Bimetal sulfur-oxygen compound as well as preparation method and application thereof
Bimetallic sulfur-oxygen compounds are prepared by molybdenum salt, zinc salt and sulfur powder to form an ultra-thin two-dimensional nanosheet interwoven structure, which solves the problem of low electrochemical activity of sodium ion battery electrode materials, and improves conductivity and electrochemical sodium storage Active, achieving efficient electrode material properties.
Patent Information
- Application Number
- CN202411043722.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The existing sodium ion battery electrode materials have problems of low electrochemical activity, volume expansion and insufficient conductivity, which limits their large-scale application.
The bimetallic sulfur-oxygen compound is prepared by calcining the molybdenum salt, zinc salt and sulfur powder, forming a composite material composed of vertical interwoven ultra-thin two-dimensional nanosheets, improving the morphology and nanostructure of the electrode material, increasing the active site and dispersing it. stress.
The electrochemical activity and conductivity are improved, the electrochemical sodium storage activity of the electrode material is enhanced, the first release/charging specific capacity reaches 870/610mAh/g, the Coulomb efficiency is close to 70%, and the process is simple, environmentally friendly, and the cost is low.
Smart Images

Figure CN118954593A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sodium ion battery electrode materials, and in particular relates to a bimetallic sulfur-oxygen compound and a preparation method and application thereof. Background Art
[0002] As an emerging electrochemical energy storage technology, sodium-ion batteries have received extensive attention in recent years due to their relatively abundant sodium resources and low cost. Metal oxide negative electrode materials for sodium-ion batteries are generally characterized by abundant resources, high theoretical specific capacity, and environmental friendliness, but they also have problems such as low conductivity, volume expansion, and voltage hysteresis, which limit their large-scale application. Research on metal oxide negative electrode materials for sodium-ion batteries is constantly progressing, and it is expected to improve their electrochemical performance and overcome existing shortcomings through methods such as material modification, structural design, and electrolyte optimization.
[0003] The Chinese patent application with patent number CN106115785A discloses a technical solution for preparing pure phase molybdenum dioxide as a negative electrode material for sodium ion batteries through the self-reduction reaction of ammonia gas, a product of thermal decomposition of ammonium molybdate. At a current density of 0.05A / g, although its first discharge specific capacity reaches about 930mAh / g, its reversible charge specific capacity is low, only about 300mAh / g. The Chinese patent application with patent number CN112310385A discloses a technical solution for assembling molybdenum dioxide nanoparticles into tremella-shaped nanospheres as negative electrode materials for sodium ion batteries by embedding them on carbon nanosheets. Although the first discharge specific capacity is low, about 730mAh / g, it effectively improves its reversible charge specific capacity to about 550mAh / g. In addition, molybdenum disulfide, as a metal sulfide negative electrode material for sodium ion batteries, has relatively high conductivity and operating voltage, but its electrochemical activity still needs to be further improved, and there is also the problem of rapid attenuation of specific capacity due to volume expansion. For example, in the Chinese patent application with patent number CN112599752A, a carbon-coated hollow kapok fiber-supported flower-shaped molybdenum disulfide composite material was prepared as a negative electrode material for a sodium ion battery. At a current density of 0.05A / g, its first discharge / charge specific capacity was only about 618 / 404mAh / g, and the first coulombic efficiency was 65%. Summary of the invention
[0004] The object of the present invention is to provide a bimetallic sulfur-oxygen compound and a preparation method and application thereof, so as to solve the technical problem of low electrochemical activity of existing sodium ion battery electrode materials.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The present invention discloses a method for preparing a bimetallic sulfur-oxygen compound, comprising the following steps:
[0007] After mixing the molybdenum salt, the zinc salt and the solvent, a solution A is obtained;
[0008] After mixing the complexing agent and the solvent, a solution B is obtained;
[0009] Solution A and solution B are mixed and stirred at room temperature to react, and after the reaction is completed, the precipitate is collected, washed and dried in sequence to obtain a product;
[0010] The product is mixed with sulfur powder and subjected to calcination treatment to obtain a bimetallic sulfur-oxygen compound.
[0011] Furthermore, the molybdenum salt is one of ammonium molybdate, sodium molybdate and potassium molybdate; and the zinc salt is one of zinc nitrate, zinc sulfate and zinc chloride.
[0012] Furthermore, the complexing agent is one of 2-ethyl-4-methylimidazole, 2-hydroxymethyl-1-methylimidazole, and 1-methyl-2-chloromethylimidazole; and the solvent is anhydrous methanol.
[0013] Furthermore, in the solution A, the usage ratio of the molybdenum salt, the zinc salt and the solvent is (1-3) mmol: (1-3) mmol: (10-20) mL.
