Gangue filling material and application
By introducing alumina powder and silicon powder into the gangue filling material and optimizing the usage of cement and fly ash, the high cost and strength problems caused by the high cement content in the prior art are solved, and the high gangue filling material is achieved. Strength and low cost, suitable for downhole filling and goaf filling.
Patent Information
- Application Number
- CN202411007922.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
AI Technical Summary
The content of cementitious materials in existing gangue filling materials is high, resulting in high cost and poor strength, which affects the promotion and application of gangue underground filling technology.
By introducing alumina powder and silicon powder into the gangue slurry and gangue paste, adjusting the amount of cement and fly ash, controlling the particle size of gangue particles, combining pumping agent and quick-setting agent, optimizing the distribution formula to reduce the The content of cementitious material improves the strength and fluidity of the material.
It achieves the acquisition of high-strength gangue filling materials at lower costs, meets the needs of underground filling and goaf filling construction, reduces material costs, and improves the compressive strength and durability of the materials.
Smart Images

Figure BDA0004963485230000061 
Figure BDA0004963485230000071
Abstract
Description
Technical Field
[0001] The present invention relates to the field of mine filling materials, and in particular to a gangue filling material and application thereof. Background Art
[0002] The ground occupation and pollution caused by the large amount of gangue discharged from ore mining has always been a prominent problem faced by the coal industry. At present, underground filling technology has the dual functions of treating gangue waste and controlling mining subsidence. On the one hand, it can be used as an effective treatment measure for goaf areas, and on the other hand, it can also handle the discharged gangue well. Gangue, which is the main filling material, is mainly used in two forms: solid and paste. The latter has a high solid waste utilization rate, strong filling body integrity, high top connection rate, and significant rock movement control effect. It is the main filling method and future development direction.
[0003] Gangue paste filling materials use gangue as aggregate, add fly ash, cement, etc. to make paste filling slurry, which is transported to the underground filling working face through pipelines. After the filling slurry solidifies and has strength, it plays a role in supporting the overburden. However, in the existing gangue paste filling materials, in order to ensure strength, the content of binders such as fly ash and cement in the gangue paste filling materials is relatively high, mostly 20 to 35%, which leads to a high cost per cubic meter of filling material, affecting the promotion and application of gangue underground filling technology.
[0004] Based on this, how to provide a new gangue filling material to achieve higher material strength at a lower binder content is a technical problem that needs to be solved in this field. Summary of the invention
[0005] The main purpose of the present invention is to provide a gangue filling material and its application, so as to solve the problems of high binder content, high cost and poor strength in the gangue filling material in the prior art.
[0006] In order to achieve the above-mentioned purpose, the present invention provides a gangue filling material on the one hand, which includes gangue slurry and gangue paste; in parts by weight, the gangue slurry includes: 50 to 80 parts of gangue A, 10 to 20 parts of alumina powder, 10 to 20 parts of silicon powder and 0.6 to 40 parts of water reducer; in parts by weight, the gangue paste includes: 50 to 95 parts of gangue B, 4 to 20 parts of cement, 1 to 50 parts of fly ash and 0.5 to 40 parts of additives; in the gangue filling material, the weight ratio of the gangue slurry to the gangue paste is (1.0 to 1.2): 1; the particle size of gangue A is smaller than the particle size of gangue B.
[0007] Furthermore, based on the total weight of the gangue filling material being 100%, the sum of the mass fractions of cement and fly ash is 2 to 18%.
[0008] Furthermore, in the gangue slurry, the particle size d of the gangue A is A 0<d A ≤0.1mm; in the gangue paste, the particle size d of gangue B B 0<d B ≤25mm, preferably 15≤d B ≤20mm.
[0009] Furthermore, in the gangue paste, the fly ash is selected from at least two of Class I fly ash, Class II fly ash and Class III fly ash.
[0010] Furthermore, in terms of weight, the fly ash includes 18 to 20 parts of Class I fly ash, 45 to 50 parts of Class II fly ash, and 30 to 35 parts of Class III fly ash.
[0011] Furthermore, in the gangue slurry, the cement is PO 42.5 ordinary Portland cement.
[0012] Furthermore, in the gangue paste, the auxiliary agent is a pumping agent and / or an accelerating setting agent.
[0013] Furthermore, in the gangue slurry, the water reducer is selected from one or more of aliphatic water reducers, polycarboxylic acid water reducers and naphthalene water reducers.
