strong corrosion resistance, etc. It is an ideal raw material for manufacturing ceramics, abrasives, molds, refractory materials, etc. It has a wide range of applications in many fields such as machinery, power electronics, chemical engineering, medicine, energy, and military industry. At present, the preparation of α-Al2O3 is mainly made by high-temperature calcination of aluminum-containing precursors, which usually requires complex processing and extremely high calcination temperatures (usually higher than 1200°C). In addition, the α-Al2O3 obtained after high-temperature calcination usually has a larger grain size, is easy to adhere to form a "worm-like" cross-linked structure, and has a difficult-to-control morphology.

[0004] Patent CN117342590A discloses a method of using pseudo-boehmite as raw material, setting thirteen different temperature zones at 100-960°C for the first calcination to obtain an intermediate, sand grinding, drying and crushing to obtain a powder, and then calcining the powder for the second time at 1050-1300°C to obtain α-Al2O3. Patent CN116135787A first mixes aluminum powder (a mixture of aluminum oxide and aluminum hydroxide) and boride in a stirring device and cools them, then pours the treated powder into a mixed solution of expired fruit juice and super acid, stirs them thoroughly, dehydrates to obtain a calcined material, and finally calcines at 1885-2195°C for 3-4h to obtain α-Al2O3. Patent CN117417180A mixes γ-alumina, oxalic acid solution and resin coating liquid to obtain a mixture, calcines at 800°C for 30min after drying, then calcines at 1100°C for 3h, and ball mills to obtain α-Al2O3. The above-mentioned patents all adopt high-temperature calcination to prepare alumina, and the temperature range is 1050~2195 ℃, and the required raw materials are of many types, the preparation process is cumbersome, and the obtained α-Al2O3 grain size is large.

[0005] At present, the industry generally believes that the preparation of α-Al2O3 needs to reach above 1200°C to transform into the α phase, which consumes huge energy. There are few studies on how to prepare α-Al2O3 at low temperatures. Patent CN102502739A obtains α-Al2O3 from industrial sodium aluminate through hydrochloric acid leaching, drying and dehydration, vacuum sublimation purification, ammonia immersion crystallization, and calcination at 800-1200°C. This patent prepares α-Al2O3 through liquid phase reaction. Although the calcination temperature is below 1200°C, the types of raw materials required are still large, the preparation process is still cumbersome, and the resulting α-Al2O3 grain size is large and the morphology is difficult to control. Summary of the invention

[0006] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing α-Al2O3 based on aluminate. Based on the similarity between the aluminate precursor and the α-Al2O3 crystal structure, the present invention prepares α-Al2O3 with high crystallinity at a relatively low temperature (650-1000°C) by calcining in a chlorine-containing organic atmosphere.

[0007] In order to achieve the above object, the technical solution of the present invention is:

[0008] The first aspect of the present invention provides a method for preparing α-Al2O3 based on metaaluminate, comprising the following steps:

[0009] Using aluminate as raw material, calcination is carried out in a chlorine-containing organic atmosphere to obtain an initial product, which is then washed to obtain α-Al2O3.

[0010] In some embodiments of the present invention, the aluminate includes lithium aluminate, sodium aluminate, potassium aluminate, calcium aluminate or magnesium aluminate.

[0011] In some embodiments of the present invention, the aluminate is lithium aluminate, sodium aluminate or potassium aluminate.

[0012] In some embodiments of the present invention, the chlorine-containing organic compound includes methane chloride, ethane chloride or propane chloride.

[0013] In some embodiments of the present invention, the chlorine-containing organic compound is a methane chloride, specifically monochloromethane, dichloromethane, trichloromethane or tetrachloromethane.

[0014] In some embodiments of the present invention, the chlorine-containing organic atmosphere comprises a protective gas and a chlorine-containing organic, and the protective gas is nitrogen or argon.

[0015] In some embodiments of the present invention, the temperature of the chlorine-containing organic matter is 1-50° C.; the flow rate of the chlorine-containing organic matter atmosphere is 10-300 sccm.

[0016] It should be noted that the chlorine-containing organic matter is blown into the reaction device using protective gas as carrier gas. In the calcination process, the chlorine-containing organic matter is excessive. Preferably, the molar ratio of chlorine atoms in the chlorine-containing organic matter to metal cations in the aluminate is 1:1 to 5:1.

[0017] In some embodiments of the present invention, the calcination temperature is 650-1000° C., the calcination time is 0.5-10 h, and the heating rate is 1-20° C. / min.