[0014] Furthermore, in the solution B, the dosage ratio of the complexing agent to the solvent is (20-40) mmol: (40-80) mL.
[0015] Furthermore, the stirring time is 24-48h.
[0016] Furthermore, before the product is mixed with sulfur powder for calcination, the product is placed in a tubular furnace for pretreatment; the pretreatment temperature is 200-400° C. and the time is 2-4 hours.
[0017] Furthermore, the mass ratio of the product to sulfur powder is 1:(2-4); the calcination temperature is 500-700°C, and the calcination time is 2-4h.
[0018] The present invention also discloses a bimetallic sulfur-oxygen compound prepared by the preparation method, wherein the bimetallic sulfur-oxygen compound is composed of vertically interwoven ultrathin two-dimensional nanosheets; the thickness of the ultrathin two-dimensional nanosheets is 15 to 20 nm.
[0019] The invention also discloses the application of the bimetallic sulfur-oxygen compound in the electrode material of a sodium ion battery.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The invention discloses a method for preparing a bimetallic sulfur-oxygen compound. Molybdenum salt, zinc salt and sulfur powder are used as raw materials to modify the morphology and nanostructure of a conventional metal oxide negative electrode material for a sodium ion battery. Bimetallic sulfide is added to obtain a composite material in which ultrathin two-dimensional nanosheets are vertically interwoven to form a three-dimensional nanostructure. The composite material can improve the electrical conductivity, increase the active sites and stabilize the nanostructure of the electrode material, thereby improving the electrochemical activity of the electrode material.
[0022] Furthermore, the bimetallic heterostructure constructed in combination with zinc sulfide can disperse stress and alleviate the volume change of the electrode material during the sodium insertion and extraction process. The three work synergistically to further improve the electrochemical sodium storage activity of the composite electrode material.
[0023] Furthermore, the raw materials of the method of the present invention are all industrial grade, abundant in source, low in cost, and harmless to the environment and human body; the preparation process is simple, has low equipment requirements, strong repeatability, no wastewater or waste liquid is generated, and the process is green and environmentally friendly.
[0024] The present invention also discloses a bimetallic sulfur-oxygen compound prepared by the above method. The prepared product has good crystallinity, special morphology and structure, and high electrochemical sodium storage activity. According to relevant experimental results, when the bimetallic sulfur-oxygen compound is used in the electrode material of a sodium ion battery, at a current density of 0.1A / g, the first discharge / charge specific capacity can reach 870 / 610mAh / g, and the first coulombic efficiency is close to 70%. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a SEM image of the bimetallic sulfur-oxygen compound prepared by the present invention;
[0026] Figure 2 This is the XRD pattern of the bimetallic sulfur-oxygen compound prepared by the present invention;
[0027] Figure 3 This is a charge and discharge curve diagram of the bimetallic sulfur-oxygen compound prepared by the present invention. DETAILED DESCRIPTION
[0028] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0029] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0030] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0031] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0032] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0033] The present invention provides a method for preparing a bimetallic sulfur-oxygen compound, comprising the following steps:
[0034] S1: Prepare solution A by ultrasonically dissolving equimolar molybdenum salt and zinc salt (1-3 mmol) in 10-20 mL of anhydrous methanol;
[0035] S2: 20-40 mmol of the complexing agent is ultrasonically dissolved in 40-80 mL of anhydrous methanol to prepare solution B;
[0036] S3: Mix solutions A and B quickly and stir at room temperature for 24 hours. After the reaction is complete, collect the precipitate, wash it, and dry it;
[0037] S4: The above product is pretreated in a tubular furnace, and then sulfur powder is added after cooling, and the bimetallic sulfur-oxygen compound is obtained after calcination.
[0038] Preferably, in S1, the molybdenum salt and zinc salt include but are not limited to ammonium molybdate, sodium molybdate, potassium molybdate, zinc nitrate, zinc sulfate, and zinc chloride.
[0039] Preferably, in S2, the complexing agent includes but is not limited to 2-ethyl-4-methylimidazole, 2-hydroxymethyl-1-methylimidazole, and 1-methyl-2-chloromethylimidazole.
[0040] Preferably, in S4, the pretreatment temperature is 200-400° C., and the pretreatment time is 2-4 hours.
[0041] Preferably, in S4, the mass ratio of the precursor solid product to the sulfur powder is 1:(2-4).
[0042] Preferably, the calcination temperature in S4 is 500-700° C., and the calcination time is 2-4 hours.
