Clinical nepheline glass ceramic as well as preparation method and application thereof

By adjusting the composition of Xiashi glass ceramics, the phosphate phase is reduced, the three-sysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysysy Efficiency, achieving high transmittance and high crystallinity ceramic materials.

CN118954955AActive Publication Date: 2024-11-15WUHAN UNIV OF TECH

Patent Information

Application Number
CN202411023844.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The chemical stability of the phosphate phase in existing xiashi glass ceramics is poor, resulting in a decrease in its corrosion resistance and affecting the yield and efficiency of the production process.

Method used

By adjusting the composition of glass ceramics, the content of the phosphate phase is reduced, and the main crystal phase is used, and chemically strengthened by ion exchange method is carried out to form glass ceramics with high crystallinity and high transmittance.

Benefits of technology

It improves the chemical stability and production efficiency of glass ceramics, achieves high crystallinity and high transmittance, and meets the application needs of electronic devices, transportation tools and construction fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004968006790000161
    Figure BDA0004968006790000161
  • Figure BDA0004968006790000171
    Figure BDA0004968006790000171
  • Figure BDA0004968006790000172
    Figure BDA0004968006790000172
Patent Text Reader

Abstract

The invention relates to the technical field of glass ceramics, and discloses a triclinite glass ceramic as well as a preparation method and application thereof. The invention relates to a glass ceramic, which comprises the following components in molar percentage: 43 to 58 mol percent of SiO2, 15 to 27 mol percent of Al2O3, 20 to 30 mol percent of Na2O and 0 to 10 mol percent of Li2O, the catalyst comprises 0-10 mol% of K2O, 0-5 mol% of P2O5 and 0-3 mol% of ZrO2. According to the glass ceramic provided by the invention, the crystallinity can reach more than 80%, the crystal size is less than 90nm, the average transmittance in a visible light wave band can reach more than 90%, the crystal phase composition can only contain a main crystal phase triclinic nepheline phase, or contain a secondary crystal phase nepheline phase and a phosphate phase, and the phosphate phase in the crystal phase is reduced or removed; the chemical stability of the glass ceramic is improved, and the glass ceramic can be chemically strengthened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of glass ceramics, and in particular to triclinic nepheline glass ceramics and a preparation method and application thereof. Background Art

[0002] Glass ceramics are a type of composite material that is made by high-temperature melting, molding, and heat treatment. Compared to glass, glass ceramics have a more stable nanocrystalline structure, higher mechanical strength, and lower thermal expansion coefficient than glass. Therefore, they are widely used in electronic devices, automobiles, construction, and other fields.

[0003] Nepheline glass ceramics have good mechanical strength and can be strengthened by known ion exchange methods. Existing nepheline glass ceramics contain a main phase of nepheline phase and a secondary phase of phosphate phase, wherein nepheline crystals can improve the mechanical strength of glass ceramics, and phosphate crystals are formed at a lower temperature than nepheline crystals and nucleate the crystallization of nepheline on a fine scale (e.g., about tens of nanometers). However, the chemical stability of the phosphate phase is poor, and its presence reduces the corrosion resistance of the nepheline glass ceramics, which is not conducive to the implementation of subsequent chemical strengthening and cleaning steps of the glass ceramics, resulting in a decrease in the yield rate and production efficiency during the production process. Summary of the invention

[0004] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, one of the purposes of the present invention is to provide a glass ceramic; the second purpose of the present invention is to provide a method for preparing the glass ceramic; the third purpose of the present invention is to provide a chemically strengthened glass ceramic; the fourth purpose of the present invention is to provide a method for preparing the chemically strengthened glass ceramic; the fifth purpose of the present invention is to provide glass ceramic, or the application of chemically strengthened glass ceramic.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] A first aspect of the present invention provides a glass ceramic comprising the following components by mole percentage:

[0007] 43~58mol%SiO2;

[0008] 15-27 mol% Al2O3;

[0009] 20-30 mol% Na2O;

[0010] 0~10mol%Li2O;

[0011] 0~10mol%K2O;

[0012] 0~5mol%P2O5;

[0013] 0~3mol%ZrO2.

[0014] Preferably, the glass ceramic further comprises the following components in terms of molar percentage: 0 to 10 mol% ZnO;

[0015] 0~10mol%CaO;

[0016] 0~10mol%MgO;

[0017] 0~10mol%SrO;

[0018] 0~10mol%B2O3;

[0019] 0~10mol%BaO.

[0020] Preferably, the glass ceramic further comprises the following components in terms of molar percentage: 0 to 4 mol% ZnO;

[0021] 0~3mol%CaO;

[0022] 0~3mol%MgO;

[0023] 0~2mol%SrO;

[0024] 0~3mol%B2O3.

[0025] Preferably, the glass-ceramic comprises the following components in terms of molar percentage: 43-58 mol% SiO2;

[0026] 15-23 mol% Al2O3;

[0027] 21-30 mol% Na2O;

[0028] 0~10mol%K2O;

[0029] 1~4mol%P2O5;

[0030] 0.3~3mol%ZrO2.

[0031] Preferably, the glass-ceramic comprises the following components in terms of molar percentage: 43-58 mol% SiO2;

[0032] 15-25 mol% Al2O3;

[0033] 21-30 mol% Na2O;

[0034] 0~10mol%Li2O;

[0035] 1~4mol%P2O5;

[0036] 0~2mol%ZrO2.

[0037] Preferably, the glass ceramic comprises the following components in terms of molar percentage: 48-58 mol% SiO2;

[0038] 15-20 mol% Al2O3;

[0039] 21-30 mol% Na2O;

[0040] 1.5~3.5mol%P2O5;

[0041] 0.3~2mol%ZrO2.

[0042] Preferably, the glass-ceramic comprises the following components in terms of mole percentage:

[0043] 43~53mol%SiO2;

[0044] 18-25 mol% Al2O3;

[0045] 20-24 mol% Na2O;

[0046] 2~6mol%Li2O;

[0047] 0~2mol%K2O;

[0048] 2.5~5mol%P2O5.

[0049] Preferably, in the glass ceramic, the content of SiO2 can also be any one of 43-56 mol%, 43-54 mol%, 43-52 mol%, 45-58 mol%, 47-58 mol%, 49-58 mol%, and 49-56 mol% in terms of molar percentage. SiO2, as a main component of the glass ceramic, constitutes the glass matrix. In addition, SiO2 can be used as a viscosity enhancer to enhance the glass forming ability and give the glass mechanical durability.

[0050] Preferably, in the glass ceramic, the content of Al2O3, measured by mole percentage, can also be any one of 15-21 mol%, 17-25 mol%, 19-25 mol%, and 19-23 mol%.