[0018] In some embodiments of the present invention, when sodium aluminate is used as a raw material, the calcination temperature is 800-1000° C., and α-Al 2 O 3 is obtained after calcination and washing.

[0019] In some embodiments of the present invention, when potassium aluminate is used as a raw material, the calcination temperature is 770-1000° C., and α-Al 2 O 3 is obtained after calcination and washing.

[0020] In some embodiments of the present invention, when lithium aluminate is used as a raw material, the calcination temperature is 700-1000° C., and α-Al 2 O 3 is obtained after calcination and washing.

[0021] In some embodiments of the present invention, the washing includes water washing and acid washing, and the initial product is sequentially washed with water, acid washed, and water washed, and then dried to obtain α-Al2O3.

[0022] In some embodiments of the present invention, the acid washing process is: mixing acid and water in a volume ratio of 1:1 to 1:7, adding the initial product after water washing, and heating and washing.

[0023] In some embodiments of the present invention, the acid is at least one of nitric acid, sulfuric acid, hydrochloric acid or phosphoric acid.

[0024] In some embodiments of the present invention, the heated washing is washing at 40-220° C. for 0.5-8 h.

[0025] The beneficial effects of the present invention are:

[0026] The present invention provides a method for preparing α-Al2O3 based on metaaluminate, wherein the metaaluminate is used as a raw material, calcined in a protective atmosphere containing chlorine-containing organic matter, and washed to obtain α-Al2O3. The technical solution provided by the present invention can obtain α-Al2O3 at a relatively low calcination temperature (650-1000°C), and obtain pure phase α-Al2O3 at a calcination temperature of 770-1000°C, which greatly reduces the calcination temperature of the traditional preparation of α-Al2O3, and the preparation method is simple, requiring only one calcination, one acid washing, and two washings, which can save manufacturing time and cost, and the obtained α-Al2O3 particles are uniform in size and have good dispersibility. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0028] Figure 1 This is a field emission scanning electron microscope image of the aluminum oxide prepared in Example 1 of the present invention;

[0029] Figure 2 The XRD diffraction pattern of the aluminum oxide prepared in Example 1 of the present invention;

[0030] Figure 3 This is a field emission scanning electron microscope image of aluminum oxide prepared in Example 2 of the present invention;

[0031] Figure 4 This is the XRD diffraction pattern of the aluminum oxide prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0032] In view of the problems of high calcination temperature and complicated procedures in the preparation process of α-Al2O3, the present invention provides a method for preparing α-Al2O3 based on metaaluminate. Based on the similarity between the crystal structures of metaaluminate and α-Al2O3, the present invention can prepare α-Al2O3 with high crystallinity at a lower temperature by calcining in a chlorine-containing organic atmosphere.

[0033] The first typical embodiment of the present invention provides a method for preparing α-Al2O3 based on metaaluminate, comprising the following steps:

[0034] Using aluminate as raw material, calcination is carried out in a chlorine-containing organic atmosphere to obtain an initial product, which is then washed to obtain α-Al2O3.

[0035] The present invention is based on the preparation of α-Al2O3 by metaaluminate. Based on the similarity between the crystal structure of the metaaluminate precursor and the α-Al2O3, the metaaluminate is calcined in a chlorine-containing organic atmosphere. The chlorine-containing organic matter decomposes at high temperature, and chlorine combines with the metal cations in the metaaluminate to generate chloride salt. As the temperature rises, the melting point of the chloride salt is reached, and the melted chloride salt is separated from the metaaluminate by volatilization. The volatilized chloride salt is separated from the reaction system along with the gas, and the metal cations in the metaaluminate are extracted. The metaaluminate is converted into α-Al2O3 at high temperature, and α-Al2O3 is obtained after washing to remove impurities (chloride salt) and non-α-Al2O3. The α-Al2O3 prepared by the method of the present invention has high crystallinity, regular morphology, uniform particle size distribution and good dispersibility.

[0036] The present invention successfully prepares α-Al2O3 by calcination. Since the melting point of chloride salt is relatively low, generally between 600 and 800°C, the calcination temperature is greatly reduced, energy is saved, and a huge space is created for the low-temperature preparation of α-Al2O3. In addition, the present invention provides a new method for preparing metal oxides, and different metal oxides can be obtained by changing the precursor, which has a huge development prospect.