[0014] Further, in parts by weight, the gangue slurry includes 60 parts of gangue A, 15 parts of alumina powder, 15 parts of silica powder, 10 parts of LQB50 water reducer and 80 parts of water, the gangue paste includes 70 parts of gangue B, 10 parts of cement, 20 parts of fly ash, 10 parts of HY-BS01 pumping agent and 10 parts of LQB50 quick-setting agent, and the weight ratio of the gangue slurry to the gangue paste is 1:1; or, in parts by weight, the gangue slurry includes 80 parts of gangue A, 20 parts of alumina powder, 10 parts of silica powder, 20 parts of LQB50 water reducer and 100 parts of water, and the gangue paste includes 90 parts of gangue B, 5 parts of cement, 30 parts of fly ash, 10 parts of HY-BS01 pumping agent and 10 parts of LQB50 accelerator, and the weight ratio of the gangue slurry to the gangue paste is 1:1; or, by weight, the gangue slurry includes 60 parts of gangue A, 10 parts of alumina powder, 10 parts of silica powder, 40 parts of LQB50 water reducer and 60 parts of water, and the gangue paste includes 50 parts of gangue B, 20 parts of cement, 40 parts of fly ash, 5 parts of HY-BS01 pumping agent and 5 parts of LQB50 accelerator, and the weight ratio of the gangue slurry to the gangue paste is 1:1.
[0015] Another aspect of the present invention provides a use of the above-mentioned gangue filling material as a filling material during the filling construction process of a goaf area.
[0016] By applying the technical solution of the present invention, a gangue filling material with a special formula is provided, which has good fluidity and meets the strength requirements after solidification and hardening, and can meet the needs of filling mining and goaf filling construction. At the same time, the preparation is simple, the materials are easily available, and the cost is lower. DETAILED DESCRIPTION
[0017] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0018] As described in the background technology, there are problems in the prior art that the gangue filling material has a high content of binder, high cost and poor strength. In order to solve the above technical problems, the present invention provides a gangue filling material on one hand, characterized in that the gangue filling material includes gangue slurry and gangue paste; by weight, the gangue slurry includes: 50-80 parts of gangue A, 10-20 parts of alumina powder, 10-20 parts of silicon powder and 0.6-40 parts of water reducer; by weight, the gangue paste includes: 50-95 parts of gangue B, 4-20 parts of cement, 1-50 parts of fly ash and 0.5-40 parts of additives; in the gangue filling material, the weight ratio of gangue slurry to gangue paste is (1.0-1.2):1; the particle size of gangue A is smaller than the particle size of gangue B.
[0019] The gangue filling material provided by the present invention includes gangue slurry and gangue paste. In the gangue slurry, the inventors have creatively introduced alumina powder and silicon powder, thereby significantly improving the strength, quality and durability of the final gangue filling material. In the component formula of the gangue paste, the inventors have reasonably adjusted the amount of binder, that is, cement and fly ash after a large number of experiments, so that it can not only ensure that the filling material can form a hardened body with a certain strength after solidification and hardening, but also can form an effective support effect on the overlying surrounding rock to prevent the collapse of the goaf. The adjustment of the amount of these two materials can also effectively reduce costs and improve the overall product added value of the gangue filling material. On the basis of the above-mentioned component types, the inventors have adjusted and matched the amount of each component in the gangue slurry and the gangue paste after a large number of experiments, so that it forms a complete formula and effectively improves the compressive strength of the obtained gangue filling material. Also, regarding the gangue components present in both the gangue slurry and the gangue paste, namely, gangue A and gangue B, the inventors compared the particle size relationship between the two through a large number of experiments, and in the technical solution provided by the present invention, controlled the particle size of gangue A to be smaller than the particle size of gangue B, thereby significantly improving the uniformity of the two when mixed, giving full play to the coordination effect of the two in terms of size dimension, and thus obtaining a gangue filling material with excellent mechanical properties.
[0020] In conclusion, the gangue filling material provided by the present invention and having the above-mentioned component types and dosage formula not only has low preparation cost, but also has good fluidity and high strength after solidification, thus being able to well meet the use requirements.
[0021] In a preferred embodiment, the total weight of the gangue filling material is 100%, and the sum of the mass fractions of cement and fly ash is 2-18%. As described in the background technology of the present invention, the gangue-based filling materials provided in the prior art, wherein the content of fly ash, cement and other binders in the gangue paste filling materials is relatively high, mostly 20 to 35%. Although such a setting can obtain a material with strength that meets the requirements, the cost is inevitably increased. The present invention can further reduce the sum of the mass fractions of the binders, i.e. cement and fly ash, to 2-18% through formula design and component optimization, thereby obtaining higher mechanical properties while having lower material and preparation costs.
