Preparation method and application of modified sodium vanadium phosphate composite material

By introducing SO4 root and liquid phase contact coating technology into sodium vanadium phosphate, defective structure and local current are formed, the problem of poor conductivity of sodium vanadium phosphate positive electrode material is solved, and the specific capacity and cycle stability of sodium ion batteries are significantly improved. Achieve efficient sodium ion battery performance.

CN118954585AActive Publication Date: 2024-11-15SHANDONG HAIHUA GRP CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411418575.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-11-15
Estimated Expiration
2044-10-12

AI Technical Summary

Technical Problem

The existing sodium vanadium phosphate positive electrode materials have poor conductivity, which affects their capacity release and cycle stability in sodium ion batteries. The existing modification methods may reduce specific capacity or cause cycle stability problems.

Method used

The method of coating of titanium dioxide by substituting multivalent anion for defective defects is adopted. By introducing SO4 roots into sodium vanadium phosphate and forming defective structures, the liquid phase contact coating technology is used to uniformly coat the titanium compound on the surface of the material to form local current and Defect - Hydrogen doped titanium dioxide layer improves the conductivity and cyclic stability of the material.

Benefits of technology

The specific capacity and cycle stability of the positive electrode material of sodium ion battery were significantly improved, and the specific capacity of 102.67mAhg-1 was released at a current density of 20C, and the Coulomb efficiency was maintained at 99.84% after 2300 cycles, avoiding material agglomeration and sintering problems. , enhances the stability and electrochemical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954585A_ABST
    Figure CN118954585A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a modified sodium vanadium phosphate composite material, and belongs to the technical field of preparation of sodium ion battery electrode materials.The preparation method comprises the steps that a chain type carbon source, a vanadium source, ammonium phosphate, ammonium sulfate and a sodium source are added into deionized water to be subjected to a heating reaction, aging and spray drying to generate a Na3V2 (PO4) 3-x (SO4) x precursor material, and the Na3V2 (PO4) 3-x (SO4) x precursor material is obtained; and placing the Na3V2 (PO4) 3-x (SO4) x precursor material, ammonia water and a liquid titanium source in ethanol, carrying out a reaction, carrying out suction filtration, washing and drying to obtain a powder material, and calcining the powder material in an Ar-H2 mixed atmosphere to obtain the modified sodium vanadium phosphate composite material. The modified sodium vanadium phosphate composite material is applied to a sodium ion battery, the specific capacity of 102.67 mAhg <-1 > is released under the current density of 20C in a rate test, and the sodium vanadium phosphate composite material has obvious beneficial effects in the field of quick charge and quick discharge application. After 2300 cycles under the current density of 0.5 C, the specific discharge capacity can still be kept at 100.59 mAhg <-1 >, the coulombic efficiency is 99.84%, and the cycle capacity fading rate is as low as 0.005%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sodium ion battery electrode material preparation, and specifically relates to a preparation method and application of a modified sodium vanadium phosphate composite material. Background Art

[0002] Human development's demand for and dependence on energy is increasing year by year. Large amounts of coal-fired power generation releases large amounts of carbon dioxide, which causes a significant greenhouse effect on the global human living environment and has a serious negative impact on the earth's ecological balance. Therefore, there is a contradiction between supply and demand. In order to balance the urgent demand for energy and the sustainable development of the ecological environment, researchers have proposed a variety of energy storage methods to store intermittent green renewable energy such as wind energy and solar energy. Electrochemical energy storage is divided into lithium battery energy storage, sodium battery energy storage, lead-acid battery energy storage, all-vanadium liquid flow battery energy storage, iron-chromium liquid flow battery energy storage and other energy storage methods.

[0003] Sodium-ion batteries can effectively avoid resource restrictions in other countries due to their abundant reserves and globally averaged resources. Sodium-ion batteries have a high capacity release rate at both high and low temperatures. Energy storage and two-wheeled electric vehicles will become the main application scenarios for sodium-ion batteries. The main technical routes for positive electrode materials for sodium-ion batteries are: layered metal oxides, Prussian blue, and polyanions. Among polyanion materials, sodium vanadium phosphate has the advantages of good thermal stability, strong cycle stability, and mild storage conditions, which has attracted more research from scholars and companies. However, the problem of poor conductivity seriously affects the release of material capacity, and it needs to be effectively modified.