[0037] In some examples of this embodiment, the metaaluminate includes but is not limited to lithium metaaluminate, sodium metaaluminate, potassium metaaluminate, calcium metaaluminate or magnesium metaaluminate. After the above metaaluminate is calcined in a chlorine-containing organic atmosphere, the melting point of the generated chloride salt is low, the melting point of sodium chloride is 801°C, the melting point of potassium chloride is 770°C, the melting point of lithium chloride is 605°C, the melting point of calcium chloride is 772°C, and the melting point of magnesium chloride is 714°C. This greatly reduces the calcination temperature, saves energy, and creates a huge space for the low-temperature preparation of α-Al2O3.

[0038] In some examples of this embodiment, the aluminate is calcined in a chlorine-containing organic compound to obtain α-Al2O3. To prepare pure phase α-Al2O3, the aluminate is preferably lithium aluminate, sodium aluminate or potassium aluminate.

[0039] In some examples of this embodiment, the chlorine-containing organic matter includes but is not limited to methane chloride, ethane chloride or propane chloride. The chlorine-containing organic matter decomposes during the calcination process to obtain carbon monoxide or carbon dioxide, chloride ions, etc. The chloride ions combine with the metal cations in the aluminate to obtain chloride salts. The aluminate is converted into α-Al2O3 under calcination conditions.

[0040] It should be noted that the chlorine-containing organic matter has different ratios of carbon atoms to chlorine atoms, which will lead to different consumption of the chlorine-containing organic matter in the actual reaction process. In order to improve the yield of α-Al2O3, the chlorine-containing organic matter is preferably a methane chloride, specifically monochloromethane, dichloromethane, trichloromethane or tetrachloromethane.

[0041] In some examples of this embodiment, the chlorine-containing organic atmosphere comprises a protective gas and a chlorine-containing organic;

[0042] The protective gas is nitrogen or argon. Nitrogen or argon is used as a carrier gas to blow the chlorine-containing organic matter into the reaction device to ensure that the aluminate is calcined in the chlorine-containing organic matter atmosphere.

[0043] In some examples of this implementation mode, the chlorine-containing organic matter is blown into the reaction device using a protective gas, specifically:

[0044] The chlorine-containing organic matter is placed in a gas washing bottle and maintained at a temperature of 1 to 50°C; a protective gas is introduced into the gas washing bottle, and the chlorine-containing organic matter is blown into the reaction device using the protective gas as a carrier gas, and the flow rate of the protective gas is 10 to 300 sccm. This flow rate can ensure that the chloride salt is fully volatilized and separated, and the residual chloride salt can be fully removed by washing.

[0045] Preferably, the gas wash bottle is a Monteggia gas wash bottle.

[0046] It should be noted that the present invention uses a carrier gas (i.e., a protective gas) to blow the chlorine-containing organic compound into the reaction device, and the blowing amount of the chlorine-containing organic compound is controlled by the carrier gas flow rate and the temperature of the chlorine-containing organic compound in the gas washing bottle. The carrier gas flow rate and the temperature of the chlorine-containing organic compound affect two important parameters of the chlorine-containing organic compound dosage. By adjusting the carrier gas flow rate and the temperature of the chlorine-containing organic compound, the flow state of the chlorine-containing organic compound can be affected, thereby affecting its dosage.

[0047] In some examples of this embodiment, the calcination temperature is 650-1000° C., the calcination time is 0.5-10 h, and the heating rate is 1-20° C. / min.

[0048] It should be noted that when aluminate is calcined in a chlorine-containing organic atmosphere, metal cations react with chlorine to form chloride salts. The melting point of chloride salts is relatively low, generally between 600 and 800°C. When the calcination temperature is greater than the melting point of chloride salts, the melted chloride salts are separated from aluminate by volatilization. Therefore, a calcination temperature between 650 and 1000°C can achieve the preparation of α-Al2O3 while saving energy.

[0049] In order to increase the yield of α-Al2O3 and obtain pure phase α-Al2O3, when sodium aluminate is used as raw material, the calcination temperature is 800-1000°C, and α-Al2O3 is obtained after calcination and washing.

[0050] When potassium aluminate is used as the raw material, the calcination temperature is 770-1000°C. After calcination and washing, α-Al2O3 is obtained.

[0051] When lithium aluminate is used as the raw material, the calcination temperature is 700-1000°C. After calcination and washing, α-Al2O3 is obtained.

[0052] In some examples of this embodiment, the washing includes water washing and acid washing, and the initial product is sequentially washed with water, acid washed, and water washed, and then dried to obtain α-Al2O3.

