Mortar prepared by compounding stone powder and fly ash
The mortar preparation by combining stone powder and fly ash has solved the problems of high maintenance and repair costs and low stability of existing mortars, high strength, permeability and crack resistance are achieved, and maintenance costs are reduced. It is suitable for different projects. Project requirements.
Patent Information
- Application Number
- CN202411046792.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-15
AI Technical Summary
The existing mortar has high maintenance and repair costs and low stability during long-term use.
The mortar is prepared by combining stone powder and fly ash. Through the steps of raw material preparation, mixing, water addition adjustment and mixing adjustment, the performance of the mortar meets the requirements, including the appropriate amount of cement, stone powder, fly ash and water Add appropriate amounts to ensure the consistency and fluidity of the mortar, and finally carry out quality inspection and storage.
The mortar with specific performance is designed according to engineering needs, with high strength, permeability and crack resistance, reducing maintenance and repair costs, and improving the working performance and durability of the mortar.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, in particular to mortar prepared by combining stone powder and fly ash. Background Art
[0002] Composite mortar usually refers to combining multiple raw materials to prepare mortar with specific properties and uses. These raw materials include cement, stone powder, fly ash, quartz sand, aggregates (such as crushed stone, river sand), admixtures (such as water reducer, plasticizer), etc.
[0003] The prior art has the following deficiencies: the maintenance and repair costs of ordinary mortar are high during long-term use, and the stability is not high. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the deficiencies in the prior art, the present invention provides a mortar prepared by combining stone powder and fly ash.
[0006] (II) Technical solution
[0007] To achieve the above object, the present invention provides the following technical solution: stone powder and fly ash are composited to prepare mortar, comprising the following steps:
[0008] S1: Raw material preparation: Stone powder and fly ash as admixtures need to be prepared in advance to ensure that their quality meets the relevant standards and requirements, and that the quality of other raw materials such as sand and cement also meets the requirements to ensure the performance of the final mortar;
[0009] S2: Mix design: Cement: The amount of cement will be determined based on the specific strength requirements and concrete mix ratio, and is part of the cement dosage.
[0010] Sand: The amount of sand used will be determined according to the mix ratio of the mortar, usually 2-4 times the amount of cement;
[0011] Stone powder: The amount of stone powder is generally between 10% and 20%, and the specific proportion depends on the quality of the stone powder used and the expected effect;
[0012] Fly ash: The amount of fly ash added is generally between 10% and 20%, which also depends on the quality of the fly ash and the expected effect;
[0013] S3: Hybrid:
[0014] Mix the stone powder, fly ash and cement evenly according to the designed mix ratio, which can be done by mechanical mixing or manual mixing;
[0015] During the mixing process, ensure that all raw materials are fully mixed to avoid lumps or unevenness;
[0016] S4: Add water to adjust:
[0017] According to the specific requirements of the mortar, gradually add appropriate amount of water to control the consistency and fluidity of the mortar;
[0018] When adding water, pay attention to adding it gradually to avoid adding too much at one time, which will make the mortar too thin;
[0019] S5: Hybrid Adjustment:
[0020] During the mixing process, the proportion of stone powder, fly ash and cement, as well as the amount of water, can be appropriately adjusted as needed to obtain more suitable mortar properties;
[0021] During the mixing process, tests can be carried out according to actual conditions to adjust the mix ratio of the mortar to achieve the best performance and use effect;
[0022] S6: Inspection and storage:
[0023] After mixing, the mortar is subjected to necessary inspections, such as measuring its fluidity, compressive strength and other indicators, to ensure that its quality meets the requirements;
[0024] Store the mixed mortar in a dry and ventilated environment to prevent it from absorbing moisture or being affected by other contamination.
[0025] Preferably, the amount of water in the stone powder and fly ash is usually not a factor directly considered when preparing mortar, because the amount of water added is mainly determined based on the performance requirements of the mortar and the humidity of the mixed materials. During the process of mixing the mortar, the water content of the stone powder and fly ash may affect the final mortar mix ratio.
[0026] Stone powder and fly ash are added to the mixture when preparing mortar, and are usually mixed in a dry state. Therefore, their water content will affect the humidity and fluidity of the final mixture. When mixing mortar, the amount of water added needs to be adjusted according to the humidity and fluidity of the mixture to ensure that the mortar has appropriate plasticity and fluidity.