[0004] A Chinese patent document with publication number CN 114156453 B discloses a dual-site doped modified sodium vanadium phosphate positive electrode material, which uses alkali metals to simultaneously replace the Na site and the V site, adjusts the local chemical bonds and electron distribution, and improves the electronic and ionic conductivity. However, replacing the Na and V sites with other elements will reduce the specific capacity, and its cycle stability in this invention is poor.

[0005] A Chinese patent document with publication number CN 115995546 B discloses a sodium vanadium phosphate material with a three-dimensional carbon framework, a preparation method and an application thereof. Carbon nanotubes, carbon materials and ZIF-8 are introduced to form NVP-ZIF / CNTs / C to construct a three-dimensional carbon framework to enhance the electronic conductivity of sodium vanadium phosphate. However, too much carbon material is introduced into the material, and the cycle capacity attenuation rate is large.

[0006] The Chinese patent document with publication number CN 114944479 B discloses a composite material of graphene-composite potassium and silicon-doped sodium vanadium phosphate and its preparation and application. + Partially replace the Na position in sodium vanadium phosphate with Si 4+Partially replace the P position in sodium vanadium phosphate to achieve dual doping of sodium vanadium phosphate to improve the conductivity of sodium vanadium phosphate. The specific capacity released in the rate performance at a current density of 20C is 86mAhg -1 , there is still room for improvement. Summary of the invention

[0007] The method of the present invention aims to provide a preparation method and application of a modified sodium vanadium phosphate composite material, and adopts a method of multivalent anion substitution combined with defective titanium dioxide coating to prepare the modified sodium vanadium phosphate composite material, thereby improving the electronic conductivity and sodium ion diffusion kinetics of the material and optimizing its electrochemical performance.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions: In one aspect, the present invention provides a method for preparing a modified sodium vanadium phosphate composite material, comprising the following steps: (1) Add a chain carbon source, a vanadium source, ammonium phosphate and ammonium sulfate into deionized water, stir and heat to react; add a sodium source to the reacted solution and stir until dissolved to form a homogeneous solution; after aging the homogeneous solution, spray dry it to obtain Na3V2(PO4) 3-x (SO4) x Precursor materials; (2) Na3V2(PO4) 3-x (SO4) x The precursor material and ammonia water are added to ethanol, ultrasonically dispersed, and a liquid titanium source is added dropwise to form a mixed solution, the mixed solution is heated and stirred to react to obtain a suspension, and the suspension is filtered, washed, and dried to obtain a powder material; the powder material is calcined in an Ar-H2 mixed atmosphere to obtain a modified sodium vanadium phosphate composite material (Na3V2(PO4) 3-x (SO4) x @H-TiO2).

[0009] Furthermore, in the step (1), the chain carbon source is one of ascorbic acid, glucose, sucrose, and citric acid; the vanadium source is one of ammonium metavanadate, sodium metavanadate, and hexacarbonyl vanadium; the ammonium phosphate salt is one of ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and ammonium hydrogen phosphate; the ammonium sulfate salt is ammonium hydrogen sulfate or ammonium sulfate; the sodium source is one of sodium carbonate, sodium oxalate, and sodium citrate; Sodium source The molar ratio of sodium, vanadium in the vanadium source, phosphate in the ammonium phosphate salt, and sulfate in the ammonium sulfate salt is 3:2:3-x:x , 0.03≤x≤0.17; the molar volume ratio of the chain carbon source to deionized water is 0.05~0.1mol:2L; the aging time is 5~10h; the spray drying temperature is 110~200℃; the flow rate is 200~300mLh -1 .

[0010] Furthermore, in the step (2), the liquid titanium source is one of tetrabutyl titanate, titanium isopropoxide, and titanium chloride; Na3V2(PO4) 3-x (SO4) x The mass volume ratio of the precursor material and the liquid titanium source is 0.3g~1.0g:0.3mL; the concentration of ammonia water is 25~28wt%; the volume ratio of ammonia water and ethanol is 0.2mL~0.3mL:50mL; the heating temperature is 45°C~65°C, and the stirring time is 10h~15h; the calcination is a two-stage calcination, the first stage calcination temperature is 350°C~450°C, the duration is 2h~4h; the second stage calcination temperature is 700°C~900°C, and the duration is 6h~10h; On the other hand, the present invention also provides an application of the modified sodium vanadium phosphate composite material prepared by the above method, and the modified sodium vanadium phosphate composite material is used as a positive electrode material for a sodium ion battery.