[0053] In some examples of this embodiment, the product after the first water washing is dried and then acid washed, and the drying temperature is 40-150°C.

[0054] In some examples of this embodiment, the acid washing process is: mixing acid and water in a volume ratio of 1:1 to 1:7, adding the initial product after water washing, and heating and washing.

[0055] In some examples of this embodiment, the acid is at least one of nitric acid, sulfuric acid, hydrochloric acid or phosphoric acid.

[0056] In some examples of this embodiment, the heated washing is washing at 40 to 220° C. for 0.5 to 8 hours.

[0057] In some examples of this embodiment, the drying is carried out at a temperature of 40 to 150°C.

[0058] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.

[0059] Example 1

[0060] This embodiment provides a method for preparing α-Al2O3 using NaAlO2, comprising the following steps:

[0061] (1) Take 0.5g NaAlO2 and place it in a corundum crucible, then put it into a tube furnace and seal it. After the tube furnace is evacuated, argon is blown into CH2Cl2. CH2Cl2 is placed in a Monte Carlo washing bottle and placed in a cooling circulating water bath. The water temperature is maintained at 15°C and the argon flow rate is maintained at 200sccm. After the gas flow is stable, heat the tube furnace to 800°C at a heating rate of 10°C / min and maintain it at this temperature for 1h. After the reaction is completed, the tube furnace is naturally cooled to room temperature.

[0062] (2) The product obtained in step (1) is washed multiple times with deionized water with the help of a suction filtration device, and the washed product is placed in an oven at 70° C. for drying.

[0063] (3) The product after drying in step (2) is mixed with dilute sulfuric acid, which is obtained by mixing 50 mL of water with 50 mL of concentrated sulfuric acid. The mixed product is placed in a high-pressure reactor and pickled at 100° C. for 4 hours to remove non-α-phase Al2O3 in the product.

[0064] (4) The product after acid washing in step (3) is washed multiple times with deionized water with the help of a suction filtration device, and the washed product is placed in an oven at 70° C. for drying to obtain pure phase α-Al 2 O 3 with a mass of 0.1559 g.

[0065] The morphology and particle size of the product obtained in this example were analyzed by field emission scanning electron microscopy (SEM, Hitachi S-4800). Figure 1 The phase of the product obtained in this example was analyzed by X-ray powder diffractometer (Bruker AXSD8 advanced), as shown in Figure 2 shown.

[0066] pass Figure 1 It can be seen that the morphology of α-Al2O3 synthesized by the reaction of NaAlO2 and CH2Cl2 is similar to a hexagonal lamellar structure, with a particle size of 0.9 to 1.2 μm, uniform particle size and good dispersibility.

[0067] Figure 2 The XRD results show that the product obtained in this embodiment has a crystal plane diffraction peak of α-Al2O3, and no other impurity peaks appear, indicating that the product obtained in this embodiment is pure phase α-Al2O3.

[0068] Example 2

[0069] This embodiment provides a method for preparing α-Al2O3 using LiAlO2, comprising the following steps:

[0070] (1) Take 0.5g LiAlO2 and place it in a corundum crucible, then put it into a tube furnace and seal it. After the tube furnace is evacuated, CHCl3 is blown in with argon. CHCl3 is placed in a Monte Carlo bottle and placed in a cooling circulating water bath. The water temperature is maintained at 20°C and the argon flow rate is maintained at 150sccm. After the gas flow is stable, heat the tube furnace to 1000°C at a heating rate of 10°C / min and maintain it at this temperature for 1h. After the reaction is completed, the tube furnace is naturally cooled to room temperature.

[0071] (2) The product obtained in step (1) is washed multiple times with deionized water with the help of a suction filtration device, and the washed product is placed in an oven at 70° C. for drying.

[0072] (3) The dried product of step (2) is mixed with dilute sulfuric acid, wherein the dilute sulfuric acid is prepared by mixing 70 mL of water with 10 mL of concentrated sulfuric acid. The mixed product is placed in a high pressure reactor and pickled at 180° C. for 2 h to remove non-α-phase Al2O3 in the product.

[0073] (4) The product after acid washing in step (3) is washed multiple times with deionized water with the help of a suction filtration device, and the washed product is placed in an oven at 70° C. for drying to obtain pure phase α-Al 2 O 3 with a mass of 0.1651 g.