[0051] Preferably, in the glass ceramic, the content of Na2O in mole percentage can also be any one of 20-28 mol%, 20-26 mol%, 22-30 mol%, 24-30 mol%, and 24-28 mol%.

[0052] Preferably, in the glass ceramic, the content of K2O in molar percentage can also be any one of 0-8 mol%, 0-6 mol%, 2-10 mol%, 4-10 mol%, and 4-8 mol%.

[0053] Preferably, in the glass ceramic, the content of Li2O can also be any one of 0-8 mol%, 0-6 mol%, 2-10 mol%, 4-10 mol%, and 4-8 mol% in mole percentage.

[0054] Preferably, in the glass ceramic, the content of ZrO2 can also be 1 to 3 mol% in terms of molar percentage.

[0055] Preferably, the glass ceramic may further include a nucleating agent; the nucleating agent includes at least one of P2O5 and ZrO2; the molar percentage content of P2O5 in the glass ceramic is 1 to 5 mol%; the molar percentage content of ZrO2 in the glass ceramic is 1 to 3 mol%; the molar percentage content ratio of P2O5 to ZrO2 is 0.25 to 4, which can be one of 4 / 1, 3 / 1, 2 / 1, 1, 1 / 2, 1 / 3, and 1 / 4.

[0056] Preferably, the glass ceramic may further include a chemical clarifier; the chemical clarifier includes at least one of SnO2, As2O3, Sb2O3, F, Cl, Br, CeO2, Fe2O3, and MnO2; when the chemical clarifier is selected from SnO2, As2O3, Sb2O3, F, Cl, and Br, the mass percentage content in the glass ceramic is 0 to 3%, and is not 0, and may be one of 3wt%, 2wt%, 1wt%, and 0.5wt%; when the chemical clarifier is selected from CeO2, Fe2O3, and MnO2, the mass percentage content in the glass ceramic is 0 to 0.5%, and is not 0, and may be one of 0.5wt%, 0.4wt%, 0.3wt%, 0.2wt%, and 0.1wt%.

[0057] Preferably, the glass ceramic may further include SnO2; the mass percentage of SnO2 in the glass ceramic may be one of 0-3%, 0-2%, 0-1%, 0-0.5%, and 0-0.1%. SnO2 is used as a reagent to adjust various physical, melting, color or forming characteristics of the glass ceramic.

[0058] Preferably, the mass percentage content of As2O3, Sb2O3 or a combination thereof in the glass ceramic is 0-0.05%, that is, the glass ceramic may not contain As2O3, Sb2O3 or a combination thereof.

[0059] Preferably, the glass ceramic consists of a main crystalline phase, a secondary crystalline phase and a residual glass phase, wherein the mass percentage of the main crystalline phase is 30-90%, and the mass percentage of the secondary crystalline phase is 0-49%.

[0060] Preferably, the mass percentage of the main crystalline phase is 60-85%.

[0061] Preferably, the mass percentage of the secondary crystalline phase is 0-10%.

[0062] Preferably, the glass ceramic is a grid-like microstructure with regional divisions; the diameter of the grid is 30 to 300 nm; the grid-like microstructure with regional divisions can limit crystal growth and has an obvious self-limiting crystallization effect.

[0063] Preferably, when the thickness of the glass ceramic is 0.7 mm, the average transmittance at a wavelength of 380 to 780 nm is 65% to 93%; further preferably, when the thickness of the glass ceramic is 0.7 mm, the average transmittance at a wavelength of 380 to 780 nm is 68% to 91%.

[0064] Preferably, the main crystalline phase includes one of a triclinic pyroxene phase, a triclinic pyroxene phase and a solid solution crystalline phase thereof.

[0065] Preferably, the triclinic pyroxene includes at least one of low-temperature triclinic pyroxene and high-temperature triclinic pyroxene; the low-temperature triclinic pyroxene (NaAlSiO4, low-carnegieite) has an orthorhombic crystal system and a space group of Pmaa; the high-temperature triclinic pyroxene (NaAlSiO4, high-carnegieite) has a cubic crystal system.

[0066] Preferably, the solid solution includes at least one of NaA1SiO4-SiO2 solid solution, (Na, K)A1SiO4 solid solution, (Na, K)A1SiO4-SiO2 solid solution, R(A1, Si)O4 (wherein R=Na, K, Mg, Ca, Ba or vacancy), (K, Na)SiO4, CaO, SiO2; the R(A1, Si)O4 (wherein R=Na, K, Mg, Ca, Ba or vacancy) is an orthorhombic (Pmaa) lattice silicate, the structure of which is a "filled" derivative of the β-cristobalite form of silica; in the (Na, K)A1SiO4-SiO2 solid solution, Na is dominant relative to K.

[0067] Preferably, the secondary crystalline phase includes at least one of a nepheline phase and a phosphate phase.

[0068] Preferably, the mass of the nepheline phase accounts for 0 to 39% of the mass of the glass ceramic; further preferably, the mass of the nepheline phase accounts for 0 to 10% of the mass of the glass ceramic.

[0069] Preferably, the mass of the phosphate phase accounts for 0-10% of the mass of the glass ceramic; further preferably, the mass of the phosphate phase accounts for 0-5% of the mass of the glass ceramic.

[0070] Preferably, the nepheline phase is a hexagonal (P63) tectosilicate, the structure of which is a "filled" derivative of the β-tridymite form of silica.

[0071] Preferably, the phosphate phase includes a crystalline phosphate phase and an amorphous phosphate phase; the amorphous or crystalline phosphate phase can be formed at a lower temperature than the nepheline crystal; the amorphous or crystalline phosphate phase (about tens of nanometers) promotes the precipitation of triclinic nepheline and nepheline; the size of the crystalline phosphate phase is ≤30nm; the amorphous phosphate phase is distributed uniformly or connected inside the glass ceramic.

[0072] Preferably, the glass-ceramic comprises at least one of triclinic nepheline phase grains, nepheline phase grains, and phosphate phase grains; the main cross-sectional dimension of the grains is less than 90 nm; further preferably, the main cross-sectional dimension of the grains is 30 to 89 nm.

[0073] Preferably, the haze of the glass ceramic is 0.1 to 0.3; further preferably, the haze of the glass ceramic is 0.1 to 0.2; the haze is the percentage of transmitted light scattered outside an angle cone of ±4.0° measured according to ASTM method D1003.

[0074] Preferably, the glass ceramic has a crystallinity of 30 to 90 wt%; further preferably, the glass ceramic has a crystallinity of 40 to 90 wt%; still further preferably, the glass ceramic has a crystallinity of 50 to 90 wt%; further preferably, the glass ceramic has a crystallinity of 60 to 90 wt%; most preferably, the glass ceramic has a crystallinity of 65 to 85 wt%.

