Method and technology for preparing basic zinc chloride particles and byproduct calcium chloride solution

By regulating the crystal form of alkaline zinc chloride in the presence of ammonium chloride, combined with multi-step filtration and evaporation treatment, the problems of alkaline zinc chloride particle size control and waste liquid treatment are solved, and high-efficiency alkaline zinc chloride is achieved Preparation and resource utilization meet the market's requirements for particle size and environmental protection.

CN118954575APending Publication Date: 2024-11-15SHENZHEN SHENTOU ENVIRONMENT TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410914221.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the existing preparation methods for alkaline zinc chloride, the particle size control is difficult, resulting in excessive crushing of the product, unable to meet the low dust export indicators of the European and American markets, and the waste liquid generated during the production process is costly and the by-product treatment is complex.

Method used

In the presence of ammonium chloride, zinc chloride is stirred and calcium hydroxide, and the reaction conditions such as stirring speed, temperature and pH are controlled. The crystal form of alkaline zinc chloride is regulated by ammonium chloride to form large-particle particles. , and the high-quality calcium chloride solution was generated through multi-step filtration and evaporation treatment, achieving resource utilization.

Benefits of technology

Prepare large-grain alkaline zinc chloride with uniform particle size, good fluidity and less dust. Through resource utilization of waste liquid, the cost of production and waste liquid treatment is reduced, and the market's requirements for particle size and environmental protection are met. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954575A_ABST
    Figure CN118954575A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of microelement feed additive manufacturing, simultaneously relates to the technical field of wastewater treatment and resource utilization, and particularly relates to a preparation method and technology of basic zinc chloride particles and a byproduct calcium chloride solution thereof. According to the preparation method of the basic zinc chloride, zinc chloride and calcium hydroxide are stirred to react in a liquid medium in the presence of ammonium chloride serving as a crystal form control agent, and the feed additive basic zinc chloride particles which are good in fluidity and less in flying dust are obtained. The embodiment of the invention provides a preparation method of basic zinc chloride particles and a byproduct calcium chloride solution thereof, namely a calcium chloride solution byproduct with relatively high quality is obtained by sequentially carrying out secondary zinc precipitation by calcium hydroxide, deep zinc removal by sodium sulfide, evaporation concentration and ammonia nitrogen removal by a break point chlorination method on a first filtrate generated in preparation of basic zinc chloride. The resource utilization of the basic zinc chloride production waste liquid is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of manufacturing trace element feed additives, as well as the technical field of wastewater treatment and resource utilization, and in particular to a method and technology for preparing basic zinc chloride particles and producing calcium chloride solution as a by-product. Background Art

[0002] Basic zinc chloride, with the molecular formula of Zn5(OH)8Cl2·H2O, has white or colorless transparent microscopic particles; it is insoluble in water, but soluble in weak acids and weak bases. As a new type of trace element feed additive, basic zinc chloride has the advantages of stable chemical structure, high bioavailability, low dosage, extremely low moisture absorption rate in the air, no agglomeration, and little destructive effect on nutrients such as oils, vitamins and enzymes, compared with traditional inorganic zinc source additives such as zinc sulfate and zinc oxide. It has the trend of replacing zinc sulfate and zinc oxide in European and American countries.

[0003] At present, there are many methods for preparing basic zinc chloride reported in the literature, which can be summarized into four categories: the first category is to use zinc chloride to neutralize with alkaline substances that do not contain zinc, such as sodium hydroxide, calcium hydroxide, ammonia water or ammonium bicarbonate, and control the pH value to 5-8 to generate basic zinc chloride precipitation. Relevant patents include CN110980799B, CN103121706B, CN101712485, CN104276595B, CN114304395A, CN112481505B, CN107324375A, CN117509711A, etc.; this type of method reacts quickly and fully, and the by-product is wastewater containing high concentrations of sodium chloride, calcium chloride or ammonium chloride and zinc ions, which needs to be treated secondary. The second type is to react zinc chloride with other zinc-containing materials such as zinc oxide, zinc hydroxide, metallic zinc + oxygen, diammine zinc dichloride, and zinc chloride ammine complex to generate basic zinc chloride precipitate. Relevant patents include CN1328171C, CN114057218A, CN101704545B, CN100496278C, CN111453762A, CN107857291B, etc. Among them, the reaction of zinc chloride solution with zinc oxide, zinc hydroxide or metallic zinc belongs to the liquid-solid phase synthesis method, and there are disadvantages such as unconverted zinc oxide or zinc hydroxide mixed in the basic zinc chloride product and low purity; and when zinc chloride solution reacts with zinc-containing materials containing high concentration of ammonia nitrogen such as diammine zinc dichloride and zinc chloride ammine complex, there are disadvantages such as high ammonia nitrogen content and low purity of the basic zinc chloride product. The third category is to prepare basic zinc chloride by reacting hydrochloric acid with zinc oxide, zinc hydroxide or zinc diammine dichloride and other zinc-containing materials, and controlling the pH value to 6-8. The relevant patents include CN100366539C and CN103053812A. This type of method reacts quickly and fully; but due to the high price of related raw materials, the overall production cost is high. The fourth category is other categories, including CN113753941A, which mentions the use of zinc oxide and ammonium chloride for solid phase heating to synthesize basic zinc chloride, but the two materials are not fully mixed before the reaction, and the purity of the product is questionable; CN111747443A mentions the distillation of zinc chloride ammonia solution to obtain basic zinc chloride, but it is difficult to completely remove ammonia nitrogen from the product by simply distilling ammonia, and the purity of the product is unknown.

[0004] However, the above-mentioned preparation method of basic zinc chloride pays less attention to the particle size of the basic zinc chloride product. In fact, if the reaction conditions are not finely controlled, the prepared basic zinc chloride particles are often small in size, large in specific surface area, and poor in filtering and washing performance; after drying, they are in powder form and cannot meet the low dust export index requirements of European and American customers. There are two types of solutions: one is to perform secondary granulation of powdered basic zinc chloride, but this will increase equipment investment and production and operation costs, and reduce the market competitiveness of the product. The second is to directly synthesize large-particle basic zinc chloride. For example, CN107857291B uses high-concentration ammonium chloride as an inducer to synthesize basic zinc chloride with large particle size and good fluidity, but there are disadvantages such as low product yield and high wastewater treatment cost; CN117509711A claims that long-term standing after the basic zinc chloride synthesis reaction is completed can make the basic zinc chloride particles gradually grow, but verification tests show that the effect is not obvious; CN104276595B synthesizes large-particle basic zinc chloride particles in an organic acid induction system, but the addition of organic inducers not only increases the difficulty of subsequent wastewater treatment, but the food safety of organic inducers has not been confirmed.