[0027] Preferably, the raw materials are collected: the main raw materials of cement include limestone (CaCO3), clay (SiO2, Al2O3, Fe2O3) and iron ore, which are usually obtained by mining and the like.
[0028] Preferably, the grinding and pretreatment: the raw materials need to undergo pretreatment processes such as crushing, pulverizing and mixing to ensure that the particle size of the raw materials is appropriate, which is beneficial to the subsequent calcination reaction.
[0029] Preferably, the calcination: the pretreated raw material mixture is sent to a cement kiln for calcination, in which the raw material mixture undergoes a chemical reaction at a high temperature of 1300-1450 degrees Celsius to generate molten clinker (clinker is a molten cement raw material without cement grinding).
[0030] Preferably, the cooling: After the clinker is taken out of the cement kiln, it needs to go through a cooling process, which helps to solidify the clinker and make it suitable for grinding processing.
[0031] Preferably, the grinding: the cooled clinker is fed into a cement mill for grinding, in which the clinker is crushed and mixed with an appropriate amount of gypsum (calcium sulfate) to form a final cement product.
[0032] Preferably, in the cement production, clinker is the main component of cement, and gypsum (calcium sulfate) is an auxiliary additive used to adjust the setting and hardening properties of cement, and the mixing ratio is between 0.5% and 5%.
[0033] (III) Beneficial effects
[0034] Compared with the prior art, the present invention provides a composite mortar made of stone powder and fly ash, which has the following advantages:
[0035] Beneficial effects:
[0036] The composite mortar provided by the present invention can be formulated according to specific engineering requirements to obtain specific performance characteristics, such as high strength, impermeability, crack resistance, etc. By rationally selecting raw materials and adding appropriate amounts of admixtures, the mortar can have better working performance and durability, can save maintenance and repair costs in long-term use, and has good economy to meet the requirements of different engineering projects. DETAILED DESCRIPTION
[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] Embodiment 1:
[0039] S1: Raw material preparation: Stone powder and fly ash as admixtures need to be prepared in advance to ensure that their quality meets the relevant standards and requirements, and that the quality of other raw materials such as sand and cement also meets the requirements to ensure the performance of the final mortar;
[0040] S2: Mix design: Cement: The amount of cement will be determined based on the specific strength requirements and concrete mix ratio, and is part of the cement dosage.
[0041] Sand: The amount of sand used will be determined according to the mix ratio of the mortar, usually twice the amount of cement;
[0042] Stone powder: The amount of stone powder is generally 10%, and the specific proportion depends on the quality of the stone powder used and the expected effect;
[0043] Fly ash: The amount of fly ash added is generally 10%, which also depends on the quality of the fly ash and the expected effect;
[0044] S3: Hybrid:
[0045] Mix the stone powder, fly ash and cement evenly according to the designed mix ratio, which can be done by mechanical mixing or manual mixing;
[0046] During the mixing process, ensure that all raw materials are fully mixed to avoid lumps or unevenness;
[0047] S4: Add water to adjust:
[0048] According to the specific requirements of the mortar, gradually add appropriate amount of water to control the consistency and fluidity of the mortar;
[0049] When adding water, pay attention to adding it gradually to avoid adding too much at one time, which will make the mortar too thin;
[0050] S5: Hybrid Adjustment:
[0051] During the mixing process, the proportion of stone powder, fly ash and cement, as well as the amount of water, can be appropriately adjusted as needed to obtain more suitable mortar properties;
[0052] During the mixing process, tests can be carried out according to actual conditions to adjust the mix ratio of the mortar to achieve the best performance and use effect;
[0053] S6: Inspection and storage:
[0054] After mixing, the mortar is subjected to necessary inspections, such as measuring its fluidity, compressive strength and other indicators, to ensure that its quality meets the requirements;
[0055] Store the mixed mortar in a dry and ventilated environment to prevent it from absorbing moisture or being affected by other contamination.
[0056] The amount of water in stone powder and fly ash is usually not a direct consideration when preparing mortar, because the amount of water added is mainly determined by the performance requirements of the mortar and the humidity of the mixed materials. During the process of mixing mortar, the water content of stone powder and fly ash may affect the final mortar mix ratio.