[0011] Compared with the prior art, the technical solution of the present invention has the following beneficial effects: In the prior art, electrode materials usually use other elements to replace Na and V sites. However, since Na and V elements are capacity-contributing elements, replacing them has a certain impact on the theoretical specific capacity. Compared with the prior art, the technical solution of the present invention uses SO4 roots with a similar tetrahedral structure to dope and replace part of the PO4 roots. Under the premise of not affecting the theoretical specific capacity of the electrode material and the stability of the framework structure of the material structure itself, SO4 roots and PO4 roots can be simultaneously present in the material framework structure to form a defect structure and generate local current, thereby effectively improving the conductivity of the material. Compared with the modification method of replacing PO4 roots with single atoms such as F and Cl, the modification method of replacing part of PO4 roots with SO4 roots has clearer substitution sites, which is convenient for precise regulation.

[0012] The technical solution of the present invention is to convert Na3V2(PO4) 3-x (SO4) x Precursor materials, ammonia water, and liquid titanium source are added to ethanol to dissolve to form solution A, so that Na3V2(PO4) 3-x (SO4) x The precursor material and the titanium source are in contact with each other in the liquid phase to increase the Na3V2(PO4) 3-x (SO4) x The diffusion efficiency and compatibility of molecules between the two liquid phases of the precursor dispersion and the titanium source liquid. Using ethanol as a solvent and adding the liquid titanium source drop by drop can reduce the hydrolysis rate of the titanium source and make the titanium compound evenly coated on the Na3V2(PO4) 3-x (SO4) xSurface layer of precursor material; Compared with solid phase contact coating, the liquid phase contact coating adopted in the technical solution of the present invention has the following advantages: first, the amount of coated titanium compound and the thickness of the titanium coating layer are controllable, thereby improving the consistency of the target material and stabilizing the electrochemical properties of the product; second, the uniformity of the titanium compound coating is improved, which not only effectively avoids the problems of material agglomeration and sintering during the calcination process; but also the uniform coating layer on the surface can effectively reduce the loss of active transition metals, avoid side reactions such as electrolyte decomposition, and improve the cycle stability of the material.

[0013] The technical solution of the present invention is to calcine the powder material in an Ar-H2 mixed atmosphere to form a modified sodium iron phosphate pyrophosphate composite material. H2 can not only prevent the iron ions from having multiple valence states and affecting the purity and specific capacity of the target material, but also dope the H element into the titanium dioxide during the calcination process to form a defect-hydrogen doped titanium dioxide coating layer on the surface of the material. There is a part of Ti 4+ and Ti 2+ , local charge flow is formed between ions of different valence states; the material has a carbon network structure inside the bulk phase and a defective titanium dioxide layer on the surface, which can effectively improve the conductivity of the material.

[0014] The technical solution of the present invention effectively improves the reaction kinetics of the modified sodium vanadium phosphate composite material by adopting the dual strategy of bulk doping SO4 roots and external coating of defective titanium dioxide, thereby achieving the effect of optimizing the electrochemical properties of the material.

[0015] The technical solution of the present invention adopts spray drying method to obtain Na3V2(PO4) 3-x (SO4) x The precursor material can obtain a spherical precursor under low energy consumption conditions by adjusting the temperature and flow rate, avoiding the problem of insufficient powder drying and nozzle clogging due to too fast flow rate and low production efficiency due to too slow flow rate.

[0016] The technical solution of the present invention comprises two stages of calcination for calcining the powder material in an Ar-H2 mixed atmosphere. The first stage is calcination at 350°C to 450°C to stabilize the material structure and shape the material morphology. The second stage is high-temperature calcination at 700°C to 900°C to further improve the crystallinity of the material while ensuring the material structure.