[0005] On the other hand, the basic zinc chloride production technology that can be applied on a large scale at present is the "liquid alkali method" process of neutralizing and precipitating zinc chloride solution with sodium hydroxide, during which a large amount of waste liquid containing sodium chloride will be produced. In addition, the "liquid alkali method" process adopted by patent CN108689427B will also add a small amount of ammonium salt to increase the particle size of basic zinc chloride; at this time, it is necessary to adopt alkaline ammonia evaporation to remove most of the ammonia nitrogen and zinc ions in the waste liquid; the small amount of zinc ions and ammonia nitrogen remaining in the sodium chloride waste liquid can be deeply removed by heavy metal capture agent precipitation method and inflection point chlorination method, and finally the traditional evaporation crystallization technology is adopted to obtain sodium chloride by-products. As for the "lime method" process adopted by patent CN103121706B, in which zinc chloride solution and calcium hydroxide suspension are neutralized and precipitated to prepare basic zinc chloride, the size of the product particle size and the destination of the waste liquid containing calcium chloride are not explained. Summary of the invention

[0006] In view of the above problems, the embodiments of the present application provide a preparation method of basic zinc chloride, basic zinc chloride particles and applications to solve the above technical problems.

[0007] In a first aspect, an embodiment of the present application provides a method for preparing basic zinc chloride, wherein zinc chloride and calcium hydroxide are stirred and reacted in a liquid medium in the presence of ammonium chloride to obtain basic zinc chloride particles.

[0008] Optionally, the stirring speed is 30-100 r / min, the reaction temperature is 70-95° C., and the reaction pH value is 5.5-6.5.

[0009] Optionally, the preparation method of basic zinc chloride comprises:

[0010] Adding ammonium chloride as a crystal control agent to a zinc chloride solution with a zinc concentration of 50 to 150 g / L to obtain a zinc chloride working solution with an ammonia nitrogen concentration of 2 to 10 g / L;

[0011] Under stirring, the zinc chloride working solution and the calcium hydroxide suspension are mixed and reacted to obtain basic zinc chloride particles, wherein the mass fraction of calcium hydroxide in the calcium hydroxide suspension is 10-30%.

[0012] Optionally, the crystal shape controlling agent is solid ammonium chloride or a saturated ammonium chloride solution;

[0013] The zinc chloride working solution and the calcium hydroxide suspension are mixed and reacted under stirring to obtain basic zinc chloride particles, including:

[0014] Adding the base solution to the reaction vessel;

[0015] Under stirring, the zinc chloride working solution and the calcium hydroxide suspension are simultaneously added into the reaction container in a parallel flow feeding manner, so that the zinc chloride working solution and the calcium hydroxide suspension are mixed and reacted to obtain a reaction solution;

[0016] The reaction solution is aged, and the aged reaction solution is filtered to obtain basic zinc chloride precipitate and a first filtrate, respectively, wherein the aging time is 30 min to 120 min.

[0017] Drying the basic zinc chloride precipitate to obtain the basic zinc chloride particles;

[0018] Wherein, the base liquid includes water or the first filtrate.

[0019] In a second aspect, the present invention provides a method for preparing basic zinc chloride particles and producing a calcium chloride solution as a by-product, comprising:

[0020] Adding ammonium chloride as a crystal control agent to the zinc chloride solution to obtain a zinc chloride working solution with an ammonia nitrogen concentration of 2 to 10 g / L;

[0021] Under stirring, the zinc chloride working solution and the calcium hydroxide suspension are simultaneously added into the reaction container in a parallel flow feeding manner, so that the zinc chloride working solution and the calcium hydroxide suspension are mixed and reacted to obtain a first reaction solution;

[0022] Aging the first reaction solution, filtering the aged first reaction solution to obtain basic zinc chloride precipitate and a first filtrate respectively; drying the basic zinc chloride precipitate to obtain basic zinc chloride particles;

[0023] The first filtrate is added to the reaction container, and under stirring, the calcium hydroxide suspension is added to the reaction container, so that the first filtrate and the calcium hydroxide suspension react to obtain a second reaction solution, and the second reaction solution is filtered to obtain zinc hydroxide mud and a second filtrate respectively;

[0024] The second filtrate is added to the reaction container, and under stirring, a sodium sulfide solution with a mass fraction of 5 to 15% is added to the reaction container, so that the second filtrate and the sodium sulfide solution react to obtain a third reaction liquid, the third reaction liquid is filtered to obtain zinc sulfide mud and a third filtrate respectively, and the third filtrate is evaporated and concentrated to obtain a concentrated liquid;

[0025] The concentrated solution is added to the reaction container, and bleaching powder or bleaching spirit is added to the reaction container under stirring, so that the concentrated solution and the bleaching powder or bleaching spirit react to obtain a fourth reaction solution, and the fourth reaction solution is filtered to obtain calcium-containing filter mud and calcium chloride solution respectively.

[0026] Optionally, the stirring speed of the zinc chloride working solution and the calcium hydroxide suspension for the mixed reaction is 30 to 100 r / min, the reaction temperature is 70 to 95° C., and the reaction pH value is 5.5 to 6.5; the aging time of the first reaction solution is 30 to 120 min;

[0027] and / or, the reaction endpoint of the reaction between the first filtrate and the calcium hydroxide suspension is a pH value of 10 to 12;

[0028] and / or, the end point of the reaction of the second filtrate and the sodium sulfide solution is that no white precipitate is produced;

[0029] And / or, the mass ratio of chlorine element to nitrogen element in the reaction solution formed by the concentrated solution and the bleaching powder or bleaching essence is 15:1.

[0030] In a third aspect, an embodiment of the present application provides basic zinc chloride particles prepared by the above-mentioned method for preparing basic zinc chloride or the above-mentioned method for preparing basic zinc chloride particles and producing calcium chloride solution as a by-product.

[0031] Optionally, the particle size of the basic zinc chloride particles is less than 40 meshes, and the mass percentage of particles with a particle size less than 200 meshes in the basic zinc chloride particles is less than 10%.

[0032] In a fourth aspect, an embodiment of the present application provides a calcium chloride solution prepared by the above-mentioned method for preparing basic zinc chloride particles and producing a calcium chloride solution as a by-product.

[0033] Optionally, the mass fraction of calcium chloride in the calcium chloride solution is 20% to 40%, the zinc content is less than or equal to 3 mg / kg, and the ammonia nitrogen content is less than or equal to 15 mg / kg.

[0034] The preparation method of basic zinc chloride and basic zinc chloride particles provided in the embodiment of the present application are as follows: in a liquid medium, zinc chloride and calcium hydroxide are stirred and reacted in the presence of ammonium chloride to obtain basic zinc chloride particles; in the above manner, ammonium chloride can regulate the crystal form of basic zinc chloride by a reversible chemical reaction of "dissolution-reprecipitation" on the surface of basic zinc chloride crystals, thereby increasing the particle size of the prepared basic zinc chloride particles, and in the presence of ammonium chloride, the prepared basic zinc chloride particles have good fluidity and less dust; the method for preparing basic zinc chloride particles and producing calcium chloride solution as a by-product provided in the embodiment of the present application is to sequentially subject the first filtrate produced by the preparation of basic zinc chloride to secondary zinc precipitation with calcium hydroxide, deep zinc removal with sodium sulfide, evaporation concentration and inflection point chlorination method to remove ammonia nitrogen, so as to obtain a high-quality calcium chloride solution by-product, thereby realizing the resource utilization of waste liquid from the production of basic zinc chloride.