[0057] Stone powder and fly ash are added to the mixture when preparing mortar, and are usually mixed in a dry state. Therefore, their water content will affect the humidity and fluidity of the final mixture. When mixing mortar, the amount of water added needs to be adjusted according to the humidity and fluidity of the mixture to ensure that the mortar has appropriate plasticity and fluidity.
[0058] Raw material collection: The main raw materials of cement include limestone (CaCO3), clay (SiO2, Al2O3, Fe2O3) and iron ore, which are usually obtained through mining and other methods.
[0059] Grinding and pretreatment: The raw materials need to go through pretreatment processes such as crushing, pulverizing and mixing to ensure that the particle size of the raw materials is suitable, which is conducive to the subsequent calcination reaction.
[0060] Calcination: The pretreated raw material mixture is sent to the cement kiln for calcination. In the cement kiln, the raw material mixture undergoes a chemical reaction at a high temperature of 1300 degrees Celsius to produce molten clinker (clinker is the molten cement raw material without cement grinding).
[0061] Cooling: After the clinker is taken out of the cement kiln, it needs to go through a cooling process. Cooling helps to solidify the clinker and make it suitable for grinding.
[0062] Grinding: The cooled clinker is fed into a cement mill for grinding where it is crushed and mixed with an appropriate amount of gypsum (calcium sulfate) to form the final cement product.
[0063] In cement production, clinker is the main component of cement, while gypsum (calcium sulfate) is an auxiliary additive used to adjust the setting and hardening properties of cement, with a mixing ratio of 0.5%.
[0064] Embodiment 2:
[0065] S1: Raw material preparation: Stone powder and fly ash as admixtures need to be prepared in advance to ensure that their quality meets the relevant standards and requirements, and that the quality of other raw materials such as sand and cement also meets the requirements to ensure the performance of the final mortar;
[0066] S2: Mix design: Cement: The amount of cement will be determined based on the specific strength requirements and concrete mix ratio, and is part of the cement dosage.
[0067] Sand: The amount of sand will be determined according to the mix ratio of the mortar, usually 3 times the amount of cement;
[0068] Stone powder: The amount of stone powder is generally 15%, and the specific proportion depends on the quality of the stone powder used and the expected effect;
[0069] Fly ash: The amount of fly ash added is generally 15%, which also depends on the quality of the fly ash and the expected effect;
[0070] S3: Hybrid:
[0071] Mix the stone powder, fly ash and cement evenly according to the designed mix ratio, which can be done by mechanical mixing or manual mixing;
[0072] During the mixing process, ensure that all raw materials are fully mixed to avoid lumps or unevenness;
[0073] S4: Add water to adjust:
[0074] According to the specific requirements of the mortar, gradually add appropriate amount of water to control the consistency and fluidity of the mortar;
[0075] When adding water, pay attention to adding it gradually to avoid adding too much at one time, which will make the mortar too thin;
[0076] S5: Hybrid Adjustment:
[0077] During the mixing process, the proportion of stone powder, fly ash and cement, as well as the amount of water, can be appropriately adjusted as needed to obtain more suitable mortar properties;
[0078] During the mixing process, tests can be carried out according to actual conditions to adjust the mix ratio of the mortar to achieve the best performance and use effect;
[0079] S6: Inspection and storage:
[0080] After mixing, the mortar is subjected to necessary inspections, such as measuring its fluidity, compressive strength and other indicators, to ensure that its quality meets the requirements;
[0081] Store the mixed mortar in a dry and ventilated environment to prevent it from absorbing moisture or being affected by other contamination.
[0082] The amount of water in stone powder and fly ash is usually not a direct consideration when preparing mortar, because the amount of water added is mainly determined by the performance requirements of the mortar and the humidity of the mixed materials. During the process of mixing mortar, the water content of stone powder and fly ash may affect the final mortar mix ratio.
[0083] Stone powder and fly ash are added to the mixture when preparing mortar, and are usually mixed in a dry state. Therefore, their water content will affect the humidity and fluidity of the final mixture. When mixing mortar, the amount of water added needs to be adjusted according to the humidity and fluidity of the mixture to ensure that the mortar has appropriate plasticity and fluidity.
[0084] Raw material collection: The main raw materials of cement include limestone (CaCO3), clay (SiO2, Al2O3, Fe2O3) and iron ore, which are usually obtained through mining and other methods.