[0017] The modified sodium vanadium phosphate composite material was applied to sodium ion batteries. In the rate test, the battery released 102.67 mAh g at a current density of 20C. -1 The specific capacity of the battery can still be maintained at 100.59 mAh g after 2300 cycles at a current density of 0.5C. -1 , the Coulomb efficiency is 99.84%. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1Na3V2(PO4) obtained in Example 1 3-x (SO4) x SEM morphology of the precursor material at a magnification of 882 times; Figure 2 The modified sodium vanadium phosphate composite material (Na3V2(PO4) 2.91 (SO4) 0.08 @H-TiO2) SEM morphology at 7510 times magnification under scanning electron microscope; Figure 3 The modified sodium vanadium phosphate composite material (Na3V2(PO4) 2.91 (SO4) 0.08 @H-TiO2) XRD diffraction pattern; Figure 4 The modified sodium vanadium phosphate composite material (Na3V2(PO4) 2.91 (SO4) 0.08 @H-TiO2) is used as a cathode material in sodium-ion batteries, and its rate performance at different current densities; Figure 5 The modified sodium vanadium phosphate composite material (Na3V2(PO4) 2.91 (SO4) 0.08 @H-TiO2) is used as a positive electrode material in sodium-ion batteries and its cycling performance at a current density of 0.5C. DETAILED DESCRIPTION

[0019] The present invention is further described in detail below in conjunction with the embodiments. The drawings and embodiments of the specification are only used to explain the present invention and do not constitute an improper limitation of the present invention. It should be noted that the ammonia water used in the following embodiments is Commercially available reagent, containing 25~28wt% ammonia. Example 1

[0020] (1) Add 0.05 mol of citric acid, 1.2 mol of ammonium metavanadate, 1.75 mol of ammonium dihydrogen phosphate and 0.05 mol of ammonium hydrogen sulfate to 2 L of deionized water, and heat and stir at 60 °C to react; add 0.9 mol of sodium carbonate to the reaction solution and stir until dissolved to form a homogeneous solution. After aging at 80 °C for 10 h, heat at 110 °C, 200 mL / h -1 Na3V2(PO4) was obtained by spray drying under the conditions of 2.91 (SO4) 0.08 Precursor materials; (2) 0.3g Na3V2(PO4) 2.91 (SO4) 0.08The precursor material and 0.2 mL 25-28 wt% ammonia water were added to 50 mL ethanol, ultrasonically dispersed for 15 min, and 0.3 mL tetrabutyl titanate was added dropwise, heated and stirred at 45 ° C for 15 h to obtain a suspension, which was filtered, washed and dried to obtain a powder material; the powder material was calcined in an Ar-H2 mixed atmosphere, first at 350 ° C for 4 h, and then at 800 ° C for 8 h, to finally obtain Na3V2(PO4) 2.91 (SO4) 0.08 @H-TiO2 composite material, that is, modified sodium vanadium phosphate composite material.

[0021] like Figure 1 As shown, the technical solution of Example 1 uses SO4 roots with a similar tetrahedral structure to dope and replace part of PO4 roots. Under the premise of not affecting the theoretical specific capacity of the electrode material and the stability of the framework structure of the material structure itself, SO4 roots and PO4 roots can be simultaneously present in the material framework structure to form a defect structure and form a local current, effectively improving the conductivity of the material. Na3V2(PO4) prepared in Example 1 2.91 (SO4) 0.08 The precursor material is a micron-sized spherical material. The amount of the coated titanium compound and the thickness of the titanium coating layer are controllable, which improves the consistency and coating uniformity of the target material. The modified sodium vanadium phosphate composite material is obtained after calcination. Figure 2 The material is shown in Figure 2. Figure 3 As shown, the successful synthesis of the modified sodium vanadium phosphate composite material is confirmed. The dual strategy of bulk doping and external coating of defective titanium dioxide not only effectively avoids the problems of material agglomeration and sintering during the calcination process, but also the uniform coating layer on the surface can effectively reduce the loss of active transition metals, avoid side reactions such as electrolyte decomposition, and improve the cyclic stability of the material. The technical solution of the present invention effectively improves the reaction kinetics of the modified sodium vanadium phosphate composite material by adopting the dual strategy of bulk doping of SO4 roots and external coating of defective titanium dioxide, thereby achieving the effect of optimizing the electrochemical properties of the material. The modified sodium vanadium phosphate composite material prepared in Example 1 was used as a positive electrode in a sodium ion battery, and the rate performance tests at different current densities were carried out as shown in the following figure. Figure 4 The cycling performance at a current density of 0.5C is shown in Figure 5 As shown in Figure 2, the discharge capacity can still be maintained at 100.59 mAh g after 2300 cycles. -1 The Coulombic efficiency is 99.84%, and the cycle capacity attenuation rate is as low as 0.005%. Example 2