[0035] These and other aspects of the present application will become more clearly understood in the description of the following embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 The schematic diagram of the process of the method for preparing basic zinc chloride particles and producing calcium chloride solution as a by-product provided in an embodiment of the present application is shown.

[0037] Figure 2 The XRD pattern of the basic zinc chloride particles prepared in Example 1 of the present application is shown. DETAILED DESCRIPTION

[0038] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.

[0039] In order to enable those skilled in the art to better understand the solutions of the present application, the technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present application.

[0040] In the embodiments of the present application, it should be noted that, in this article, relational terms such as first and second, etc. are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship or order between these entities or operations.

[0041] Moreover, the terms "comprises," "comprising," or any other variation thereof are intended to encompass non-exclusive inclusion, such that a process, method, article, or apparatus that includes a list of elements includes not only those elements, but also other elements not explicitly listed, or elements inherent to such process, method, article, or apparatus. In the absence of further limitations, an element defined by the phrase "comprising a ..." does not exclude the presence of additional identical elements in the process, method, article, or apparatus that includes the element.

[0042] In the description of the embodiments of the present application, words such as "example" or "for example" are used to indicate examples, illustrations or descriptions. Any embodiment or design described as "example" or "for example" in the embodiments of the present application is not to be interpreted as being more preferred or having more advantages than another embodiment or design. The use of words such as "example" or "for example" is intended to present relative concepts in a clear manner.

[0043] In addition, the "plurality" in the embodiments of the present application refers to two or more than two. In view of this, in the embodiments of the present application, "plurality" can also be understood as "at least two". "At least one" can be understood as one or more, for example, one, two or more. For example, including at least one means including one, two or more, and there is no limit on which ones are included. For example, including at least one of A, B and C, then A, B, C, A and B, A and C, B and C, or A, B and C can be included.

[0044] It should be noted that, in the embodiments of the present application, "and / or" describes the association relationship of the associated objects, indicating that three relationships may exist. For example, A and / or B may represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / ", unless otherwise specified, generally indicates that the associated objects before and after are in an "or" relationship.

[0045] As used herein, the description of “a1-a2” means “greater than or equal to a1” and “less than or equal to a2”, for example, x is 0-1, that is: 0≤x≤1.

[0046] An embodiment of the present application provides a method for preparing basic zinc chloride, wherein zinc chloride and calcium hydroxide are stirred and reacted in a liquid medium in the presence of ammonium chloride to obtain basic zinc chloride particles.

[0047] Wherein, ammonium chloride, zinc chloride and calcium hydroxide are dissolved in a liquid medium to form a solution. For example, the liquid medium can be water. The reaction equation for preparing basic zinc chloride by reacting zinc chloride with calcium hydroxide is shown in formula (I):

[0048] 5ZnCl2+4Ca(OH)2+H2O=Zn5(OH)8Cl2·H2O↓+4CaCl2(I).

[0049] Among them, ammonium chloride is used to regulate the crystal shape of the basic zinc chloride (Zn5(OH)8Cl2·H2O) generated by the reaction, which can increase the particle size of the prepared basic zinc chloride particles. In addition, in the presence of ammonium chloride, the prepared basic zinc chloride particles have good fluidity and less dust.

[0050] The applicant has found that in the presence of ammonium chloride, the particle size of the prepared basic zinc chloride particles is larger, and they exhibit good fluidity and less dust.

[0051] The applicant speculates that one of the mechanisms by which ammonium chloride regulates the crystal form of basic zinc chloride may be as follows: at the moment when calcium hydroxide is added, in addition to the main reaction of formula (I), a reversible chemical reaction of "dissolution-reprecipitation" as shown in formula (II) will also occur on the surface of the previously generated basic zinc chloride microcrystals, in which basic zinc chloride, calcium hydroxide and ammonium chloride participate, so that the small particles of basic zinc chloride crystals gradually grow.

[0052]

[0053] The applicant does not exclude the possibility that ammonium chloride may regulate the crystal form of basic zinc chloride, and that there may be other involvement of at least one physical reaction process and / or chemical reaction process.

[0054] Those skilled in the art should understand that the above-mentioned applicant's speculation on the mechanism of ammonium chloride regulating the crystal form of basic zinc chloride cannot constitute a limitation on the protection scope of this application. It is only one of the ways for ammonium chloride to regulate the crystal form of basic zinc chloride. There may be other physical reaction processes and / or chemical reaction processes in the way that ammonium chloride regulates the crystal form of basic zinc chloride. All schemes that increase the particle size of basic zinc chloride particles by adding ammonium chloride are within the protection scope of this application.

[0055] As an embodiment, in the reaction of zinc chloride and calcium hydroxide to generate basic zinc chloride, the stirring speed is 30 to 100 r / min, the reaction temperature is 70 to 95° C., and the reaction pH is 5.5 to 6.5.

[0056] As an embodiment, the preparation method of basic zinc chloride specifically comprises the following steps:

[0057] S11) adding ammonium chloride as a crystal control agent to the zinc chloride solution to obtain a zinc chloride working solution with an ammonia nitrogen concentration of 2 to 10 g / L.

[0058] The zinc concentration in the zinc chloride solution is 50-150 g / L, and the ammonium chloride used as the crystal shape control agent can be solid ammonium chloride or a saturated ammonium chloride solution. + ), free ammonia (NH3) and zinc ammine complex ion (Zn(NH3)2 2+ ) and other forms of nitrogen.

[0059] Among them, controlling the ammonia nitrogen concentration in the zinc chloride working solution to 2-10 g / L is beneficial to simultaneously increasing the size of the basic zinc chloride particles and improving the purity of the basic zinc chloride particles.

[0060] S12) under stirring, the zinc chloride working solution and the calcium hydroxide suspension are mixed and reacted to obtain basic zinc chloride particles.

[0061] Wherein, the zinc chloride working solution and the calcium hydroxide suspension flow into the reaction vessel in parallel under stirring conditions, which is conducive to maintaining the relative stability of the pH value of the reaction system and providing an environment with a relatively stable pH value for the crystal growth of basic zinc chloride. In this step, the zinc chloride working solution and the calcium hydroxide suspension are mixed quickly and evenly by feeding and stirring at the same time.

[0062] Wherein, the mass fraction of calcium hydroxide in the calcium hydroxide suspension is 10-30%.

[0063] In this embodiment, the zinc chloride solution and the calcium hydroxide suspension can be provided separately.