[0074] The morphology and particle size of the product obtained in this example were analyzed by field emission scanning electron microscopy (SEM, Hitachi S-4800). Figure 3The phase of the product obtained in this example was analyzed by X-ray powder diffractometer (Bruker AXSD8 advanced), as shown in Figure 4 shown.

[0075] pass Figure 3 It can be seen that the α-Al2O3 synthesized by the reaction of LiAlO2 and CHCl3 has a long strip shape with regular shape and uniform particle size distribution.

[0076] Figure 4 The XRD results show that the product obtained in this embodiment has a crystal plane diffraction peak of α-Al2O3, and no other impurity peaks appear, indicating that the product obtained in this embodiment is pure phase α-Al2O3.

[0077] Example 3

[0078] This embodiment provides a preparation method of α-Al2O3 using KAlO2, which differs from the preparation method of Example 1 in that: in step (1), 0.5 g of KAlO2 is placed in a corundum crucible, and after the airflow is stable, the tube furnace is heated to 770°C at a heating rate of 10°C / min, and the remaining steps are consistent with Example 1.

[0079] The physical phase of the product obtained in this embodiment was analyzed by an X-ray powder diffractometer (Bruker AXSD8 advanced). The XRD results showed that the product obtained in this embodiment had a crystal plane diffraction peak of α-Al2O3, and no other impurity peaks appeared, indicating that the product obtained in this embodiment was pure phase α-Al2O3.

[0080] In summary, through the method of the present invention, NaAlO2 reacts with CH2Cl2 to obtain pure phase α-Al2O3 with uniform particle size at 800°C; KAlO2 reacts with CH2Cl2 to obtain pure phase α-Al2O3 with uniform particle size at 770°C; LiAlO2 reacts with CHCl3 to obtain pure phase α-Al2O3 with uniform particle size at 1000°C. And the method has the advantage of simple preparation process. Compared with the calcination temperature of traditional synthetic α-Al2O3, which mostly exceeds 1200°C, the technical solution provided by the present invention reduces the calcination temperature of α-Al2O3, can save energy, and create huge space for the low-temperature preparation of α-Al2O3. And the present invention provides a new method for preparing metal oxides, which can be expected to obtain different metal oxides by changing the precursor, and has great development prospects.

[0081] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing α-Al2O3 based on metaaluminate, characterized in that: The steps include: Using aluminate as raw material, calcination is carried out in a chlorine-containing organic atmosphere to obtain an initial product, which is then washed to obtain α-Al2O3.

2. The method according to claim 1, characterized in that The aluminate includes lithium aluminate, sodium aluminate, potassium aluminate, calcium aluminate or magnesium aluminate; Preferably, the aluminate is lithium aluminate, sodium aluminate or potassium aluminate.

3. The method according to claim 1, characterized in that The chlorine-containing organic matter includes methane chloride, ethane chloride or propane chloride; Preferably, the chlorine-containing organic compound is a methane chloride, specifically monochloromethane, dichloromethane, trichloromethane or tetrachloromethane.

4. The method according to claim 1, characterized in that The chlorine-containing organic atmosphere comprises a protective gas and a chlorine-containing organic, and the protective gas is nitrogen or argon.

5. The method according to claim 4, characterized in that The temperature of the chlorine-containing organic matter is 1-50° C.; the flow rate of the chlorine-containing organic matter atmosphere is 10-300 sccm.

6. The method according to claim 1, characterized in that The calcination temperature is 650-1000°C, the calcination time is 0.5-10h, and the heating rate is 1-20°C / min; Preferably, when sodium aluminate is used as the raw material, the calcination temperature is 800-1000°C, and after calcination and washing, α-Al2O3 is obtained; Preferably, when potassium aluminate is used as the raw material, the calcination temperature is 770-1000°C, and after calcination and washing, α-Al2O3 is obtained; Preferably, when lithium aluminate is used as the raw material, the calcination temperature is 700-1000°C, and after calcination and washing, α-Al2O3 is obtained.

7. The method according to claim 1, characterized in that The washing includes water washing and acid washing. The initial product is sequentially washed with water, acid washed, and water washed, and then dried to obtain α-Al2O3.

8. The method according to claim 7, characterized in that The pickling process is as follows: acid and water are mixed in a volume ratio of 1:1 to 1:7, the initial product after water washing is added, and heating and washing are performed.

9. The method according to claim 8, characterized in that The acid is at least one of nitric acid, sulfuric acid, hydrochloric acid or phosphoric acid.

10. The method according to claim 8, characterized in that The heating washing is washing at 40 to 220° C. for 0.5 to 8 hours.