[0085] Grinding and pretreatment: The raw materials need to go through pretreatment processes such as crushing, pulverizing and mixing to ensure that the particle size of the raw materials is suitable, which is conducive to the subsequent calcination reaction.
[0086] Calcination: The pretreated raw material mixture is sent to the cement kiln for calcination. In the cement kiln, the raw material mixture undergoes a chemical reaction at a high temperature of 1375 degrees Celsius to produce molten clinker (clinker is the molten cement raw material without cement grinding).
[0087] Cooling: After the clinker is taken out of the cement kiln, it needs to go through a cooling process. Cooling helps to solidify the clinker and make it suitable for grinding.
[0088] Grinding: The cooled clinker is fed into a cement mill for grinding where it is crushed and mixed with an appropriate amount of gypsum (calcium sulfate) to form the final cement product.
[0089] In cement production, clinker is the main component of cement, while gypsum (calcium sulfate) is an auxiliary additive used to adjust the setting and hardening properties of cement, with a mixing ratio of 3%.
[0090] Embodiment three:
[0091] S1: Raw material preparation: Stone powder and fly ash as admixtures need to be prepared in advance to ensure that their quality meets the relevant standards and requirements, and that the quality of other raw materials such as sand and cement also meets the requirements to ensure the performance of the final mortar;
[0092] S2: Mix design: Cement: The amount of cement will be determined based on the specific strength requirements and concrete mix ratio, and is part of the cement dosage.
[0093] Sand: The amount of sand used will be determined according to the mix ratio of the mortar, usually 4 times the amount of cement;
[0094] Stone powder: The amount of stone powder is generally between 20%, and the specific proportion depends on the quality of the stone powder used and the expected effect;
[0095] Fly ash: The amount of fly ash added is generally between 20%, which also depends on the quality of the fly ash and the expected effect;
[0096] S3: Hybrid:
[0097] Mix the stone powder, fly ash and cement evenly according to the designed mix ratio, which can be done by mechanical mixing or manual mixing;
[0098] During the mixing process, ensure that all raw materials are fully mixed to avoid lumps or unevenness;
[0099] S4: Add water to adjust:
[0100] According to the specific requirements of the mortar, gradually add appropriate amount of water to control the consistency and fluidity of the mortar;
[0101] When adding water, pay attention to adding it gradually to avoid adding too much at one time, which will make the mortar too thin;
[0102] S5: Hybrid Adjustment:
[0103] During the mixing process, the proportion of stone powder, fly ash and cement, as well as the amount of water, can be appropriately adjusted as needed to obtain more suitable mortar properties;
[0104] During the mixing process, tests can be carried out according to actual conditions to adjust the mix ratio of the mortar to achieve the best performance and use effect;
[0105] S6: Inspection and storage:
[0106] After mixing, the mortar is subjected to necessary inspections, such as measuring its fluidity, compressive strength and other indicators, to ensure that its quality meets the requirements;
[0107] Store the mixed mortar in a dry and ventilated environment to prevent it from absorbing moisture or being affected by other contamination.
[0108] The amount of water in stone powder and fly ash is usually not a direct consideration when preparing mortar, because the amount of water added is mainly determined by the performance requirements of the mortar and the humidity of the mixed materials. During the process of mixing mortar, the water content of stone powder and fly ash may affect the final mortar mix ratio.
[0109] Stone powder and fly ash are added to the mixture when preparing mortar, and are usually mixed in a dry state. Therefore, their water content will affect the humidity and fluidity of the final mixture. When mixing mortar, the amount of water added needs to be adjusted according to the humidity and fluidity of the mixture to ensure that the mortar has appropriate plasticity and fluidity.
[0110] Raw material collection: The main raw materials of cement include limestone (CaCO3), clay (SiO2, Al2O3, Fe2O3) and iron ore, which are usually obtained through mining and other methods.
[0111] Grinding and pretreatment: The raw materials need to go through pretreatment processes such as crushing, pulverizing and mixing to ensure that the particle size of the raw materials is suitable, which is conducive to the subsequent calcination reaction.
[0112] Calcination: The pretreated raw material mixture is sent to the cement kiln for calcination. In the cement kiln, the raw material mixture undergoes a chemical reaction at a high temperature of 1450 degrees Celsius to produce molten clinker (clinker is the molten cement raw material without cement grinding).