[0064] Exemplarily, the calcium hydroxide suspension is prepared by the following method: it is prepared with calcium hydroxide that meets the quality standard of "Food Additive Calcium Hydroxide" (GB25572-2010), or it is prepared with calcium hydroxide that meets the quality standard of "Industrial Calcium Hydroxide" (HG / T 4120-2009) for superior products.

[0065] Illustratively, the zinc chloride solution is prepared by the following method: using solid zinc chloride that meets the quality standard of "Industrial Zinc Chloride" (HG / T2323-2019) and has arsenic and cadmium contents of no more than 3 mg / kg; or using zinc oxide as raw material, dissolving it in hydrochloric acid and removing impurities.

[0066] In some embodiments, in step S12, the zinc chloride working solution and the calcium hydroxide suspension are mixed and reacted under stirring to obtain basic zinc chloride particles, which specifically includes the following steps:

[0067] S21) adding a base liquid into a reaction vessel;

[0068] Before the zinc chloride working solution and the calcium hydroxide suspension flow in, the base liquid is added first, and the stirring paddle stirs in the base liquid to provide a rotating environment, which can ensure that the zinc chloride working solution and the calcium hydroxide suspension are mixed in time and evenly after flowing in. For example, in an actual reaction scenario, the amount of base liquid added is sufficient to stir and immerse the pH meter probe.

[0069] The base liquid may include water; or, the base liquid may include the first filtrate obtained in the subsequent step S23; or, the base liquid may include water and the first filtrate mixed in any proportion.

[0070] S22) under stirring, adding zinc chloride working solution and calcium hydroxide suspension into the reaction vessel in a parallel flow feeding mode simultaneously, so that the zinc chloride working solution and the calcium hydroxide suspension are mixed and reacted to obtain a reaction solution;

[0071] Among them, the parallel flow feeding method is conducive to maintaining the relative stability of the pH value of the reaction system, and provides an environment with a relatively stable pH value for the crystal growth of basic zinc chloride.

[0072] S23) aging the reaction solution, and filtering the aged reaction solution to obtain basic zinc chloride precipitate and a first filtrate respectively;

[0073] Among them, during the aging process, Ostwald ripening may occur in the growth process of basic zinc chloride crystals, that is, the process in which smaller crystalline particles in the solute dissolve and redeposit on larger crystalline particles. Ostwald ripening can promote the aggregation and growth of small basic zinc chloride particles.

[0074] For example, the aging time may be 30 min to 120 min. The first filtrate includes unreacted zinc chloride.

[0075] S24) drying the basic zinc chloride precipitate to obtain basic zinc chloride particles;

[0076] The basic zinc chloride precipitate may be washed (for example, with water) first, and then the washed precipitate is heat-dried to obtain basic zinc chloride particles.

[0077] In this embodiment, the prepared basic zinc chloride particles have a larger particle size, exhibit good fluidity, and generate less dust.

[0078] The prepared basic zinc chloride has a large particle size, so it has a technical effect of good fluidity. Since the specific surface area of ​​the powder is inversely proportional to the particle size, the smaller the powder particle size, the larger the specific surface area. As the powder particle size decreases, the molecular attraction and electrostatic attraction between the powders gradually increase, reducing the fluidity of the powder particles; secondly, the smaller the powder particle size, the easier it is for the particles to adsorb and aggregate into agglomerates, the greater the adhesion, resulting in an increase in the angle of repose and poor fluidity.

[0079] The prepared basic zinc chloride has less dust content, so it has the technical effect of less dust. Dust refers to solid particles that can be suspended in the air for a long time. The particle size of the particles will affect the time they stay in the air. Generally speaking, the smaller the particle size of the particles, the longer they stay in the air. This is because small particles are more affected by the collision and diffusion of gas molecules, resulting in a slower movement speed in the air. In contrast, large particles are less affected by gas molecules, move faster, and therefore stay for a shorter time.

[0080] An embodiment of the present application provides basic zinc chloride particles, which are prepared by the above-mentioned preparation method of basic zinc chloride.

[0081] In this embodiment, the particle size of the basic zinc chloride particles is less than 40 meshes, and the mass percentage of particles with a particle size less than 200 meshes in the basic zinc chloride particles is less than 10%. In addition, the basic zinc chloride particles do not contain a binder.

[0082] In this embodiment, the product quality indicators except "fineness" all meet the requirements of "Feed Additive Basic Zinc Chloride" (GB / T 22546-2008), and the calcium content is not more than 0.50% (mass fraction), and the ammonia nitrogen content is not more than 0.20% (mass fraction).

[0083] One embodiment of the present application provides a method for preparing basic zinc chloride particles and producing calcium chloride solution as a by-product. Figure 1 As shown, the method for preparing basic zinc chloride particles and producing calcium chloride solution as a by-product comprises the following steps:

[0084] S31) adding ammonium chloride as a crystal control agent to the zinc chloride solution to obtain a zinc chloride working solution with an ammonia nitrogen concentration of 2 to 10 g / L;

[0085] S32) under stirring, adding zinc chloride working solution and calcium hydroxide suspension into the reaction vessel in a parallel flow feeding mode, so that the zinc chloride working solution and the calcium hydroxide suspension are mixed and reacted to obtain a first reaction solution;

[0086] S33) aging the first reaction solution, filtering the aged first reaction solution to obtain basic zinc chloride precipitate and a first filtrate respectively; drying the basic zinc chloride precipitate to obtain basic zinc chloride particles;

[0087] Steps S31 to S33 can refer to the corresponding description of the above embodiment, such as the description of step S11 and step S12 and the description of step S21 to step S24, which will not be repeated here. As an embodiment, the stirring speed of the zinc chloride working solution and the calcium hydroxide suspension for the mixed reaction is 30 to 100 r / min, the reaction temperature is 70 to 95° C., and the reaction pH value is 5.5 to 6.5. As an embodiment, the aging time of the first reaction solution is 30 min to 120 min.

[0088] S34) adding the first filtrate into the reaction container, adding the calcium hydroxide suspension into the reaction container under stirring, reacting the first filtrate and the calcium hydroxide suspension to obtain a second reaction solution, filtering the second reaction solution to obtain zinc hydroxide mud and a second filtrate respectively.

[0089] After the first filtrate is added to the reaction container, the pH meter probe is immersed therein, and then the calcium hydroxide suspension is added, while feeding and stirring. The first filtrate includes unreacted zinc chloride. The reaction equation for the reaction of zinc chloride contained in the first filtrate with calcium hydroxide to obtain zinc hydroxide mud is shown in formula (III):

[0090] Ca(OH)2+ZnCl2=Zn(OH)2↓+CaCl2(III).

[0091] The mass fraction of calcium hydroxide in the added calcium hydroxide suspension is 10-30%.

[0092] The end point of the reaction between the first filtrate and the calcium hydroxide suspension is a pH value of 10 to 12.

