Sodium-ion battery composite electrode material and preparation method thereof
By preparing a composite electrode material with bimetal sulfide-doped zinc oxide nanosheets loaded with carbon nanocage, the problem of poor volume expansion and cycle stability of zinc oxide negative electrode material in sodium ion batteries is solved, and the charging and discharging efficiency and battery life are improved.
Patent Information
- Application Number
- CN202411043724.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-31
AI Technical Summary
Zinc oxide (ZnO) negative electrode material expands volumetrically during charging and discharging of sodium ion batteries, resulting in a degradation of battery performance, and its cycle stability and first-time Coulomb efficiency are poor, affecting the mechanical stability and life of the battery.
Using raw materials such as zinc salt, complexing agent, dopamine and molybdenum salt, the composite electrode material with bimetal sulfide-doped zinc oxide nanosheets loaded with carbon nanocage is formed to form ultra-thin two-dimensional nanosheets vertically interwoven to form a three-dimensional microsphere structure. , improve the electron transfer rate and redox reaction rate, and buffer volume changes to damage the structural damage of the electrode material.
The first Coulomb efficiency of the ZnO negative electrode material is significantly improved, the cycle stability and electrochemical performance of the battery are enhanced, and the life of the battery is extended.
Smart Images

Figure CN118954573A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nanocomposite materials, and in particular relates to a sodium ion battery composite electrode material and a preparation method thereof. Background Art
[0002] As a negative electrode material for sodium ion batteries, compared with NiO, Co 3 O 4 and Fe 3 O 4 Zinc oxide (ZnO) has a higher theoretical specific capacity (~978 mAh g -1 ), lower cost and harmless to the environment, but during the charge and discharge process, the structure of ZnO will change, resulting in its volume expansion. This volume expansion will lead to a decrease in the overall performance of the battery, and may even cause dangerous situations such as short circuits. Volume expansion is a major problem facing the ZnO negative electrode because it affects the mechanical stability and cycle life of the battery; at the same time, the material of the ZnO negative electrode will inevitably undergo redox reactions during the charge and discharge process, which accelerates the aging process of the negative electrode material. With the increase in the number of charge and discharge cycles, the material will undergo a fixed structural change, which will eventually lead to a decrease in its capacity, thereby shortening the life of the battery; in addition, the negative electrode has inherent low conductivity and severe crushing during the cycle, resulting in poor rate and cycle performance. In general, designing nanostructure morphology, metal sulfide doping and preparing composite materials are effective methods to solve these problems. However, although the above methods have improved the electrochemical activity of the ZnO negative electrode, its cycle stability is still poor, especially the first coulombic efficiency of charge and discharge is still poor. Summary of the invention
[0003] The object of the present invention is to provide a sodium ion battery composite electrode material and a preparation method thereof, so as to solve the technical problem that the existing modified ZnO negative electrode material has poor first coulomb efficiency of charge and discharge.
[0004] In order to achieve the above object, the present invention adopts the following technical solutions:
[0005] The invention discloses a method for preparing a composite electrode material for a sodium ion battery, comprising the following steps:
[0006] After the zinc salt, the complexing agent and the solvent are mixed and stirred for reaction, the product is collected, washed and dried in sequence to obtain a precursor A;
[0007] Precursor A, dopamine and deionized water are mixed and stirred to react, and the resulting material is collected and calcined to obtain an intermediate product B;
[0008] Dispersing molybdenum salt, dopamine and intermediate product B in deionized water, stirring to react, and collecting solid products in sequence;
[0009] The solid product and sulfur powder are mixed and calcined to obtain a sodium ion battery composite electrode material.
[0010] Furthermore, in the step of obtaining precursor A, the usage ratio of the zinc salt, the complexing agent and the solvent is (1-3) g: (1-3) g: 150 mL, and the stirring time is 10-20 h.
[0011] Furthermore, in the step of obtaining the intermediate product B, the amount ratio of the precursor A, dopamine and deionized water is (5-10) g: 1 g: 150 mL, and the stirring time is 10-12 h.