[0022] (1) Add 0.1 mol ascorbic acid, 1.2 mol sodium metavanadate, 1.78 mol diammonium hydrogen phosphate and 0.02 mol ammonium sulfate to 2 L of deionized water, and heat and stir at 60 °C to react; add 0.9 mol sodium oxalate to the reaction solution and stir until dissolved to form a homogeneous solution. After aging at 80 °C for 8 h, heat at 150 °C for 300 mL / h. -1 Na3V2(PO4) was obtained by spray drying under the conditions of 2.97 (SO4) 0.03 Precursor materials; (2) 0.5g Na3V2(PO4) 2.97 (SO4) 0.03 The precursor material and 0.2 mL 25-28 wt% ammonia water were added to 50 mL ethanol, ultrasonically dispersed for 15 min, and 0.3 mL titanium isopropoxide was added dropwise, heated and stirred at 65 ° C for 10 h to obtain a suspension, which was filtered, washed and dried to obtain a powder material; the powder material was calcined in an Ar-H2 mixed atmosphere, first at 400 ° C for 2 h, and then at 900 ° C for 6 h, to finally obtain Na3V2(PO4) 2.97 (SO4) 0.03 @H-TiO2 composite material, that is, modified sodium vanadium phosphate composite material. Example 3

[0023] (1) 0.05 mol glucose, 1.2 mol vanadium hexacarbonyl, 1.7 mol ammonium hydrogen phosphate and 0.1 mol ammonium sulfate were added to 2 L deionized water and heated at 60 °C for reaction. 0.6 mol sodium citrate was added to the reaction solution and stirred until dissolved to form a homogeneous solution. After aging at 80 °C for 5 h, the solution was heated at 180 °C for 200 mL / h. -1 Na3V2(PO4) was obtained by spray drying under the conditions of 2.83 (SO4) 0.17 Precursor materials; (2) 0.5g Na3V2(PO4) 2.83 (SO4) 0.17 The precursor material and 0.3 mL 25-28 wt% ammonia water were added to 50 mL ethanol, ultrasonically dispersed for 15 min, and 0.3 mL titanium chloride was added dropwise, heated and stirred at 55 ° C for 13 h to obtain a suspension, which was filtered, washed and dried to obtain a powder material; the powder material was calcined in an Ar-H2 mixed atmosphere, first at 350 ° C for 4 h, and then at 800 ° C for 8 h, to finally obtain Na3V2(PO4) 2.83 (SO4) 0.17 @H-TiO2 composite material, that is, modified sodium vanadium phosphate composite material. Example 4

[0024] (1) 0.1 mol sucrose, 2.4 mol hexacarbonyl vanadium, 3.4 mol ammonium hydrogen phosphate and 0.2 mol ammonium sulfate were added to 2 L deionized water and heated at 60 °C for reaction. 1.2 mol sodium citrate was added to the reaction solution and stirred until dissolved to form a homogeneous solution. After aging at 80 °C for 10 h, the solution was heated at 200 °C for 200 mL / h. -1 Na3V2(PO4) was obtained by spray drying under the conditions of 2.83 (SO4) 0.17 Precursor materials; (2) 1.0g Na3V2(PO4) 2.83 (SO4) 0.17 The precursor material and 0.3 mL 25-28 wt% ammonia water were added to 50 mL ethanol, ultrasonically dispersed for 15 min, and 0.3 mL titanium chloride was added dropwise, heated and stirred at 65 ° C for 10 h to obtain a suspension, which was filtered, washed and dried to obtain a powder material; the powder material was calcined in an Ar-H2 mixed atmosphere, first at 450 ° C for 3 h, and then at 700 ° C for 10 h, to finally obtain Na3V2(PO4) 2.83 (SO4) 0.17 @H-TiO2 composite material, that is, modified sodium vanadium phosphate composite material.