[0093] S35) adding the second filtrate into the reaction container, and under stirring, adding a sodium sulfide solution with a mass fraction of 5 to 15% into the reaction container, allowing the second filtrate and the sodium sulfide solution to react to obtain a third reaction liquid, filtering the third reaction liquid to respectively obtain zinc sulfide mud and a third filtrate, and evaporating and concentrating the third filtrate to obtain a concentrated solution.

[0094] The sodium sulfide solution is added while feeding and stirring. The second filtrate includes unreacted zinc chloride. The reaction equation for the zinc chloride contained in the second filtrate to react with sodium sulfide to obtain zinc sulfide mud is shown in formula (IV):

[0095] ZnCl2+Na2S=ZnS↓+2NaCl(IV).

[0096] The zinc content of the third filtrate is less than 1 mg / kg. The third filtrate can be concentrated by evaporation under reduced pressure or normal pressure, and the evaporation temperature can be 40-120° C. The obtained concentrated solution has a calcium chloride content of 20%-40% and contains a small amount of ammonia nitrogen, and evaporated condensed water is obtained at the same time.

[0097] The end point of the reaction between the second filtrate and the sodium sulfide solution is when no more white precipitate is produced.

[0098] S36) adding the concentrated solution into the reaction container, and adding the bleaching powder or bleaching spirit into the reaction container under stirring, so that the concentrated solution and the bleaching powder or bleaching spirit react to obtain a fourth reaction solution, and filtering the fourth reaction solution to obtain calcium-containing filter mud and calcium chloride solution respectively.

[0099] The first filtrate, the second filtrate, the third filtrate and the concentrated solution contain ammonia nitrogen respectively. The main components of the bleaching spirit or bleaching powder are (i) calcium hypochlorite or (ii) calcium hypochlorite and calcium chloride, and the effective component of the bleaching powder or bleaching spirit is calcium hypochlorite. The reaction equation for obtaining calcium chloride by the reaction of ammonia nitrogen contained in the concentrated solution with calcium hypochlorite contained in the bleaching powder or bleaching spirit is shown in Formula (V):

[0100] 3Ca(ClO)2+4NH3=3CaCl2+2N2↑+6H2O(V).

[0101] The mass ratio of chlorine element to nitrogen element in the reaction solution formed by the concentrated solution and the bleaching powder or bleaching essence is 15:1.

[0102] In step S36, the material is fed and stirred at the same time, and stirring is continued for 30 min to 60 min after the feeding is completed; a small amount of calcium-containing filter mud and a fourth filtrate are obtained by filtration, and the fourth filtrate can be directly used as a by-product calcium chloride solution. The calcium chloride content in the calcium chloride solution is 20% to 40%, the zinc content is not more than 3 mg / kg, and the ammonia nitrogen content is not more than 15 mg / kg.

[0103] In this embodiment, zinc chloride solution containing a small amount of ammonium chloride and calcium hydroxide suspension are used as raw materials, which are fed in parallel and heated to synthesize a feed additive basic zinc chloride granule product that meets national standards, has good fluidity and less dust. The product can be used as a high-quality zinc supplement in the field of feed production.

[0104] In this embodiment, the waste liquid generated by the preparation of basic zinc chloride is treated through a series of steps such as secondary zinc precipitation with calcium hydroxide, deep zinc removal with sodium sulfide, evaporation concentration and ammonia nitrogen removal by inflection point chlorination to obtain a calcium chloride solution product that meets national standards, thereby realizing the resource utilization of the waste liquid from the production of basic zinc chloride.

[0105] An embodiment of the present application provides basic zinc chloride particles, which are prepared by the above-mentioned method for preparing basic zinc chloride particles and producing calcium chloride solution as a by-product.

[0106] In this embodiment, the particle size of the basic zinc chloride particles is less than 40 mesh (less than 0.450 mm), and the mass percentage of particles with a particle size less than 200 mesh (less than 0.071 mm) in the basic zinc chloride particles is less than 10%. In addition, the basic zinc chloride particles do not contain a binder.

[0107] In this embodiment, the product quality indicators except "fineness" all meet the requirements of "Feed Additive Basic Zinc Chloride" (GB / T 22546-2008), and the calcium content is not more than 0.50% (mass fraction), and the ammonia nitrogen content is not more than 0.20% (mass fraction).

[0108] An embodiment of the present application provides a calcium chloride solution, which is prepared by the above-mentioned method of preparing basic zinc chloride particles and producing calcium chloride solution as a by-product.

[0109] In this embodiment, the product quality of the calcium chloride solution meets the index requirements of the calcium chloride solution product in "Industrial Calcium Chloride" (GB / T 26520-2021), wherein the calcium chloride content in the calcium chloride solution is 20% to 40%, the zinc content is not more than 3 mg / kg, and the ammonia nitrogen content is not more than 15 mg / kg.

[0110] Example 1

[0111] The basic zinc chloride particles of this embodiment are prepared by the following method:

[0112] Analytical grade zinc chloride, ammonium chloride and purified water were prepared into 1500 ml of zinc chloride working solution containing 150 g / L zinc and 10 g / L ammonia nitrogen. Analytical grade calcium hydroxide and purified water were prepared into 2500 g of suspension containing 10% of zinc. Then 150 ml of distilled water was added to a 5-liter four-necked glass flask and placed in a constant temperature water bath. A stirring paddle, a pH meter, a thermometer, a zinc chloride working solution and a calcium hydroxide suspension feeding tube were installed respectively. The stirring device was turned on and the The temperature was raised to 98°C, and then the zinc chloride working solution and the calcium hydroxide suspension were added to the four-necked flask in parallel, and the reaction pH was controlled at 5.5-5.8, the temperature was 93-95°C, and the stirring speed was 100r / min; after the addition was completed, the mixture was aged for 30 minutes, and the precipitate and the primary filtrate 3042ml were filtered; the precipitate was washed, placed in a 105°C oven and dried to constant weight, and all passed through a 40-mesh sieve, and finally 339.0g of the basic chloride product was obtained. All the finished products were sieved with 60-mesh, 80-mesh, 100-mesh, 150-mesh, and 200-mesh nylon sieves, and the size distribution data of the basic zinc chloride particles are shown in Table 1 below. In addition, the finished product has good fluidity and little dust.

[0113] The crystal composition and structure of the finished product are tested by XRD method. Figure 2 As shown, the XRD spectrum of the finished product is consistent with the standard spectrum, and it can be determined that the finished product is basic zinc chloride. At the same time, the finished product was tested with reference to the national standard GB / T 22546-2008, and the test results were: zinc content 59.7%, chlorine content 12.8%, water-soluble chloride 0.11%, arsenic content less than 2mg / kg, lead content less than 0.9mg / kg, cadmium content less than 0.09mg / kg, which meets the national standard for feed-grade basic zinc chloride; calcium content 0.09%, ammonia nitrogen content 0.03%, which meets the company's internal control standards.