[0012] Furthermore, in the step of obtaining the intermediate product B, the calcination treatment is carried out in an inert atmosphere at a temperature of 600 to 800° C. for a time of 1 to 3 hours.
[0013] Furthermore, in the step of obtaining a solid product, the molybdenum salt, dopamine, intermediate product B and deionized water are used in a ratio of 1 g: 1 g: (0.1-0.3) g: 150 mL, and the stirring time is 6-8 h.
[0014] Furthermore, before the solid product and sulfur powder are mixed and calcined, the solid product is pretreated in a tube furnace at 300-500°C for 2-4 hours; the calcination temperature of the solid product and sulfur powder after calcination is 500-600°C and the time is 2-4 hours.
[0015] Furthermore, the mass ratio of the solid product to sulfur powder is 1:(2-4).
[0016] Furthermore, the zinc salt is one or more of zinc nitrate, zinc sulfate and zinc chloride; the complexing agent is one or more of 2-ethylimidazole, 4-hydroxymethylimidazole and 2-chloromethylimidazole; the solvent is anhydrous methanol; and the molybdenum salt is one or both of ammonium molybdate and sodium molybdate.
[0017] The invention also discloses a sodium ion battery composite electrode material prepared by the preparation method.
[0018] Furthermore, the microstructure of the sodium ion battery composite electrode material is composed of bimetallic sulfide-doped zinc oxide nanosheets loaded with carbon nanocages; the thickness of the zinc oxide nanosheets is 25-30nm; the size of the carbon nanocage is 100nm and the wall thickness is 20nm.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The invention discloses a method for preparing a composite electrode material for a sodium ion battery. Zinc salt, a complexing agent, dopamine and a molybdenum salt are used as raw materials. In the preparation process, a complexing agent is introduced and preparation process parameters are adjusted to prepare a composite electrode material for a sodium ion battery in which ultra-thin two-dimensional nanosheets are vertically interwoven to form a three-dimensional micron ball structure. The abundant pores between the nanosheets are conducive to the rapid infiltration of an electrolyte, promote the contact between active substances and sodium ions, and are also conducive to the release of sodium ions. At the same time, bimetallic sulfide is doped to replace part of the sites of the ZnO lattice, thereby improving the electron transmission rate of ZnO and its surface redox reaction rate, and buffering the structural damage of the electrode material caused by the volume change of ZnO during the charge and discharge process. A layer of carbon nanocage is loaded on the surface of the ZnO nanosheet, wherein the carbon nanocage has a size of about 100 nm and a wall thickness of about 20 nm, and simultaneously plays a role in improving the transmission rate of its electrons and ions, thereby effectively improving the first coulomb efficiency of the charge and discharge of the ZnO negative electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The SEM and TEM images of the carbon nanocages in the microstructure of the composite electrode material for sodium ion batteries of the present invention are shown;
[0022] Among them: a-SEM image; b-TEM image;
[0023] Figure 2 This is a SEM image of the composite electrode material for a sodium ion battery of the present invention;
[0024] Figure 3 is the XRD diagram of the composite electrode material for sodium ion battery of the present invention;
[0025] Figure 4 This is a charge and discharge curve diagram of the sodium ion battery composite electrode material of the present invention. DETAILED DESCRIPTION
[0026] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0027] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0028] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0029] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0030] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0031] The present invention provides a method for preparing a composite electrode material for a sodium ion battery, comprising the following steps:
[0032] S1: Dissolve zinc salt (1-3 g) and complexing agent (1-3 g) in 150 mL of anhydrous methanol by ultrasonication, stir at room temperature for 10-20 h, collect the product, wash and dry it to prepare precursor A;
[0033] S2: Precursor A and dopamine were added into 150 mL of deionized water in a mass ratio of 5 to 10:1, stirred at room temperature for 10 to 12 h, the product was collected, and calcined under an argon atmosphere to prepare an intermediate product B;
[0034] S3: Disperse the molybdenum salt, dopamine and intermediate product B in 150 mL of deionized water in a mass ratio of 1:1:0.1-0.3, stir at room temperature for 6-8 hours, collect the solid product, wash and dry it;
[0035] S4: The above product is pretreated in a tubular furnace, and then sulfur powder is added after cooling, and the composite electrode material of the sodium ion battery is obtained after calcination.