[0025]

[0026] The materials obtained in each embodiment were used to prepare pole pieces and assemble sodium ion batteries, and the test data are shown in Table 1. From the comparison of the results, under the experimental conditions of Example 1, the doping of sulfate to form Na3V2(PO4) 2.91 (SO4) 0.08 When the battery is charged and discharged, the specific capacity and cycle performance of the battery are optimal.

Claims

1. A method for preparing a modified sodium vanadium phosphate composite material, It is characterized in that The steps include: (1) Add a chain carbon source, a vanadium source, ammonium phosphate and ammonium sulfate into deionized water, stir and heat to react; add a sodium source to the reacted solution and stir until dissolved to form a homogeneous solution; age the homogeneous solution and then spray dry it to obtain Na 3 V 2 (PO 4 ) 3-x (SO 4 ) x Precursor materials; (2) Put Na 3 V 2 (PO 4 ) 3-x (SO 4 ) x The precursor material and ammonia water are added to ethanol, ultrasonically dispersed, and a liquid titanium source is added dropwise to form a mixed solution, the mixed solution is heated and stirred to react to obtain a suspension, and the suspension is filtered, washed, and dried to obtain a powder material; in an Ar-H 2 The powder material is calcined in a mixed atmosphere to obtain a modified sodium vanadium phosphate composite material.

2. The method for preparing the modified sodium vanadium phosphate composite material according to claim 1, It is characterized in that In the step (1), the chain carbon source is one of ascorbic acid, glucose, sucrose, and citric acid; the vanadium source is one of ammonium metavanadate, sodium metavanadate, and hexacarbonyl vanadium; the ammonium phosphate salt is one of diammonium dihydrogen phosphate, diammonium hydrogen phosphate, and ammonium hydrogen phosphate; the ammonium sulfate salt is ammonium hydrogen sulfate or ammonium sulfate; the sodium source is one of sodium carbonate, sodium oxalate, and sodium citrate; the molar ratio of sodium in the sodium source, vanadium in the vanadium source, phosphate in the ammonium phosphate salt, and sulfate in the ammonium sulfate salt is 3:2:3-x:x, 0.03≤x≤0.17; the molar volume ratio of the chain carbon source to deionized water is 0.05~0.1mol:2L; the aging time is 5~10h; the spray drying temperature is 110~200℃; the flow rate is 200~300mLh -1 .

3. The method for preparing the modified sodium vanadium phosphate composite material according to claim 1, It is characterized in that In the step (2), the liquid titanium source is one of tetrabutyl titanate, titanium isopropoxide and titanium chloride; Na 3 V 2 (PO 4 ) 3-x (SO 4 ) x The mass volume ratio of the precursor material and the liquid titanium source is 0.3g~1.0g:0.3mL; the concentration of ammonia water is 25~28wt%; the volume ratio of ammonia water and ethanol is 0.2mL~0.3mL:50mL; the heating temperature is 45℃~65℃, and the stirring time is 10h~15h; the calcination is a two-stage calcination, the first stage calcination temperature is 350℃~450℃, and the duration is 2h~4h; the second stage calcination temperature is 700℃~900℃, and the duration is 6h~10h.

4. An application of a modified sodium vanadium phosphate composite material prepared by the method according to any one of claims 1 to 3, It is characterized in that The modified sodium vanadium phosphate composite material is used as a positive electrode material for sodium ion batteries.

Citation Information

Patent Citations

  • Preparation method of carbon coated vanadium sodium phosphate positive electrode material

    CN105336924A

  • Preparation method of high-power and long-service life lithium vanadium phosphate sodium / carbon positive electrode material

    CN106684384A

  • Metal-doped Na3V2(PO4)3 composite electrode material and preparation method and application thereof

    CN107611390A

  • Sodium vanadium fluorophosphate and carbon compound and preparation method and application thereof

    CN109841800A

  • Doped polyion material, preparation method and application

    CN116632230A