[0075] Preferably, the glass ceramic is colorless and transparent.

[0076] Preferably, the refractive index of the glass ceramic is 1.4-1.6.

[0077] Preferably, the Vickers hardness of the glass ceramic is 5 to 8.5 GPa.

[0078] The second aspect of the present invention provides a method for preparing the glass ceramic according to the first aspect of the present invention, comprising the following steps:

[0079] S1, melting and mixing the components at 1400-1600° C. to obtain a precursor glass;

[0080] S2. Heat-treating the precursor glass to obtain the glass ceramic.

[0081] Preferably, in step S1, the time for mixing and melting is 3 to 5 hours.

[0082] Preferably, in the step S1, after the mixed melting, the steps of casting and annealing are also included; the annealing temperature is 550-700° C. and the time is 3-5 hours.

[0083] Preferably, in step S1, the precursor glass may be a glass sheet or any other shape. The glass sheet may be formed by rolling, float, spin coating, pressing and the like, and may have a thickness of less than 5 mm.

[0084] Preferably, in step S2, the heat treatment method is selected from any one of one-step ceramicization and two-step ceramicization.

[0085] Preferably, the one-step ceramicization is as follows: heating the precursor glass from room temperature to 620-800° C. at a heating rate of 1-10° C. / min, and keeping the temperature for 0.5-8 h to obtain glass ceramics.

[0086] Preferably, the two-step ceramicization is selected from any one of the following:

[0087] (1) heating the precursor glass from room temperature to 600-650° C. at a heating rate of 1-10° C. / min, keeping the temperature for 0.5-2 h, and then heating to 650-750° C. at a heating rate of 1-10° C. / min, keeping the temperature for 1-8 h, to obtain a glass ceramic;

[0088] (2) heating the precursor glass from room temperature to 700-800° C. at a heating rate of 1-10° C. / min, keeping the temperature for 1-2 hours, and then heating it to 800-850° C. at a heating rate of 1-10° C. / min, keeping the temperature for 2-4 hours, to obtain glass ceramics.

[0089] Preferably, after the heat treatment is completed, a step of cooling to room temperature is also included.

[0090] The third aspect of the present invention provides a chemically strengthened glass-ceramic, comprising the glass-ceramic described in the first aspect of the present invention.

[0091] Preferably, the chemically strengthened glass-ceramics can form a surface compressive stress in the range of 200 to 3000 MPa, and the depth of the surface compressive stress in the range of 10 to 160 μm.

[0092] Preferably, the Vickers hardness of the chemically strengthened glass-ceramic is 6.5 to 9 GPa.

[0093] The fourth aspect of the present invention provides a method for preparing the chemically strengthened glass-ceramic according to the third aspect of the present invention, comprising the following steps:

[0094] The glass ceramic is placed in a mixed salt bath containing NaNO3 and / or KNO3 to perform single or multiple ion exchanges to obtain the chemically strengthened glass ceramic.

[0095] Preferably, the preparation method of the chemically strengthened glass-ceramic adopts a one-step strengthening method, using K + Na exchange in glass ceramics + , producing a compressive stress layer and improving the strength of the glass.

[0096] Preferably, the mass ratio of NaNO3 to KNO3 is 1:(0.25-4).

[0097] Preferably, the ion exchange temperature is 400-600°C.

[0098] Preferably, the ion exchange time is 1 to 12 hours; further preferably, the ion exchange time is 2 to 10 hours; still further preferably, the ion exchange time is 2 to 8 hours; further still preferably, the ion exchange time is 4 to 8 hours.

[0099] The fifth aspect of the present invention provides the use of the glass ceramics described in the first aspect of the present invention, or the chemically strengthened glass ceramics described in the third aspect in the fields of electronic devices, transportation vehicles, construction, and explosion-proofing.

[0100] Compared with the prior art, the present invention has the following beneficial effects:

[0101] 1) The glass ceramics provided by the present invention have a crystallinity of more than 80%, a crystal size of less than or equal to 80 nm, an average transmittance in the visible light band of more than 90%, and a crystalline phase composition containing only a main crystalline phase of triclinic nepheline phase, or containing a secondary crystalline phase of nepheline phase and a phosphate phase. The reduction or removal of the phosphate phase in the crystalline phase improves the chemical stability of the glass ceramics, enables the glass ceramics to be chemically strengthened, and is beneficial to ensuring the yield and production efficiency in the production process.

[0102] 2) The preparation method of the glass ceramics provided by the present invention has simple steps and a short time. The temperature-time distribution of the heat treatment step and the precursor glass composition can control the ratio of the secondary crystalline phase and the residual glass phase to form a variety of crystalline phase compositions and grain sizes.

[0103] 3) The chemically strengthened glass-ceramics provided by the present invention have good physical properties such as hardness.

[0104] 4) The glass ceramics and chemically strengthened glass ceramics provided by the present invention have excellent performance and can meet the application requirements in electronic devices, transportation vehicles, construction, and explosion-proof fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0105] Figure 1 This is a picture of the glass ceramic sample in Example 1;

[0106] Figure 2 is the XRD curve of the glass ceramic in Example 3;

[0107] Figure 3 is the transmittance curve of the glass ceramic in Example 1;

[0108] Figure 4 is the transmittance curve of the glass ceramic in Example 8;

[0109] Figure 5 This is the SEM image of the glass ceramic in Example 13. DETAILED DESCRIPTION

[0110] The present invention is further described in detail below by specific examples. Unless otherwise specified, the raw materials, reagents or devices used in the examples and comparative examples can be obtained from conventional commercial sources or can be obtained by prior art methods. Unless otherwise specified, the experiments or test methods are conventional methods in the art.

[0111] Example 1

[0112] This embodiment provides a glass ceramic, the components of which are shown in Table 1:

[0113] Table 1 Example 1 Glass ceramic components

[0114] Components Content (mol%) Components Content (mol%) <![CDATA[SiO2]]> 49.2 ZnO 0 <![CDATA[Al2O3]]> 15.3 CaO 0 <![CDATA[B2O3]]> 1.3 MgO 0 <![CDATA[Na2O]]> 30 <![CDATA[P2O5]]> 2.4 <![CDATA[Li2O]]> 0 <![CDATA[ZrO2]]> 1.5 <![CDATA[K2O]]> 0 SrO 0.3

[0115] Glass ceramics are prepared by the following steps:

[0116] S1, melt-refining each raw material at 1600° C. for 4 hours, casting it into a rectangular slab, and annealing the slab at 600° C. for 4 hours to obtain a precursor glass;

[0117] S2. Heat the precursor glass from room temperature to 620°C at a heating rate of 5°C / min, keep it warm for 8 hours, and cool it to room temperature to obtain glass ceramics.