[0036] Preferably, in S1, the zinc salt includes but is not limited to zinc nitrate, zinc sulfate, zinc chloride, and the complexing agent includes but is not limited to 2-ethylimidazole, 4-hydroxymethylimidazole, and 2-chloromethylimidazole.
[0037] Preferably, in S2, the calcination temperature is 600-800° C., and the calcination time is 1-3 hours.
[0038] Preferably, in S3, the molybdenum salt includes but is not limited to ammonium molybdate and sodium molybdate.
[0039] Preferably, in S4, the pretreatment temperature is 300-500° C., and the pretreatment time is 2-4 hours.
[0040] Preferably, in S4, the mass ratio of the solid product to the sulfur powder is 1:2-4.
[0041] Preferably, in S4, the calcination temperature is 500-600° C., and the calcination time is 2-4 hours.
[0042] The invention also discloses a sodium ion battery composite electrode material prepared by the preparation method. The sodium ion battery composite electrode material is composed of bimetallic sulfide-doped zinc oxide nanosheets loaded with carbon nanocages. The thickness of the nanosheets is 25-30nm, the size of the carbon nanocage is 100nm, and the wall thickness is 20nm.
[0043] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0044] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0045] Example 1
[0046] A method for preparing a composite electrode material for a sodium ion battery comprises the following steps:
[0047] S1: 3 g zinc nitrate (zinc salt) and 3 g 4-hydroxymethylimidazole (complexing agent) were ultrasonically dissolved in 150 mL of anhydrous methanol, stirred at room temperature for 10 h, the product was collected, washed, and dried to obtain precursor A;
[0048] S2: 10 g of precursor A and 1 g of predopamine were added to 150 mL of deionized water, stirred at room temperature for 12 h, the product was collected, and calcined at 800 °C for 3 h in an argon atmosphere to obtain an intermediate product B;
[0049] S3: Disperse 1 g of ammonium molybdate (molybdenum salt), 1 g of dopamine and 0.3 g of intermediate product B in 150 mL of deionized water, stir at room temperature for 8 h, collect the solid product, wash and dry;
[0050] S4: 1 g of the solid product was pretreated in a tubular furnace at 500°C for 4 h, and then 4 g of sulfur powder was added and calcined at 600°C for 4 h to obtain a sodium ion battery composite electrode material.
[0051] Example 2
[0052] A method for preparing a composite electrode material for a sodium ion battery comprises the following steps:
[0053] S1: Dissolve 1 g zinc chloride (zinc salt) and 2 g 2-chloromethylimidazole (complexing agent) in 150 mL anhydrous methanol by ultrasonication, stir at room temperature for 15 h, collect the product, wash and dry it to obtain precursor A;
[0054] S2: 8 g of precursor A and 1 g of predopamine were added to 150 mL of deionized water, stirred at room temperature for 10 h, the product was collected, and calcined at 700 °C in an argon atmosphere for 2 h to obtain an intermediate product B;
[0055] S3: Disperse 1 g of sodium molybdate (molybdenum salt), 1 g of dopamine and 0.2 g of intermediate product B in 150 mL of deionized water, stir at room temperature for 6 h, collect the solid product, wash and dry;
[0056] S4: 1 g of the solid product was pretreated in a tubular furnace at 400°C for 3 h, and then 3 g of sulfur powder was added and calcined at 550°C for 3 h to obtain a sodium ion battery composite electrode material.