[0113] Cooling: After the clinker is taken out of the cement kiln, it needs to go through a cooling process. Cooling helps to solidify the clinker and make it suitable for grinding.
[0114] Grinding: The cooled clinker is fed into a cement mill for grinding where it is crushed and mixed with an appropriate amount of gypsum (calcium sulfate) to form the final cement product.
[0115] In cement production, clinker is the main component of cement, while gypsum (calcium sulfate) is an auxiliary additive used to adjust the setting and hardening properties of cement, with a mixing ratio of 5%.
[0116] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. The mortar is prepared by compounding stone powder and fly ash, characterized in that: It includes 1 part of cement, 2-4 parts of sand, 0.1-0.2 parts of stone powder and 0.1-0.2 parts of fly ash; The preparation method comprises the following steps: S1: Raw material preparation: Stone powder and fly ash as admixtures need to be prepared in advance to ensure that their quality meets the relevant standards and requirements, and that the quality of other raw materials such as sand and cement also meets the requirements to ensure the performance of the final mortar; S2: Hybrid: Mix the stone powder, fly ash and cement evenly according to the designed mix ratio, which can be done by mechanical mixing or manual mixing; During the mixing process, ensure that all raw materials are fully mixed to avoid lumps or unevenness; S3: Add water to adjust: According to the specific requirements of the mortar, gradually add appropriate amount of water to control the consistency and fluidity of the mortar; When adding water, pay attention to adding it gradually to avoid adding too much at one time, which will make the mortar too thin; S4: Hybrid Adjustment: During the mixing process, the proportion of stone powder, fly ash and cement, as well as the amount of water, can be appropriately adjusted as needed to obtain more suitable mortar properties; During the mixing process, tests can be carried out according to actual conditions to adjust the mix ratio of the mortar to achieve the best performance and use effect; S5: Inspection and storage: After mixing, the mortar is subjected to necessary inspections, such as measuring its fluidity, compressive strength and other indicators, to ensure that its quality meets the requirements; Store the mixed mortar in a dry and ventilated environment to prevent it from absorbing moisture or being affected by other contamination.
2. The composite mortar prepared from stone powder and fly ash according to claim 1, characterized in that: The amount of water in the stone powder and fly ash is not a factor that is directly considered when preparing mortar, because the amount of water added is determined based on the performance requirements of the mortar and the humidity of the mixed materials. In the process of mixing the mortar, the water content of the stone powder and fly ash will affect the final mortar mix ratio. The stone powder and fly ash are added to the mixture when preparing the mortar and are mixed in a dry state. The water content will affect the humidity and fluidity of the final mixture. When mixing the mortar, the amount of water added needs to be adjusted according to the humidity and fluidity of the mixture to ensure that the mortar has plasticity and fluidity.
3. The mortar prepared by composite stone powder and fly ash according to claim 1, characterized in that: Raw material collection: The raw materials of cement include limestone CaCO3, clay SiO2, Al2O3, Fe2O3 and iron ore, which are obtained through mining and other methods.
4. The mortar prepared by composite stone powder and fly ash according to claim 1, characterized in that: During the grinding and pretreatment, the raw materials need to go through a crushing, pulverizing and mixing pretreatment process to ensure that the particle size of the raw materials is appropriate, which is beneficial to the subsequent calcination reaction.
5. The composite mortar prepared from stone powder and fly ash according to claim 1, characterized in that: The calcination: the pretreated raw material mixture is sent to a cement kiln for calcination. In the cement kiln, the raw material mixture undergoes a chemical reaction at a temperature of 1300-1450 degrees Celsius to generate molten clinker.
6. The composite mortar prepared from stone powder and fly ash according to claim 1, characterized in that: Cooling: After the clinker is taken out of the cement kiln, it goes through a cooling process, which helps to solidify the clinker and make it suitable for grinding.
7. The composite mortar made of stone powder and fly ash according to claim 1, characterized in that: Grinding: The cooled clinker is fed into a cement mill for grinding, in which the clinker is crushed and mixed with gypsum to form a final cement product.
8. The composite mortar made of stone powder and fly ash according to claim 1, characterized in that: In cement production, clinker is a component of cement, while gypsum is an auxiliary additive used to adjust the setting and hardening properties of cement, with a mixing ratio between 0.5% and 5%.