[0114] Table 1 Size distribution of granular basic zinc chloride (pH 5.5-5.8)

[0115] pH 5.5~5.8 40~60 mesh 60~80 mesh 80~100 mesh 100~150 mesh 150~200 mesh <200th total Weight g 0.00 0.75 78.23 98.56 127.52 33.94 339.0 Proportion 0.0% 0.2% 23.1% 29.1% 37.6% 10.0% 100%

[0116] The calcium chloride solution of the present embodiment is prepared as follows:

[0117] First, 3000ml of the primary filtrate was added to a 5-liter beaker, 10% calcium hydroxide suspension was added to pH 12 under stirring, and 105g of zinc hydroxide mud and 3288ml of secondary filtrate were obtained by filtration. Then, 3250ml of the secondary filtrate was added to a 5-liter beaker, 15% sodium sulfide solution was added dropwise under stirring until no new white precipitate was produced, and 4.36g of zinc sulfide mud and 3250ml of tertiary filtrate were obtained by filtration. Then, 3200ml of the tertiary filtrate was added to an atmospheric distillation bottle, placed in an oil bath at 120°C for evaporation and concentration, and 768ml of calcium chloride concentrated solution was obtained. Finally, 750ml of the concentrated solution was added to a 1-liter beaker, and 65% of available chlorine was added according to the chlorine-nitrogen ratio = 15 (weight ratio), and filtered after stirring for 30min to obtain 1037g of calcium chloride solution and 0.13g of calcium-containing filter mud.

[0118] The calcium chloride solution was tested in accordance with the national standard GB / T 26520-2021, and the measurement results were: calcium chloride content was 39.6%, alkalinity was 0.05%, total alkali metal chloride was 0.18%, sulfate was 0.01%, and total magnesium was 0.04%, which met the national standard for calcium chloride solution; zinc content was 2.51 mg / kg, and ammonia nitrogen content was 8.2 mg / kg, which met the company's internal control standards.

[0119] Example 2

[0120] The basic zinc chloride particles of this embodiment are prepared by the following method:

[0121] Industrial-grade zinc chloride, industrial-grade ammonium chloride and tap water are prepared into 30L of zinc chloride working solution containing 100g / L zinc and 5g / L ammonia nitrogen, and food-grade calcium hydroxide and tap water are prepared into 15kg of suspension with a content of 20%; then 3L of 10% calcium chloride solution is added into a 50-liter glass reactor as a simulated primer, and a stirring paddle, a pH meter, a thermometer, a zinc chloride working solution and a calcium hydroxide suspension feeding pipe are installed respectively; the stirring device is turned on, and the temperature of the oil bath heating system is increased to 90°C at the same time, and the zinc chloride working solution and the calcium hydroxide suspension are added into the reactor in a parallel flow manner, the reaction pH is controlled at 5.9-6.1, the temperature is 80-82°C, and the stirring speed is 60r / min. After the addition is completed, it is aged for 60min, and a precipitate and a primary filtrate of 38.24L are obtained by filtering; the precipitate is washed, placed in a 105°C oven in batches to dry to constant weight, and all are sieved through a 40-mesh sieve to finally obtain 4750g of a finished product. 300g of the finished product was uniformly sampled and sieved with 60 mesh, 80 mesh, 100 mesh, 150 mesh and 200 mesh nylon sieves respectively. The particle size distribution data is shown in Table 2. At the same time, the finished product has good fluidity and little dust.

[0122] The crystal composition and structure of the finished product were tested by XRD detection method. The XRD spectrum of the finished product was consistent with the standard spectrum, which confirmed that the finished product was basic zinc chloride. At the same time, the finished product was tested with reference to the national standard GB / T 22546-2008. The test results were: zinc content 60.2%, chlorine content 12.1%, water-soluble chloride 0.15%, arsenic content less than 2mg / kg, lead content less than 0.9mg / kg, cadmium content less than 0.09mg / kg, which met the national standard for feed-grade basic zinc chloride; calcium content 0.19%, ammonia nitrogen content 0.06%, which met the internal control standards of the enterprise.

[0123] Table 2 Size distribution of granular basic zinc chloride (pH 5.9-6.1)

[0124] pH 5.9~6.1 40~60 mesh 60~80 mesh 80~100 mesh 100~150 mesh 150~200 mesh <200th total Weight g 0.00 23.91 202.85 35.90 23.34 14.00 300 Proportion 0.0% 8.0% 67.6% 12.0% 7.8% 4.7% 100%

[0125] The calcium chloride solution of the present embodiment is prepared as follows:

[0126] First, pour 38.0L of the primary filtrate back into a 50-liter glass reactor, add 20% calcium hydroxide suspension to pH 11 under stirring, and filter to obtain 686g of zinc hydroxide mud and 38.7L of secondary filtrate. Next, pour 38.5L of the secondary filtrate back into a 50-liter glass reactor, add 10% sodium sulfide solution under stirring until no new white precipitate is produced, and filter to obtain 26.93g of zinc sulfide mud and 38.5L of tertiary filtrate. Then, repeat the above steps of basic zinc chloride preparation, secondary zinc precipitation and deep zinc removal three times to obtain 154L of tertiary filtrate; pump 154L of tertiary filtrate into a low-temperature evaporator, evaporate and concentrate at 40-41°C to obtain 53.6L of calcium chloride concentrate. Finally, 53.5 L of concentrated solution was added to a 100 L PP plastic barrel, and 35% bleaching powder with available chlorine was added according to the chlorine-nitrogen ratio = 15 (weight ratio). After stirring for 60 min, the mixture was filtered to obtain 69.1 kg of calcium chloride solution and 43.0 g of calcium-containing filter mud.

[0127] The calcium chloride solution was tested in accordance with the national standard GB / T 26520-2021, and the measurement results were: calcium chloride content was 31.2%, alkalinity was 0.06%, total alkali metal chloride was 0.31%, sulfate was 0.02%, and total magnesium was 0.19%, which met the national standard for calcium chloride solution; zinc content was 1.98 mg / kg, and ammonia nitrogen content was 3.5 mg / kg, which met the company's internal control standards.