[0022] The gangue filling material provided by the present invention uses gangue particles in both the gangue slurry and the gangue paste. In several typical implementations, in the gangue slurry, the particle size d of the gangue A is A 0<d A ≤0.1mm; in the gangue paste, the particle size d of gangue B B 0<d B ≤25mm. The particle size of the gangue in the gangue slurry is preferably 0<d according to the process route and index requirements. A ≤0.1mm, thereby improving its fluidity and enhancing the strength of the obtained gangue filling material after solidification. As for the gangue paste, the inventors also conducted a lot of experiments and chose to use 0<d B Gangue aggregate within the range of ≤25mm is used as paste filling aggregate to replace conventional aggregate, thereby further reducing costs, improving environmental friendliness, and taking into account higher performance. The fine aggregate gangue A and coarse aggregate gangue B with different particle size ranges provided by the present invention can cooperate with each other in the final gangue filling material to improve its compressive strength and structural uniformity, and can also more effectively utilize existing solid waste. And, regarding the use of the above two types of gangue particles in the present invention, the inventors have mixed the two into gangue slurry and gangue paste respectively after a large number of experiments, and after the two are respectively formed into a uniform whole with other components, they are mixed. Compared with directly mixing the two solids and solidifying them, such a setting can improve the uniformity of gangue particles with different particle sizes when mixing, more effectively play the role of cooperation between the two, and effectively reduce internal defects when the gangue filling material is finally formed, and significantly improve the compressive strength. After a large number of experiments, the inventors further screened the particle size of the gangue B and found that when 15≤d BWhen the particle size is ≤20mm, it can better match the size of the gangue A with a particle size less than 0.1mm, thereby further improving the density and compressive strength of the gangue filling material.
[0023] Regarding the gangue filling material provided by the present invention, the fly ash included in the gangue paste is one of the binders. It is a volcanic ash-like mixed material formed by high-temperature combustion of coal powder, and is mainly solid waste discharged from coal-fired power plants, smelting, chemical industry and other industries. According to the fineness and loss on ignition of the fly ash, it can be divided into three grades, namely: Grade I fly ash, the 0.045mm square hole sieve residue is less than 12%, and the loss on ignition is less than 5%; Grade II fly ash, the 0.045mm square hole sieve residue is less than 20%, and the loss on ignition is less than 8%; Grade III fly ash, the 0.045mm square hole sieve residue is less than 45%, and the loss on ignition is less than 15%. In a preferred embodiment, the fly ash in the gangue paste provided by the present invention is selected from at least two of Grade I fly ash, Grade II fly ash and Grade III fly ash. That is to say, the present invention utilizes the combination of fly ash of different grades (equivalent to the combination of fly ash of different sizes and ignition loss amounts) to achieve a bonding effect that is equivalent to or even better than that of a higher amount with a lower amount of fly ash, thereby obtaining a gangue filling material with higher compressive strength at a lower cost, and its application value is significantly improved.
[0024] Furthermore, in parts by weight, the fly ash includes 18 to 20 parts of Class I fly ash, 45 to 50 parts of Class II fly ash, and 30 to 35 parts of Class III fly ash.
[0025] For the cement in the gangue filling material provided by the present invention, in a preferred embodiment, the cement in the gangue paste is PO 42.5 ordinary Portland cement. Its main chemical components are calcium oxide, silicon dioxide and a small amount of aluminum oxide and iron oxide. The main mineral components are tricalcium silicate C3S, dicalcium silicate C2S, tricalcium aluminate C3A and tetracalcium aluminoferrite C4AF. When it is hydrated to form the gangue filling material, the following reaction will occur:
[0026] 2(3CaO·SiO 2 )+6H 2 O=3CaO·2SiO 2 ·3H 2 O+3Ca(OH) 2 , i.e., hydration of C3S;
[0027] 2(2CaO·SiO 2 )+4H 2 O=3CaO·2SiO 2 ·3H 2 O+Ca(OH) 2, i.e., hydration of C2S;
[0028] 3CaO·Al 2 O 3 +6H 2 O=3CaO·Al 2 O 3 6H 2 O, i.e., hydration of C3A;
[0029] 4CaO·Al 2 O 3 ·Fe 2 O 3 +7H 2 O=3CaO·Al 2 O 3 6H 2 O+CaO·Fe 2 O 3 ·H 2 O, namely the hydration of C4AF.
[0030] The above-mentioned several minerals react as above when mixed to obtain the gangue filling material, and each mineral phase also affects each other during the hydration process. In the process of hydration to form the gangue filling material provided by the present invention, there are the following stages: in the early stage of the induction period, it dissolves rapidly, and tricalcium aluminate is rapidly hydrated in an alkaline environment to generate calcium sulfaluminate, at which time the first exothermic peak is formed; then enters the induction period, CSH and CH are in the nucleation stage; in the subsequent acceleration period, the hydration of tricalcium silicate mainly occurs, forming the second exothermic peak; and in the deceleration period, the transformation of calcium sulfaluminate AFt to monosulfur hydrated calcium sulfoaluminate AFm mainly occurs, and the generated hydration products are filled between the cement particles, and a network structure is gradually formed; finally, it enters the stable period, the hydration heat release rate is low, the cumulative heat release tends to be stable, the microstructure gradually becomes dense, a hardened slurry structure is formed, and finally the gangue filling material with excellent compressive strength in the present application is obtained.