[0118] Figure 1 is a picture of the glass ceramic sample in Example 1, Figure 1 It can be seen that the obtained glass ceramics are colorless and transparent.

[0119] Example 2

[0120] This embodiment provides a glass ceramic, the components of which are shown in Table 2:

[0121] Table 2 Example 2 Glass ceramic components

[0122] Components Content (mol%) Components Content (mol%) <![CDATA[SiO2]]> 52 ZnO 3.1 <![CDATA[Al2O3]]> 15 CaO 2.8 <![CDATA[B2O3]]> 0 MgO 0 <![CDATA[Na2O]]> 21.8 <![CDATA[P2O5]]> 3.3 <![CDATA[Li2O]]> 0 <![CDATA[ZrO2]]> 2 <![CDATA[K2O]]> 0 SrO 0

[0123] Glass ceramics are prepared by the following steps:

[0124] S1, melt-refining each raw material at 1600° C. for 4 hours, casting it into a rectangular slab, and annealing the slab at 600° C. for 4 hours to obtain a precursor glass;

[0125] S2. Heat the precursor glass from room temperature to 600°C at a heating rate of 5°C / min, keep it warm for 2 hours, then heat it to 650°C at a heating rate of 5°C / min, keep it warm for 1 hour, and cool it to room temperature to obtain glass ceramics.

[0126] Example 3

[0127] This embodiment provides a glass ceramic, the components of which are shown in Table 3:

[0128] Table 3 Example 3 Glass ceramic components

[0129] Components Content (mol%) Components Content (mol%) <![CDATA[SiO2]]> 53 ZnO 0 <![CDATA[Al2O3]]> 18 CaO 0 <![CDATA[B2O3]]> 0 MgO 0 <![CDATA[Na2O]]> 20 <![CDATA[P2O5]]> 2.7 <![CDATA[Li2O]]> 4.3 <![CDATA[ZrO2]]> 0 <![CDATA[K2O]]> 1.7 SrO 0.3

[0130] Glass ceramics are prepared by the following steps:

[0131] S1, melt-refining each raw material at 1600° C. for 4 hours, casting it into a rectangular slab, and annealing the slab at 600° C. for 4 hours to obtain a precursor glass;

[0132] S2. Heat the precursor glass from room temperature to 720°C at a heating rate of 5°C / min, keep it warm for 0.5h, and cool it to room temperature to obtain glass ceramics.

[0133] Example 4

[0134] This embodiment provides a glass ceramic, the components of which are shown in Table 4:

[0135] Table 4 Example 4 Glass ceramic components

[0136] Components Content (mol%) Components Content (mol%) <![CDATA[SiO2]]> 47.4 ZnO 0.5 <![CDATA[Al2O3]]> 20.5 CaO 0 <![CDATA[B2O3]]> 0.3 MgO 0 <![CDATA[Na2O]]> 23.4 <![CDATA[P2O5]]> 5 <![CDATA[Li2O]]> 2.3 <![CDATA[ZrO2]]> 0 <![CDATA[K2O]]> 0 SrO 0.6

[0137] Glass ceramics are prepared by the following steps:

[0138] S1, melt-refining each raw material at 1600° C. for 4 hours, casting it into a rectangular slab, and annealing the slab at 600° C. for 4 hours to obtain a precursor glass;

[0139] S2. Heat the precursor glass from room temperature to 650°C at a heating rate of 5°C / min, keep it warm for 1 hour, then heat it to 730°C at a heating rate of 5°C / min, keep it warm for 1 hour, and cool it to room temperature to obtain glass ceramics.

[0140] Example 5

[0141] This embodiment provides a glass ceramic, the components of which are shown in Table 5:

[0142] Table 5 Example 5 Glass Ceramic Components

[0143] Components Content (mol%) Components Content (mol%) <![CDATA[SiO2]]> 58 ZnO 0 <![CDATA[Al2O3]]> 16.4 CaO 0 <![CDATA[B2O3]]> 0 MgO 0 <![CDATA[Na2O]]> 23.2 <![CDATA[P2O5]]> 2.1 <![CDATA[Li2O]]> 0 <![CDATA[ZrO2]]> 0.3 <![CDATA[K2O]]> 0 SrO 0

[0144] Glass ceramics are prepared by the following steps:

[0145] S1, melt-refining each raw material at 1600° C. for 4 hours, casting it into a rectangular slab, and annealing the slab at 600° C. for 4 hours to obtain a precursor glass;

[0146] S2. Heat the precursor glass from room temperature to 800°C at a heating rate of 5°C / min, keep it at this temperature for 1.5 hours, and cool it to room temperature to obtain glass ceramics.

[0147] Example 6

[0148] This embodiment provides a glass ceramic, the components of which are shown in Table 6:

[0149] Table 6 Example 6 Glass ceramic components

[0150] Components Content (mol%) Components Content (mol%) <![CDATA[SiO2]]> 45.1 ZnO 0 <![CDATA[Al2O3]]> 15 CaO 3 <![CDATA[B2O3]]> 1.3 MgO 1.9 <![CDATA[Na2O]]> 21.4 <![CDATA[P2O5]]> 1.3 <![CDATA[Li2O]]> 10 <![CDATA[ZrO2]]> 1 <![CDATA[K2O]]> 0 SrO 0

[0151] Glass ceramics are prepared by the following steps:

[0152] S1, melt-refining each raw material at 1600° C. for 4 hours, casting it into a rectangular slab, and annealing the slab at 600° C. for 4 hours to obtain a precursor glass;

[0153] S2. Heat the precursor glass from room temperature to 620°C at a heating rate of 5°C / min, keep it warm for 1 hour, then heat it to 740°C at a heating rate of 5°C / min, keep it warm for 1 hour, and cool it to room temperature to obtain glass ceramics.

[0154] Example 7

[0155] This embodiment provides a glass ceramic, the components of which are shown in Table 7:

[0156] Table 7 Example 7 Glass Ceramic Composition

[0157] Components Content (mol%) Components Content (mol%) <![CDATA[SiO2]]> 43 ZnO 2.9 <![CDATA[Al2O3]]> 23 CaO 0 <![CDATA[B2O3]]> 0 MgO 2.1 <![CDATA[Na2O]]> 26.3 <![CDATA[P2O5]]> 1.9 <![CDATA[Li2O]]> 0 <![CDATA[ZrO2]]> 0.4 <![CDATA[K2O]]> 0.4 SrO 0

[0158] Glass ceramics are prepared by the following steps:

[0159] S1, melt-refining each raw material at 1600° C. for 4 hours, casting it into a rectangular slab, and annealing the slab at 600° C. for 4 hours to obtain a precursor glass;

[0160] S2. Heat the precursor glass from room temperature to 770°C at a heating rate of 5°C / min, keep it at that temperature for 2 hours, and cool it to room temperature to obtain glass ceramics.