[0043] The bimetallic sulfur-oxygen compound prepared by the preparation method is composed of vertically interwoven ultrathin two-dimensional nanosheets, and the thickness of the nanosheets is 20 nm.
[0044] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0045] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0046] Example 1
[0047] A method for preparing a bimetallic sulfur-oxygen compound comprises the following steps:
[0048] S1: 3 mmol of ammonium molybdate (molybdenum salt) and 3 mmol of zinc nitrate (zinc salt) were ultrasonically dissolved in 20 mL of anhydrous methanol to obtain solution A;
[0049] S2: 40 mmol 2-hydroxymethyl-1-methylimidazole (complexing agent) was ultrasonically dissolved in 80 mL anhydrous methanol to obtain solution B;
[0050] S3: quickly mix solution A and solution B, stir at room temperature for 24 hours, collect the precipitate after the reaction, wash and dry to obtain the product;
[0051] S4: 1 g of the above product was placed in a tubular furnace for pretreatment at 400° C. for 4 h, and then 4 g of sulfur powder was added and calcined at 700° C. for 4 h to obtain a bimetallic sulfur-oxygen compound.
[0052] Example 2
[0053] A method for preparing a bimetallic sulfur-oxygen compound comprises the following steps:
[0054] S1: 2 mmol potassium molybdate (molybdenum salt) and 1 mmol zinc sulfate (zinc salt) were ultrasonically dissolved in 15 mL anhydrous methanol to obtain solution A;
[0055] S2: 30 mmol of 1-methyl-2-chloromethylimidazole (complexing agent) was ultrasonically dissolved in 60 mL of anhydrous methanol to obtain solution B;
[0056] S3: quickly mix solution A and solution B, stir at room temperature for 24 hours, collect the precipitate after the reaction, wash and dry to obtain the product;
[0057] S4: 1 g of the above product was placed in a tubular furnace for pretreatment at 300° C. for 3 h, and then 3 g of sulfur powder was added and calcined at 600° C. for 3 h to obtain a bimetallic sulfur-oxygen compound.
[0058] Example 3
[0059] A method for preparing a bimetallic sulfur-oxygen compound comprises the following steps:
[0060] S1: 1 mmol of sodium molybdate (molybdenum salt) and 1 mmol of zinc chloride (zinc salt) were ultrasonically dissolved in 10 mL of anhydrous methanol to obtain solution A;
[0061] S2: 20 mmol of 2-ethyl-4-methylimidazole (complexing agent) was ultrasonically dissolved in 40 mL of anhydrous methanol to obtain solution B;
[0062] S3: quickly mix solution A and solution B, stir at room temperature for 24 hours, collect the precipitate after the reaction, wash and dry to obtain the product;
[0063] S4: 1 g of the above product was placed in a tubular furnace for pretreatment at 200° C. for 2 h, and then 2 g of sulfur powder was added and calcined at 500° C. for 2 h to obtain a bimetallic sulfur-oxygen compound.
[0064] Example 4
[0065] A method for preparing a bimetallic sulfur-oxygen compound comprises the following steps:
[0066] S1: 1 mmol of sodium molybdate (molybdenum salt) and 3 mmol of zinc nitrate (zinc salt) were ultrasonically dissolved in 20 mL of anhydrous methanol to obtain solution A;
[0067] S2: 25 mmol of 2-hydroxymethyl-1-methylimidazole (complexing agent) was ultrasonically dissolved in 50 mL of anhydrous methanol to obtain solution B;
[0068] S3: quickly mix solutions A and B, stir at room temperature for 48 hours, collect the precipitate after the reaction, wash and dry to obtain the product;
[0069] S4: The above product g was first placed in a tubular furnace at 350°C for pretreatment for 2 hours, and then 3g of sulfur powder was added and calcined at 650°C for 3 hours to obtain a bimetallic sulfur-oxygen compound.
[0070] Example 5
[0071] A method for preparing a bimetallic sulfur-oxygen compound comprises the following steps:
[0072] S1: 2 mmol sodium molybdate (molybdenum salt) and 2 mmol zinc nitrate (zinc salt) were ultrasonically dissolved in 15 mL anhydrous methanol to obtain solution A;
[0073] S2: 20 mmol of 1-methyl-2-chloromethylimidazole (complexing agent) was ultrasonically dissolved in 15 mL of anhydrous methanol to obtain solution B;
[0074] S3: quickly mix solution A and solution B, stir at room temperature for 24 hours, collect the precipitate after the reaction, wash and dry to obtain the product;
[0075] S4: 1 g of the above product was placed in a tubular furnace at 400°C for pretreatment for 2 h, and then 4 g of sulfur powder was added and calcined at 550°C for 3 h to obtain a bimetallic sulfur-oxygen compound.