[0128] Example 3

[0129] The basic zinc chloride particles of this embodiment are prepared by the following method:

[0130] Use industrial hydrochloric acid to dissolve zinc oxide and remove impurities to prepare zinc chloride solution, add industrial ammonium chloride and tap water to prepare 6000 liters of zinc chloride working solution containing 50g / L zinc and 2g / L ammonia nitrogen, and add industrial-grade high-quality calcium hydroxide and tap water to prepare 1000kg of suspension with 30% content. 3600L of 10% calcium chloride solution was added to the enamel reactor as a simulated primer, and an industrial online pH meter, an online thermometer, a zinc chloride working solution and a calcium hydroxide suspension feeding pipe were installed respectively; the stirring device was turned on, and steam was passed through the jacket at the same time to heat the primer to 90°C, and then the zinc chloride working solution and the calcium hydroxide suspension were added to the reactor in parallel, and the reaction pH was controlled at 6.3-6.5, the temperature was 70-75°C, and the stirring speed was 30r / min. After the addition was completed, the reaction was aged for 120min, and the precipitate and the primary filtrate 6630L were filtered; the precipitate was washed and dried with an air flow dryer to a moisture content of less than 1%, and all were sieved through a 40-mesh sieve, and finally 485kg of the finished product was obtained. 500g of the finished product was uniformly sampled and sieved with 60-mesh, 80-mesh, 100-mesh, 150-mesh, and 200-mesh nylon sieves, and the particle size distribution data were shown in Table 3 below. At the same time, the finished product has good fluidity and less dust.

[0131] The crystal composition and structure of the finished product were tested by XRD detection method. The XRD spectrum of the finished product was consistent with the standard spectrum, which confirmed that the finished product was basic zinc chloride. At the same time, the finished product was tested with reference to the national standard GB / T 22546-2008. The test results were: zinc content 59.6%, chlorine content 12.3%, water-soluble chloride 0.25%, arsenic content less than 2mg / kg, lead content less than 0.9mg / kg, cadmium content less than 0.09mg / kg, which met the national standard for feed-grade basic zinc chloride; calcium content 0.15%, ammonia nitrogen content 0.03%, which met the internal control standards of the enterprise.

[0132] Table 3 Size distribution of granular basic zinc chloride (pH 6.2-6.5)

[0133] pH 6.2~6.5 40~60 mesh 60~80 mesh 80~100 mesh 100~150 mesh 150~200 mesh <200th total Weight g 0.50 8.63 35.21 142.64 269.82 43.20 500 Proportion 0.1% 1.7% 7.0% 28.5% 54.0% 8.6% 100%

[0134] The calcium chloride solution of the present embodiment is prepared as follows:

[0135] First, pour the primary filtrate 6620L back to the 10m 3 In the enameled reactor, 30% calcium hydroxide suspension was added to pH 10 under stirring, and 32.6 kg of zinc hydroxide mud and 6630 L of secondary filtrate were obtained by filtration. Then, the secondary filtrate 6630 L was poured back into the 10m 3 In the enameled reactor, add 5% sodium sulfide solution under stirring until no new white precipitate is produced, and filter to obtain 4.50 kg of zinc sulfide mud and 6650 liters of tertiary filtrate. Pump 6650 L of tertiary filtrate into the MVR evaporator, evaporate and concentrate at 95-100 ° C to obtain 2200 L of calcium chloride concentrate. Finally, add 5m 3In a glass fiber reinforced plastic reactor, 35% effective chlorine bleaching powder was added according to the chlorine-nitrogen ratio = 15 (weight ratio), and the mixture was stirred for 60 minutes and then filtered to obtain 2601 kg of calcium chloride solution and 1.20 kg of calcium-containing filter mud.

[0136] The calcium chloride solution was tested in accordance with the national standard GB / T 26520-2021, and the measurement results were: calcium chloride content was 20.8%, alkalinity was 0.04%, total alkali metal chloride was 0.14%, sulfate was 0.01%, and total magnesium was 0.11%, which met the national standard for calcium chloride solution; zinc content was 2.09 mg / kg, and ammonia nitrogen content was 12.1 mg / kg, which met the company's internal control standards.

[0137] Comparative Example 1

[0138] The basic zinc chloride powder of this comparative example was prepared by the following method:

[0139] Analytical pure zinc chloride and pure water are prepared into 1000 ml of zinc chloride working solution containing 180 g / L of zinc, and analytical pure calcium hydroxide and pure water are prepared into 3500 g of suspension with a content of 5%; then 150 ml of pure water is added to a 5-liter four-necked glass flask and placed in a constant temperature water bath, and a stirring paddle, a pH meter, a thermometer, and a zinc chloride working solution and a calcium hydroxide suspension feeding tube are installed respectively; the stirring device is turned on, and the temperature is raised to 65° C. at the same time, and then the zinc chloride working solution and the calcium hydroxide suspension are added to the four-necked flask in a parallel flow manner, and the reaction pH is controlled at 6.7-7.0, the temperature is 50-52° C., and the stirring speed is 100 r / min; after the addition is completed, it is aged for 60 minutes, and a precipitate and a primary filtrate of 3968 ml are obtained by filtering; the precipitate is washed, placed in a 105° C. oven to dry to constant weight, and all are sieved through a 40-mesh sieve, and finally 292.1 g of a finished product is obtained. All finished products were sieved with 60 mesh, 80 mesh, 100 mesh, 150 mesh and 200 mesh nylon screens, and the particle size distribution data of basic zinc chloride are shown in Table 4. In addition, the finished product has poor fluidity and large dust.

[0140] The crystal composition and structure of the finished product were tested by XRD detection method. The XRD spectrum of the finished product was consistent with the standard spectrum, and it can be determined that the finished product is basic zinc chloride. At the same time, the finished product was tested with reference to the national standard GB / T 22546-2008. The test results are: zinc content 60.3%, chlorine content 12.1%, water-soluble chloride 0.55%, arsenic content less than 2mg / kg, lead content less than 0.9mg / kg, cadmium content less than 0.09mg / kg, which meets the national standard for feed-grade basic zinc chloride.

[0141] Table 4 Size distribution of powdered basic zinc chloride (pH 6.7-7.0)

[0142] pH 6.7-7.0 40~60 mesh 60~80 mesh 80~100 mesh 100~150 mesh 150~200 mesh <200th total Weight g 0.00 0.00 5.67 2.98 26.85 256.61 292.10 Proportion 0.0% 0.0% 1.9% 1.0% 9.2% 87.8% 100%

[0143] Comparative Example 2

[0144] The basic zinc chloride powder of this comparative example was prepared by the following method:

[0145] Analytical pure zinc chloride and pure water are prepared into 3000 ml of zinc chloride working solution containing 40 g / L of zinc, and analytical pure calcium hydroxide and pure water are prepared into 350 g of suspension with a content of 34%; then 150 ml of pure water is added to a 5-liter four-necked glass flask and placed in a constant temperature oil bath, and a stirring paddle, a pH meter, a thermometer, and a zinc chloride working solution and a calcium hydroxide suspension feeding tube are installed respectively; the stirring device is turned on, and the temperature is raised to 110° C. at the same time, and then the zinc chloride working solution and the calcium hydroxide suspension are added to the four-necked flask in a parallel flow manner, and the reaction pH is controlled at 5.0-5.2, the temperature is 98-100° C., and the stirring speed is 100 r / min; after the addition is completed, it is aged for 60 minutes, and a precipitate and a primary filtrate of 3173 ml are obtained by filtering; the precipitate is washed, placed in a 105° C. oven to dry to constant weight, and all are sieved through a 40-mesh sieve, and finally 149.5 g of a finished product is obtained. All finished products were screened with 60 mesh, 80 mesh, 100 mesh, 150 mesh and 200 mesh nylon screens, and the particle size distribution data of basic zinc chloride are shown in Table 5. In addition, the finished product has poor fluidity and large dust.