[0161] Example 8

[0162] This embodiment provides a glass ceramic, the components of which are shown in Table 8:

[0163] Table 8 Example 8 Glass Ceramic Components

[0164] Components Content (mol%) Components Content (mol%) <![CDATA[SiO2]]> 46.8 ZnO 0 <![CDATA[Al2O3]]> 17.2 CaO 0 <![CDATA[B2O3]]> 0 MgO 0 <![CDATA[Na2O]]> 22.6 <![CDATA[P2O5]]> 1 <![CDATA[Li2O]]> 0 <![CDATA[ZrO2]]> 2.4 <![CDATA[K2O]]> 10 SrO 0

[0165] Glass ceramics are prepared by the following steps:

[0166] S1, melt-refining each raw material at 1600° C. for 4 hours, casting it into a rectangular slab, and annealing the slab at 600° C. for 4 hours to obtain a precursor glass;

[0167] S2. Heat the precursor glass from room temperature to 630°C at a heating rate of 5°C / min, keep it warm for 0.5h, then heat it to 660°C at a heating rate of 5°C / min, keep it warm for 1h, and cool it to room temperature to obtain glass ceramics.

[0168] Example 9

[0169] This embodiment provides a glass ceramic, the components of which are shown in Table 9:

[0170] Table 9 Example 9 Glass Ceramic Components

[0171] Components Content (mol%) Components Content (mol%) <![CDATA[SiO2]]> 44.1 ZnO 0 <![CDATA[Al2O3]]> 15.5 CaO 0 <![CDATA[B2O3]]> 1.5 MgO 0 <![CDATA[Na2O]]> 27.6 <![CDATA[P2O5]]> 0.9 <![CDATA[Li2O]]> 2 <![CDATA[ZrO2]]> 3 <![CDATA[K2O]]> 4 SrO 1.4

[0172] Glass ceramics are prepared by the following steps:

[0173] S1, melt-refining each raw material at 1600° C. for 4 hours, casting it into a rectangular slab, and annealing the slab at 600° C. for 4 hours to obtain a precursor glass;

[0174] S2. Heat the precursor glass from room temperature to 700°C at a heating rate of 5°C / min, keep it at this temperature for 2 hours, and cool it to room temperature to obtain glass ceramics.

[0175] Example 10

[0176] This embodiment provides a glass ceramic, the components of which are shown in Table 10:

[0177] Table 10 Example 10 Glass ceramic components

[0178] Components Content (mol%) Components Content (mol%) <![CDATA[SiO2]]> 43.5 ZnO 0 <![CDATA[Al2O3]]> 25 CaO 0 <![CDATA[B2O3]]> 0 MgO 0 <![CDATA[Na2O]]> 23.2 <![CDATA[P2O5]]> 3.2 <![CDATA[Li2O]]> 5.1 <![CDATA[ZrO2]]> 0 <![CDATA[K2O]]> 0 SrO 0

[0179] Glass ceramics are prepared by the following steps:

[0180] S1, melt-refining each raw material at 1600° C. for 4 hours, casting it into a rectangular slab, and annealing the slab at 600° C. for 4 hours to obtain a precursor glass;

[0181] S2. Heat the precursor glass from room temperature to 760°C at a heating rate of 5°C / min, keep it warm for 2 hours, then heat it to 850°C at a heating rate of 5°C / min, keep it warm for 4 hours, and cool it to room temperature to obtain glass ceramics.

[0182] Embodiment 11

[0183] This embodiment provides a glass ceramic, the components of which are shown in Table 11:

[0184] Table 11 Example 11 Glass ceramic components

[0185] Components Content (mol%) Components Content (mol%) <![CDATA[SiO2]]> 47 ZnO 0 <![CDATA[Al2O3]]> 19 CaO 0 <![CDATA[B2O3]]> 0 MgO 0 <![CDATA[Na2O]]> 28 <![CDATA[P2O5]]> 2.5 <![CDATA[Li2O]]> 0 <![CDATA[ZrO2]]> 1.5 <![CDATA[K2O]]> 2 SrO 0

[0186] Glass ceramics are prepared by the following steps:

[0187] S1, melt-refining each raw material at 1600° C. for 4 hours, casting it into a rectangular slab, and annealing the slab at 600° C. for 4 hours to obtain a precursor glass;

[0188] S2. Heat the precursor glass from room temperature to 740°C at a heating rate of 5°C / min, keep it warm for 1 hour, and cool it to room temperature to obtain glass ceramics.

[0189] Example 12

[0190] This embodiment provides a glass ceramic, the components of which are shown in Table 12:

[0191] Table 12 Example 12 Glass ceramic components

[0192] Components Content (mol%) Components Content (mol%) <![CDATA[SiO2]]> 50 ZnO 0 <![CDATA[Al2O3]]> 16 CaO 0 <![CDATA[B2O3]]> 2.2 MgO 0 <![CDATA[Na2O]]> 27.1 <![CDATA[P2O5]]> 2.5 <![CDATA[Li2O]]> 1 <![CDATA[ZrO2]]> 0.2 <![CDATA[K2O]]> 1 SrO 0

[0193] Glass ceramics are prepared by the following steps:

[0194] S1, melt-refining each raw material at 1600° C. for 4 hours, casting it into a rectangular slab, and annealing the slab at 600° C. for 4 hours to obtain a precursor glass;

[0195] S2. Heat the precursor glass from room temperature to 650°C at a heating rate of 5°C / min, keep it warm for 1 hour, then heat it to 730°C at a heating rate of 5°C / min, keep it warm for 0.5 hour, and cool it to room temperature to obtain glass ceramics.

[0196] Embodiment 13

[0197] This embodiment provides a glass ceramic, the components of which are shown in Table 13:

[0198] Table 13 Example 13 Glass ceramic components

[0199] Components Content (mol%) Components Content (mol%) <![CDATA[SiO2]]> 48 ZnO 0 <![CDATA[Al2O3]]> 20 CaO 0 <![CDATA[B2O3]]> 0 MgO 0 <![CDATA[Na2O]]> 30 <![CDATA[P2O5]]> 1.5 <![CDATA[Li2O]]> 0 <![CDATA[ZrO2]]> 0.5 <![CDATA[K2O]]> 0 SrO 0

[0200] Glass ceramics are prepared by the following steps:

[0201] S1, melt-refining each raw material at 1600° C. for 4 hours, casting it into a rectangular slab, and annealing the slab at 600° C. for 4 hours to obtain a precursor glass;

[0202] S2. Heat the precursor glass from room temperature to 700°C at a heating rate of 5°C / min, keep it at this temperature for 2 hours, and cool it to room temperature to obtain glass ceramics.