[0057] Example 3
[0058] A method for preparing a composite electrode material for a sodium ion battery comprises the following steps:
[0059] S1: Dissolve 1 g zinc sulfate (zinc salt) and 1 g 2-ethylimidazole (complexing agent) in 150 mL anhydrous methanol by ultrasonication, stir at room temperature for 10 h, collect the product, wash and dry it to obtain precursor A;
[0060] S2: 5 g of precursor A and 1 g of predopamine were added to 150 mL of deionized water, stirred at room temperature for 10 h, the product was collected, and calcined at 600 °C in an argon atmosphere for 1 h to obtain an intermediate product B;
[0061] S3: Disperse 1 g of ammonium molybdate (molybdenum salt), 1 g of dopamine and 0.1 g of intermediate product B in 150 mL of deionized water, stir at room temperature for 6 h, collect the solid product, wash and dry;
[0062] S4: 1 g of the solid product was pretreated in a tubular furnace at 300°C for 2 h, and then 2 g of sulfur powder was added and calcined at 500°C for 2 h to obtain a sodium ion battery composite electrode material.
[0063] Example 4
[0064] A method for preparing a composite electrode material for a sodium ion battery comprises the following steps:
[0065] S1: 3 g zinc chloride (zinc salt) and 1 g 4-hydroxymethylimidazole (complexing agent) were ultrasonically dissolved in 150 mL of anhydrous methanol, stirred at room temperature for 15 h, the product was collected, washed, and dried to obtain precursor A;
[0066] S2: 8 g of precursor A and 1 g of predopamine were added to 150 mL of deionized water, stirred at room temperature for 10 h, the product was collected, and calcined at 650 °C for 2 h in an argon atmosphere to obtain an intermediate product B;
[0067] S3: Disperse 1 g of sodium molybdate (molybdenum salt), 1 g of dopamine and 0.3 g of intermediate product B in 150 mL of deionized water, stir at room temperature for 8 h, collect the solid product, wash and dry;
[0068] S4: 1 g of the solid product was pretreated in a tubular furnace at 330° C. for 3 h, and then 4 g of sulfur powder was added and calcined at 500° C. for 3 h to obtain a sodium ion battery composite electrode material.
[0069] Example 5
[0070] A method for preparing a composite electrode material for a sodium ion battery comprises the following steps:
[0071] S1: 2 g zinc nitrate (zinc salt) and 3 g 2-chloromethylimidazole (complexing agent) were ultrasonically dissolved in 150 mL of anhydrous methanol, stirred at room temperature for 18 h, the product was collected, washed, and dried to obtain precursor A;
[0072] S2: 6 g of precursor A and 1 g of predopamine were added to 150 mL of deionized water, stirred at room temperature for 10 h, the product was collected, and calcined at 700 °C in an argon atmosphere for 2 h to obtain an intermediate product B;
[0073] S3: Disperse 1 g of sodium molybdate (molybdenum salt), 1 g of dopamine and 0.3 g of intermediate product B in 150 mL of deionized water, stir at room temperature for 6 h, collect the solid product, wash and dry;
[0074] S4: 1 g of the solid product was pretreated in a tubular furnace at 400°C for 2 h, and then 4 g of sulfur powder was added and calcined at 580°C for 4 h to obtain a sodium ion battery composite electrode material.
[0075] Figure 1 The SEM and TEM images of the carbon nanocage in the microstructure of the sodium ion battery composite electrode material of the present invention show that the carbon nanocage has a size of 100 nm and a wall thickness of 20 nm.
[0076] Figure 2 and Figure 3 The SEM image and XRD image of the sodium ion battery composite electrode material of the present invention show that the microstructure of the sodium ion battery composite electrode material is composed of bimetallic sulfide-doped zinc oxide nanosheets loaded with carbon nanocages, and the thickness of the zinc oxide nanosheets is 25-30 nm.
[0077] Figure 4 This is a charge and discharge curve diagram of the sodium ion battery composite electrode material of the present invention. It can be seen that the composite electrode material prepared by the present invention has a first discharge specific capacity of 471 mAh / g at 0.1 A / g, a first coulombic efficiency of 93%, and a discharge specific capacity of 361 mAh / g after 100 cycles.