[0146] The crystal composition and structure of the finished product were tested by XRD detection method. The XRD spectrum of the finished product was consistent with the standard spectrum, and it can be determined that the finished product is basic zinc chloride. At the same time, the finished product was tested with reference to the national standard GB / T 22546-2008. The test results are: zinc content 58.1%, chlorine content 12.8%, water-soluble chloride 0.37%, arsenic content less than 2mg / kg, lead content less than 0.9mg / kg, cadmium content less than 0.09mg / kg, which meets the national standard for feed-grade basic zinc chloride.

[0147] Table 5 Size distribution of powdered basic zinc chloride (pH 5.0-5.2)

[0148] pH 5.0~5.2 40~60 mesh 60~80 mesh 80~100 mesh 100~150 mesh 150~200 mesh <200th total Weight g 0.00 1.13 18.14 18.35 19.95 91.92 149.50 Proportion 0.0% 0.8% 12.1% 12.3% 13.3% 61.5% 100%

[0149] According to Tables 1 to 5, the particle size distributions of the basic zinc chloride particles prepared in Example 1, Example 2 and Example 3 are superior to the particle size distributions of the basic zinc chloride particles prepared in Comparative Example 1 and Comparative Example 2, respectively.

[0150] The above is only an implementation method of the present application. It should be pointed out that a person skilled in the art can make improvements without departing from the inventive concept of the present application, but these improvements are within the scope of protection of the present application.

Claims

1. A method for preparing basic zinc chloride, characterized in that: In a liquid medium, zinc chloride and calcium hydroxide are stirred and reacted in the presence of ammonium chloride to obtain basic zinc chloride particles.

2. The method for preparing basic zinc chloride according to claim 1, wherein The stirring speed is 30-100 r / min, the reaction temperature is 70-95°C, and the reaction pH value is 5.5-6.

5.

3. The preparation method of basic zinc chloride according to claim 1, characterized in that The preparation method of the basic zinc chloride comprises: Adding ammonium chloride as a crystal control agent to a zinc chloride solution with a zinc concentration of 50 to 150 g / L to obtain a zinc chloride working solution with an ammonia nitrogen concentration of 2 to 10 g / L; Under stirring, the zinc chloride working solution and the calcium hydroxide suspension are mixed and reacted to obtain basic zinc chloride particles, wherein the mass fraction of calcium hydroxide in the calcium hydroxide suspension is 10-30%.

4. The method for preparing basic zinc chloride according to claim 3, wherein The crystal shape controlling agent is solid ammonium chloride or saturated ammonium chloride solution; The zinc chloride working solution and the calcium hydroxide suspension are mixed and reacted under stirring to obtain basic zinc chloride particles, including: Adding the base solution to the reaction vessel; Under stirring, the zinc chloride working solution and the calcium hydroxide suspension are simultaneously added into the reaction container in a parallel flow feeding manner, so that the zinc chloride working solution and the calcium hydroxide suspension are mixed and reacted to obtain a reaction solution; Aging the reaction solution, filtering the aged reaction solution to obtain basic zinc chloride precipitate and a first filtrate, respectively, wherein the aging time is 30 min to 120 min; Drying the basic zinc chloride precipitate to obtain the basic zinc chloride particles; Wherein, the base liquid includes water or the first filtrate.

5. A method for preparing basic zinc chloride particles and producing calcium chloride solution as a by-product, characterized in that: include: Adding ammonium chloride as a crystal control agent to the zinc chloride solution to obtain a zinc chloride working solution with an ammonia nitrogen concentration of 2 to 10 g / L; Under stirring, the zinc chloride working solution and the calcium hydroxide suspension are simultaneously added into the reaction container in a parallel flow feeding manner, so that the zinc chloride working solution and the calcium hydroxide suspension are mixed and reacted to obtain a first reaction solution; Aging the first reaction solution, filtering the aged first reaction solution to obtain basic zinc chloride precipitate and a first filtrate respectively; Drying the basic zinc chloride precipitate to obtain basic zinc chloride particles; The first filtrate is added to the reaction container, and under stirring, the calcium hydroxide suspension is added to the reaction container, so that the first filtrate and the calcium hydroxide suspension react to obtain a second reaction solution, and the second reaction solution is filtered to obtain zinc hydroxide mud and a second filtrate respectively; The second filtrate is added to the reaction container, and under stirring, a sodium sulfide solution with a mass fraction of 5 to 15% is added to the reaction container, so that the second filtrate and the sodium sulfide solution react to obtain a third reaction liquid, the third reaction liquid is filtered to obtain zinc sulfide mud and a third filtrate respectively, and the third filtrate is evaporated and concentrated to obtain a concentrated liquid; The concentrated solution is added to the reaction container, and bleaching powder or bleaching spirit is added to the reaction container under stirring, so that the concentrated solution and the bleaching powder or bleaching spirit react to obtain a fourth reaction solution, and the fourth reaction solution is filtered to obtain calcium-containing filter mud and calcium chloride solution respectively.

6. The method for preparing basic zinc chloride particles and producing calcium chloride solution as a byproduct according to claim 5, characterized in that: The stirring speed of the zinc chloride working solution and the calcium hydroxide suspension for the mixed reaction is 30-100 r / min, the reaction temperature is 70-95° C., and the reaction pH value is 5.5-6.5; the aging time of the first reaction solution is 30 min-120 min; and / or, the reaction endpoint of the reaction between the first filtrate and the calcium hydroxide suspension is a pH value of 10 to 12; and / or, the end point of the reaction between the second filtrate and the sodium sulfide solution is that no white precipitate is produced; And / or, the mass ratio of chlorine element to nitrogen element in the reaction solution formed by the concentrated solution and the bleaching powder or bleaching essence is 15:

1.

7. Basic zinc chloride granules prepared by the method for preparing basic zinc chloride according to any one of claims 1 to 4 or the method for preparing basic zinc chloride granules and producing calcium chloride solution as a by-product according to claim 5 or 6.

8. The basic zinc chloride granules according to claim 7, characterized in that The particle size of the basic zinc chloride particles is less than 40 meshes, and the mass percentage of particles with a particle size less than 200 meshes in the basic zinc chloride particles is less than 10%.

9. A calcium chloride solution prepared by the method for preparing basic zinc chloride particles and producing calcium chloride solution as a by-product as claimed in claim 5 or 6.

10. Calcium chloride solution according to claim 9, characterized in that The mass fraction of calcium chloride in the calcium chloride solution is 20% to 40%, the zinc content is less than or equal to 3 mg / kg, and the ammonia nitrogen content is less than or equal to 15 mg / kg.