[0203] Embodiment 14

[0204] This embodiment provides a glass ceramic, the components of which are shown in Table 14:

[0205] Table 14 Example 14 Glass ceramic components

[0206] Components Content (mol%) Components Content (mol%) <![CDATA[SiO2]]> 49 ZnO 0 <![CDATA[Al2O3]]> 17.6 CaO 0 <![CDATA[B2O3]]> 0 MgO 0 <![CDATA[Na2O]]> 26.7 <![CDATA[P2O5]]> 3 <![CDATA[Li2O]]> 3.3 <![CDATA[ZrO2]]> 0.4 <![CDATA[K2O]]> 0 SrO 0

[0207] Glass ceramics are prepared by the following steps:

[0208] S1, melt-refining each raw material at 1600° C. for 4 hours, casting it into a rectangular slab, and annealing the slab at 600° C. for 4 hours to obtain a precursor glass;

[0209] S2. Heat the precursor glass from room temperature to 720°C at a heating rate of 5°C / min, keep it warm for 0.5h, and cool it to room temperature to obtain glass ceramics.

[0210] Embodiment 15

[0211] This embodiment provides a glass ceramic, the components of which are shown in Table 15:

[0212] Table 15 Example 15 Glass Ceramic Components

[0213] Components Content (mol%) Components Content (mol%) <![CDATA[SiO2]]> 53 ZnO 0 <![CDATA[Al2O3]]> 16.4 CaO 0 <![CDATA[B2O3]]> 0 MgO 0 <![CDATA[Na2O]]> 22 <![CDATA[P2O5]]> 0.4 <![CDATA[Li2O]]> 4.2 <![CDATA[ZrO2]]> 1.6 <![CDATA[K2O]]> 2.4 SrO 0

[0214] Glass ceramics are prepared by the following steps:

[0215] S1, melt-refining each raw material at 1600° C. for 4 hours, casting it into a rectangular slab, and annealing the slab at 600° C. for 4 hours to obtain a precursor glass;

[0216] S2. Heat the precursor glass from room temperature to 650°C at a heating rate of 5°C / min, keep it warm for 1 hour, then heat it to 700°C at a heating rate of 5°C / min, keep it warm for 8 hours, and cool it to room temperature to obtain glass ceramics.

[0217] Comparative Example 1

[0218] This comparative example provides a glass ceramic, the components of which are shown in Table 16:

[0219] Table 16 Comparative Example 1 Glass Ceramic Components

[0220] Components Content (mol%) Components Content (mol%) <![CDATA[SiO2]]> 49 ZnO 0 <![CDATA[Al2O3]]> 17.6 CaO 0 <![CDATA[B2O3]]> 0 MgO 0 <![CDATA[Na2O]]> 26.7 <![CDATA[P2O5]]> 3 <![CDATA[Li2O]]> 3.3 <![CDATA[ZrO2]]> 0.4 <![CDATA[K2O]]> 0 SrO 0

[0221] Glass ceramics are prepared by the following steps:

[0222] S1, melt-refining each raw material at 1600° C. for 4 hours, casting it into a rectangular slab, and annealing the slab at 600° C. for 4 hours to obtain a precursor glass;

[0223] S2. Heat the precursor glass from room temperature to 740°C at a heating rate of 5°C / min, keep it warm for 1 hour, and cool it to room temperature to obtain glass ceramics.

[0224] Comparative Example 2

[0225] This comparative example provides a glass ceramic, the components of which are shown in Table 17:

[0226] Table 17 Comparative Example 2 Glass Ceramic Components

[0227] Components Content (mol%) Components Content (mol%) <![CDATA[SiO2]]> 53 ZnO 0 <![CDATA[Al2O3]]> 16.4 CaO 0 <![CDATA[B2O3]]> 0 MgO 0 <![CDATA[Na2O]]> 22 <![CDATA[P2O5]]> 0.4 <![CDATA[Li2O]]> 4.2 <![CDATA[ZrO2]]> 1.6 <![CDATA[K2O]]> 2.4 SrO 0

[0228] Glass ceramics are prepared by the following steps:

[0229] S1, melt-refining each raw material at 1600° C. for 4 hours, casting it into a rectangular slab, and annealing the slab at 600° C. for 4 hours to obtain a precursor glass;

[0230] S2. Heat the precursor glass from room temperature to 650°C at a heating rate of 5°C / min, keep it warm for 1 hour, then heat it to 700°C at a heating rate of 5°C / min, keep it warm for 8 hours, and cool it to room temperature to obtain glass ceramics.

[0231] Glass ceramic characterization and performance testing

[0232] 1. The crystal phase compositions of the glass ceramics in Examples 1-15 and Comparative Examples 1-2 were analyzed. The results are shown in Table 18:

[0233] Table 18 Crystalline phase composition of glass ceramics in Examples 1-15 and Comparative Examples 1-2

[0234]

[0235]

[0236] Note: In the table, “LC” stands for low-temperature triclinic nepheline, and “HC” stands for high-temperature triclinic nepheline.

[0237] Table 18 is the crystal phase composition of the glass ceramics in Examples 1-15. It can be seen from Table 18 that the crystal phases of the ceramic glass in Examples 1-15 include only triclinic nepheline crystal phase, triclinic nepheline crystal phase and its solid solution (solid solution includes at least one of NaA1SiO4-SiO2 solid solution, (Na, K)A1SiO4 solid solution, (Na, K)A1SiO4-SiO2 solid solution, R(A1, Si)O4 (wherein R=Na, K, Mg, Ca, Ba or vacancy), (K, Na)SiO4, CaO, SiO2), triclinic nepheline crystal phase and nepheline crystal phase, triclinic nepheline crystal phase and phosphate phase, triclinic nepheline crystal phase and its solid solution, nepheline phase and phosphate phase. X-ray diffraction analysis was performed on the glass ceramics in Example 3. Figure 2 is the XRD curve of the glass ceramic in Example 3, Figure 2 It can be seen that the glass ceramic in Example 3 has only one crystal phase of triclinic nepheline, and the crystal peak is obvious and the crystallinity is high. That is, the crystal phase composition of the glass ceramic provided by the present invention can only contain triclinic nepheline crystal phase, and the reduction of phosphate phase is conducive to the improvement of the chemical stability of ceramic glass.