[0076] Figure 1 This is a SEM image of the bimetallic sulfur-oxygen compound prepared by the present invention. From the image, it can be seen that the bimetallic sulfur-oxygen compound is composed of vertically interwoven ultrathin two-dimensional nanosheets, and the thickness of the ultrathin two-dimensional nanosheets is 15-20nm.
[0077] Figure 2 This is the XRD diagram of the bimetallic sulfur-oxygen compound prepared by the present invention. From the figure, it can be seen that the bimetallic sulfur-oxygen compound is composed of MoS 2 、ZnS、MoO 2 .
[0078] Figure 3 This is a charge and discharge curve diagram of the bimetallic sulfur-oxygen compound prepared by the present invention. It can be seen that at a current density of 0.1A / g, the first discharge specific capacity of the prepared bimetallic sulfur-oxygen compound can reach 870mAh / g, and the first coulombic efficiency is close to 70%.
[0079] Table 1 shows the electrochemical performance data of the bimetallic sulfur-oxygen compound prepared in Example 1 of the present invention and the products in patent numbers CN106115785A, CN112310385A, and CN112599752A. It can be seen that the composite electrode material prepared by the present invention has comprehensive electrochemical performance advantages such as discharge and charge specific capacity and first coulombic efficiency.
[0080] Table 1 Comparison of electrochemical properties of the products prepared by the present invention and related products
[0081]
[0082] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a bimetallic sulfur-oxygen compound, characterized in that: The following steps are involved: After mixing the molybdenum salt, the zinc salt and the solvent, a solution A is obtained; After mixing the complexing agent and the solvent, a solution B is obtained; Solution A and solution B are mixed and stirred at room temperature to react, and after the reaction is completed, the precipitate is collected, washed and dried in sequence to obtain a product; The product is mixed with sulfur powder and subjected to calcination treatment to obtain a bimetallic sulfur-oxygen compound.
2. The method for preparing a bimetallic sulfur-oxygen compound according to claim 1, characterized in that: The molybdenum salt is one of ammonium molybdate, sodium molybdate and potassium molybdate; the zinc salt is one of zinc nitrate, zinc sulfate and zinc chloride.
3. The method for preparing a bimetallic sulfur-oxygen compound according to claim 1, characterized in that: The complexing agent is one of 2-ethyl-4-methylimidazole, 2-hydroxymethyl-1-methylimidazole, and 1-methyl-2-chloromethylimidazole; and the solvent is anhydrous methanol.
4. The method for preparing a bimetallic sulfur-oxygen compound according to claim 1, characterized in that: In the solution A, the usage ratio of the molybdenum salt, the zinc salt and the solvent is (1-3) mmol: (1-3) mmol: (10-20) mL.
5. The method for preparing a bimetallic sulfur-oxygen compound according to claim 1, characterized in that: In the solution B, the dosage ratio of the complexing agent to the solvent is (20-40) mmol: (40-80) mL.
6. The method for preparing a bimetallic sulfur-oxygen compound according to claim 1, characterized in that: The stirring time is 24-48h.
7. The method for preparing a bimetallic sulfur-oxygen compound according to claim 1, characterized in that: Before the product is mixed with sulfur powder for calcination, the product is placed in a tubular furnace for pretreatment; the pretreatment temperature is 200-400° C. and the time is 2-4 hours.
8. The method for preparing a bimetallic sulfur-oxygen compound according to claim 1, characterized in that: The mass ratio of the product to sulfur powder is 1:(2-4); the calcination temperature is 500-700°C and the calcination time is 2-4h.
9. A bimetallic sulfur-oxygen compound, characterized in that: The bimetallic sulfur-oxygen compound is prepared by the preparation method described in any one of claims 1 to 8; the bimetallic sulfur-oxygen compound is composed of ultrathin two-dimensional nanosheets vertically interwoven; the thickness of the ultrathin two-dimensional nanosheets is 15 to 20 nm.
10. Use of the bimetallic sulfur-oxygen compound according to claim 9 in an electrode material for a sodium ion battery.
Citation Information
Patent Citations
Preparation method and application of hollow porous transition metal chalcogenide nanosheets
CN106698365A
High-specific-capacity lithium ion battery material, preparation method and lithium ion battery
CN110931755A
Sodium ion battery cobalt-iron-copper sulfide negative electrode material and preparation method thereof
CN111092222A
Method for preparing Zn-Co-S composite material based on multi-element metal organic framework compound
CN111533178A
Novel oxysulfide, method of producing oxysulfide, and photocatalyst, electrode for water photolysis reaction, and method of producing hydrogen, using the same