[0078] Table 1 is a comparison of the electrochemical properties of the sodium ion battery composite electrode material prepared in Example 1 of the present invention and the product obtained in the prior art. From the table, it can be seen that the composite electrode material prepared by the present invention has advantages in comprehensive electrochemical performance such as specific capacity, first coulombic efficiency, rate, and cycle.
[0079] Table 1 Comparison of electrochemical properties of the products prepared by the present invention and related products
[0080]
[0081]
[0082] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a composite electrode material for a sodium ion battery, characterized in that: The following steps are involved: After the zinc salt, the complexing agent and the solvent are mixed and stirred for reaction, the product is collected, washed and dried in sequence to obtain a precursor A; Precursor A, dopamine and deionized water are mixed and stirred to react, and the resulting material is collected and calcined to obtain an intermediate product B; Dispersing molybdenum salt, dopamine and intermediate product B in deionized water, stirring to react, and collecting solid products in sequence; The solid product and sulfur powder are mixed and calcined to obtain a sodium ion battery composite electrode material.
2. The method for preparing a composite electrode material for a sodium ion battery according to claim 1, characterized in that: In the step of obtaining precursor A, the usage ratio of the zinc salt, the complexing agent and the solvent is (1-3) g: (1-3) g: 150 mL, and the stirring time is 10-20 h.
3. The method for preparing a composite electrode material for a sodium ion battery according to claim 1, characterized in that: In the step of obtaining the intermediate product B, the amount ratio of the precursor A, dopamine and deionized water is (5-10) g: 1 g: 150 mL, and the stirring time is 10-12 h.
4. The method for preparing a composite electrode material for a sodium ion battery according to claim 1, characterized in that: In the step of obtaining the intermediate product B, the calcination treatment is carried out in an inert atmosphere at a temperature of 600 to 800° C. for a time of 1 to 3 hours.
5. The method for preparing a composite electrode material for a sodium ion battery according to claim 1, characterized in that: In the step of obtaining a solid product, the molybdenum salt, dopamine, intermediate product B and deionized water are used in a ratio of 1 g: 1 g: (0.1-0.3) g: 150 mL, and the stirring time is 6-8 h.
6. The method for preparing a composite electrode material for a sodium ion battery according to claim 1, characterized in that: Before the solid product and sulfur powder are mixed and calcined, the solid product is pretreated in a tube furnace at 300-500°C for 2-4 hours; the calcination temperature of the solid product and sulfur powder after calcination is 500-600°C and the time is 2-4 hours.
7. The method for preparing a composite electrode material for a sodium ion battery according to claim 1, characterized in that: The mass ratio of the solid product to sulfur powder is 1:(2-4).
8. The method for preparing a composite electrode material for a sodium ion battery according to claim 1, characterized in that: The zinc salt is one or more of zinc nitrate, zinc sulfate and zinc chloride; the complexing agent is one or more of 2-ethylimidazole, 4-hydroxymethylimidazole and 2-chloromethylimidazole; the solvent is anhydrous methanol; and the molybdenum salt is one or both of ammonium molybdate and sodium molybdate.
9. A sodium ion battery composite electrode material, characterized in that: The preparation method is described in any one of claims 1 to 8.
10. A sodium ion battery composite electrode material according to claim 9, characterized in that: The microstructure of the sodium ion battery composite electrode material is composed of bimetallic sulfide-doped zinc oxide nanosheets loaded with carbon nanocages; the thickness of the zinc oxide nanosheets is 25-30nm; the size of the carbon nanocage is 100nm, and the wall thickness is 20nm.
Citation Information
Patent Citations
Zinc-cobalt sulfide / nitrogen-doped carbon composite material and preparation method and application thereof
CN108281628A
Preparation method and application of fast-charging type long-circulation SnO2 (at) C nanocage negative electrode material
CN116314701A
High-performance sodium ion battery negative electrode ZnS / Sb2S3 (at) NC composite material and preparation method thereof
CN117712378A