[0238] 2. The transmittance, haze, crystallinity, refractive index and crystal size of the glass ceramics in Examples 1-15 and Comparative Examples 1-2 were measured. The results are shown in Table 19:

[0239] Table 19 Relevant properties of glass ceramics in Examples 1-15 and Comparative Examples 1-2

[0240]

[0241]

[0242] Table 19 shows the relevant properties of the glass ceramics in Examples 1-15 and Comparative Examples 1-2. It can be seen from Table 19 that the crystallinity of the ceramic glass in Examples 1-15 is greater than 30wt%; the crystal size is less than or equal to 89nm; the average transmittance of the glass ceramics with a thickness of 0.7mm at a wavelength of 380-780nm is greater than or equal to 68%, and the refractive index is 1.46-1.51. Figure 3 is the transmittance curve of the glass ceramic in Example 1, Figure 4 is the transmittance curve of the glass ceramic in Example 8, Figure 3 and Figure 4It can be seen that the glass ceramics of Example 1 and Example 8 have an average transmittance of 90% and 91% respectively. It can be seen that the ceramic glass provided by the present invention has a high average transmittance and a high crystallinity. Figure 5 is the SEM picture of the glass ceramic in Example 13, Figure 5 It can be seen that a grid-like microstructure with obvious regional separation appears inside the glass ceramic. The diameter of the grid is about 200 nm. The existence of the grid hinders ion migration. The crystal size in Example 13 is only about 58 nm, which shows that it has an obvious self-limiting crystallization effect.

[0243] 2. Chemical stability test of the glass ceramics in Examples 11-15 and Comparative Examples 1-2:

[0244] The test reference standard is GB / T 32644-2016, and the test results are shown in Table 20. Specifically: the weight loss method is used for testing, and a 25mm×50mm×1mm sample to be tested is prepared. After being cleaned with neutral, organic solvents, and water ultrasonic vibrations that do not corrode the sample to be tested, it is dried in an oven at 110°C for 30 minutes. The sample to be tested is weighed with a balance and placed in a dryer. During the test, the acid and alkali concentrations, corrosion temperature and time and other conditions are followed. After the test, the sample is washed with pure water and weighed with a balance. The balance weighs the sample mass with an accuracy of 0.01 mg; the calculation formula for the total surface area is as shown in formula (Ⅰ), and the calculation formula for the mass change per unit area is as shown in formula (Ⅱ):

[0245] A=(L×W×2)+[(L×W)×T×2] (Ⅰ);

[0246] Where, L: length of the sample to be tested, cm;

[0247] W: width of the sample to be tested, cm;

[0248] T: thickness of the sample to be tested, cm;

[0249] A: Total surface area of ​​the sample to be tested, cm 2 ;

[0250]

[0251] Where, W1: original mass of the sample, mg;

[0252] W2: mass of the sample after the test, mg;

[0253] A: Total surface area of ​​the sample to be tested, cm 2 ;

[0254] W A : Change in mass per unit area, mg / cm 2 .

[0255] Chemical stability testing includes:

[0256] (1) Chemical stability 1: Mass loss of glass ceramics after immersion in 10% HF solution at 20°C for 20 min;

[0257] (2) Chemical stability 2: Mass loss of glass ceramics after immersion in 5% NaOH solution at 95 °C for 6 h;

[0258] (3) Chemical stability 3: Mass loss of glass ceramics after immersion in 5% HCl solution at 95 °C for 24 h;

[0259] (4) Chemical stability 4: Mass loss of glass ceramics after immersion in 10% NH4F-HF buffer at 20°C for 20 min.

[0260] Table 20 Chemical stability test results of glass ceramics in Examples 11-15 and Comparative Examples 1-2

[0261]

[0262] Table 20 is the chemical stability test result of the glass ceramics in Examples 11-15 and Comparative Examples 1-2. As shown in Table 20, the mass per unit area of ​​the glass ceramics in Examples 11-15 after immersion in HF solution, NaOH solution, HCl solution and NH4F-HF buffer solution is less, especially the glass ceramics containing only triclinic nepheline crystal phase in Examples 12 and 13, chemical stability 1-4 is better than the remaining embodiments, and in Comparative Examples 1-2, the raw materials and process conditions of the glass ceramics are similar to those in Examples 13 and 14, respectively, but because the crystal phases of the glass ceramics are composed of nepheline phase and phosphate phase, the presence of phosphate increases the mass loss, making the chemical stability of the two poor, compared with Examples 13 and 14, the mass loss is significantly increased. It can be seen that the glass ceramics without phosphate phase provided by the present invention have good chemical stability, which is conducive to ensuring the yield rate and production efficiency during production.

[0263] 3. Chemically strengthen the glass ceramics in Examples 11-15. Specifically, the glass ceramics are placed in a mixed salt bath containing NaNO3 and KNO3 for ion exchange. The molten salt ratio is 1:1, the ion exchange temperature is 450°C, and the total ion exchange time is 4h to obtain chemically strengthened glass ceramics. Hardness tests are performed on the glass ceramics before and after chemical strengthening, and the surface compressive stress (CS) and compressive stress depth (DOL) of the glass ceramics after chemical strengthening are tested. The hardness test conditions are: maximum load 1.961N, peak holding time 15s, and the test results are shown in Table 21:

[0264] Table 21 Properties of glass ceramics before and after chemical strengthening in Examples 11-15

[0265]

[0266] Table 21 is the performance before and after chemical strengthening of glass ceramics in embodiment 11-15, as shown in Table 21, chemical strengthening is carried out by ion exchange method, the small radius cation present in large radius cation exchange glass ceramics is made, and compared with before strengthening, the Vickers hardness of chemically strengthened glass ceramics increases, and physical property improves.Potassium cation exchange enters glass ceramics, particularly enters triclinic nepheline crystal, sodium cation or smaller cation exchange is taken out of glass ceramics, the unit cell of triclinic nepheline crystal can be expanded, and larger compressive stress and darker compressive stress layer are produced on glass ceramic surface.It can be seen that the glass ceramics provided by the present invention, which does not contain phosphate phase or content is relatively low, is conducive to the carrying out of chemical strengthening treatment.

[0267] The glass ceramic provided by the present invention is a glass ceramic with triclinic nepheline as the main crystal phase, the mass percentage of the main crystal phase is greater than or equal to 30%, and can contain at least one secondary crystal phase of nepheline phase and phosphate phase, the mass percentage of the secondary crystal phase is 0-49%, and the chemical stability of the glass ceramic is improved by reducing the content of the secondary crystal phase (especially the phosphate phase), which is conducive to the implementation of subsequent chemical strengthening and cleaning steps, and ensures the yield rate and production efficiency in the production process; the crystallinity of the glass ceramic can reach more than 80%, the crystal size is less than or equal to 89nm, and the average transmittance in the visible light band can reach more than 90%; the crystal phase composition is diverse, and can be regulated according to the heat treatment step in the preparation method, and the heat treatment time is short; the chemically strengthened glass ceramic has good physical properties and can meet the application in electronic devices, transportation vehicles, construction, and explosion-proof fields.

Claims

1. A glass ceramic, characterized in that: In terms of mole percentage, it includes the following components: 43~58mol%SiO2; 15-27 mol% Al2O3; 20-30 mol% Na2O; 0~10mol%Li2O; 0~10mol%K2O; 0~5mol%P2O5; 0~3mol%ZrO2.

2. The glass ceramic according to claim 1, characterized in that In terms of mole percentage, the glass-ceramic further comprises the following components: 0~10mol%ZnO; 0~10mol%CaO; 0~10mol%MgO; 0~10mol%SrO; 0~10mol%B2O3; 0~10mol%BaO.

3. The glass ceramic according to claim 2, characterized in that: In terms of mole percentage, the glass-ceramic further comprises the following components: 0~4mol%ZnO; 0~3mol%CaO; 0~3mol%MgO; 0~2mol%SrO; 0~3mol%B2O3.

4. The glass ceramic according to claim 1, characterized in that In terms of mole percentage, the glass-ceramic comprises the following components: 43~58mol%SiO2; 15-23 mol% Al2O3; 21-30 mol% Na2O; 0~10mol%K2O; 1~4mol%P2O5; 0.3~3mol%ZrO2.

5. The glass ceramic according to claim 1, characterized in that: In terms of mole percentage, the glass-ceramic comprises the following components: 43~58mol%SiO2; 15-25 mol% Al2O3; 21-30 mol% Na2O; 0~10mol%Li2O; 1~4mol%P2O5; 0~2mol%ZrO2.

6. The glass ceramic according to claim 1, characterized in that: In terms of mole percentage, the glass-ceramic comprises the following components: 48~58mol%SiO2; 15-20 mol% Al2O3; 21-30 mol% Na2O; 1.5~3.5mol%P2O5; 0.3~2mol%ZrO2.

7. The glass ceramic according to claim 1, characterized in that In terms of mole percentage, the glass-ceramic comprises the following components: 43~53mol%SiO2; 18-25 mol% Al2O3; 20-24 mol% Na2O; 2~6mol%Li2O; 0~2mol%K2O; 2.5~5mol%P2O5.

8. The glass ceramic according to any one of claims 1 to 7, characterized in that: The glass ceramics are composed of a main crystalline phase, a secondary crystalline phase and a residual glass phase, wherein the mass percentage of the main crystalline phase is 30-90%, and the mass percentage of the secondary crystalline phase is 0-49%.

9. The glass ceramic according to any one of claims 1 to 7, characterized in that: The glass ceramic is a grid-like microstructure with separated regions; the diameter of the grid is 30-300 nm.

10. The glass ceramic according to any one of claims 1 to 7, characterized in that: When the thickness of the glass ceramic is 0.7 mm, the average transmittance at a wavelength of 380 to 780 nm is 65% to 93%.

11. The glass ceramic according to claim 8, characterized in that: The main crystal phase includes one of a triclinic nepheline phase, a triclinic nepheline phase and a solid solution crystal phase thereof.

12. The glass ceramic according to claim 11, characterized in that The triclinic nepheline includes at least one of low-temperature triclinic nepheline and high-temperature triclinic nepheline; And / or, the solid solution includes at least one of NaA1SiO4-SiO2 solid solution, (Na, K)A1SiO4 solid solution, (Na, K)A1SiO4-SiO2 solid solution, R(A1, Si)O4 (wherein R = Na, K, Mg, Ca, Ba or vacancy), (K, Na)SiO4, CaO, and SiO2.

13. The glass ceramic according to claim 8, characterized in that The secondary crystalline phase includes at least one of a nepheline phase and a phosphate phase; Preferably, the mass of the nepheline phase accounts for 0 to 39% of the mass of the glass ceramic; Preferably, the mass of the phosphate phase accounts for 0-10% of the mass of the glass ceramic.

14. The method for preparing the glass ceramic according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1, melting and mixing the components at 1400-1600° C. to obtain a precursor glass; S2. Heat-treating the precursor glass to obtain the glass ceramic.

15. The preparation method according to claim 14, characterized in that: In step S2, the heat treatment method is selected from any one of one-step ceramicization and two-step ceramicization; Preferably, the one-step ceramicization is as follows: heating the precursor glass from room temperature to 620-800° C. at a heating rate of 1-10° C. / min, and keeping the temperature for 0.5-8 hours to obtain glass ceramics; Preferably, the two-step ceramicization is selected from any one of the following: (1) heating the precursor glass from room temperature to 600-650° C. at a heating rate of 1-10° C. / min, keeping the temperature for 0.5-2 h, and then heating to 650-750° C. at a heating rate of 1-10° C. / min, keeping the temperature for 1-8 h, to obtain a glass ceramic; (2) heating the precursor glass from room temperature to 700-800° C. at a heating rate of 1-10° C. / min, keeping the temperature for 1-2 hours, and then heating it to 800-850° C. at a heating rate of 1-10° C. / min, keeping the temperature for 2-4 hours, to obtain glass ceramics.

16. A chemically strengthened glass ceramic, characterized in that: The invention comprises the glass ceramics as described in any one of claims 1 to 7.

17. The chemically strengthened glass-ceramic according to claim 16, characterized in that: The chemically strengthened glass ceramic can form a surface compressive stress in the range of 200 to 3000 MPa, and the depth of the surface compressive stress is in the range of 10 to 160 μm.

18. The method for preparing the chemically strengthened glass-ceramic according to any one of claims 16 to 17, characterized in that: The following steps are involved: The glass ceramic is placed in a mixed salt bath containing NaNO3 and / or KNO3 to perform single or multiple ion exchanges to obtain the chemically strengthened glass ceramic.

19. The preparation method according to claim 18, characterized in that: The ion exchange temperature is 400-600°C; And / or, the ion exchange time is 1 to 12 hours.

20. Use of the glass ceramic according to any one of claims 1 to 7, or the chemically strengthened glass ceramic according to any one of claims 16 to 17 in the fields of electronic devices, transportation vehicles, construction, and explosion-proofing.

Citation Information

Patent Citations

  • Transparent glass-ceramic articles, glass-ceramic precursor glasses and methods for forming the same

    CN106660860A

  • High-crystallinity sodium nepheline transparent glass-ceramics and preparation method thereof

    CN109608047A

  • Method for one-step chemical strengthening of sodium nepheline microcrystalline glass and chemically strengthened sodium nepheline microcrystalline glass

    CN113149444A

  • Glass ceramic, preparation method thereof, reinforced glass ceramic and application

    CN118026536A

  • Lithium ion-conductive glass ceramic, method for producing a lithium ion-conductive glass ceramic, ion conductor and use of the ion conductor

    WO2013164116A1

Cited By

  • Triclinic nepheline glass ceramic, and preparation method therefor and use thereof

    WO2026026329A1