[0031] In several typical embodiments, in the gangue paste, the auxiliary agent is a pumping agent for increasing the mass concentration of the gangue paste and / or an accelerator for helping the paste to quickly achieve initial setting. And further preferably, the pumping agent is HY-BS01; and / or, preferably, the accelerator is J85 and / or LQB50. Theoretically, both the pumping agent and the accelerator can use the types commonly used in the field, and the inventor has selected the above specific types after a large number of experiments and comparisons, and found that they can better adapt to the gangue filling material system provided by the present invention, so as to obtain better performance. Specifically, the above-mentioned pumping agents can more significantly improve the fluidity of the paste and enhance the uniformity of the mixing of the gangue slurry and the gangue paste; the above-mentioned additives make the filling material easier to transport by pipe, and can also improve the strength of the gangue filling material after solidification and hardening.
[0032] In order to increase the fluidity of the slurry, the present invention adds a water reducer therein, and in a preferred embodiment, the water reducer in the gangue slurry is selected from one or more of aliphatic water reducers, polycarboxylic acid water reducers and naphthalene water reducers. With respect to the gangue slurry system and the final gangue filling material system provided by the present invention, the inventors further preferred the water reducer to be one or more of TPED-100, FDN-A and FDN-C after a large number of experiments, and found that it can better adapt to the gangue material, the binder and other various additives, thereby more significantly improving the uniformity of the mixture and enhancing the mechanical properties.
[0033] In several more preferred embodiments, the gangue slurry includes 60 parts of gangue A, 15 parts of alumina powder, 15 parts of silica powder, 10 parts of LQB50 water reducer and 80 parts of water, and the gangue paste includes 70 parts of gangue B, 10 parts of cement, 20 parts of fly ash, 10 parts of HY-BS01 pumping agent and 10 parts of LQB50 quick-setting agent, and the weight ratio of the gangue slurry to the gangue paste is 1:1; or, the gangue slurry includes 80 parts of gangue A, 20 parts of alumina powder, 10 parts of silica powder, 20 parts of LQB50 water reducer and 100 parts of water, and the gangue gypsum includes 70 parts of gangue B, 10 parts of cement, 20 parts of fly ash, 10 parts of HY-BS01 pumping agent and 10 parts of LQB50 quick-setting agent, and the weight ratio of the gangue slurry to the gangue paste is 1:1. The gangue slurry comprises 90 parts of gangue B, 5 parts of cement, 30 parts of fly ash, 10 parts of HY-BS01 pumping agent and 10 parts of LQB50 quick-setting agent, and the weight ratio of the gangue slurry to the gangue paste is 1:1; or, by weight, the gangue slurry comprises 60 parts of gangue A, 10 parts of alumina powder, 10 parts of silica powder, 40 parts of LQB50 water reducer and 60 parts of water, and the gangue paste comprises 50 parts of gangue B, 20 parts of cement, 40 parts of fly ash, 5 parts of HY-BS01 pumping agent and 5 parts of LQB50 quick-setting agent, and the weight ratio of the gangue slurry to the gangue paste is 1:1. After a large number of experiments, the inventor screened and adjusted the dosage of each component in the gangue slurry and the gangue paste, and optimized the above scheme. When the gangue filling material is the above formula, the coordination effect between the components is stronger, the compressive strength of the obtained gangue filling material is higher, and the cost is also lower.
[0034] The gangue filling material provided by the present invention has the following preparation method: gangue A, alumina powder, silica powder, water reducer and water are mixed to obtain gangue slurry; gangue B, cement, fly ash and additives are mixed to obtain gangue paste; gangue slurry and gangue paste are mixed to obtain gangue filling material, which is used for filling goaf.
[0035] Another aspect of the present invention provides an application of the above-mentioned waste rock filling material as a filling material in the filling construction process of the goaf. After being filled into the goaf and solidified, the above-mentioned waste rock filling material provided by the present invention has good compressive strength and lower cost, and can well meet the requirements of filling materials used in underground filling technology.
[0036] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0037] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0038] Example 1
[0039] A gangue filling material:
[0040] Gangue slurry: mix 60 parts of gangue A with a particle size of less than 0.1 mm, 15 parts of alumina powder, 15 parts of silicon powder and 10 parts of LQB50 water reducer, add 80 parts of water and mix well to obtain gangue slurry;
[0041] Gangue paste: 70 parts of gangue B with a particle size of 15 to 20 mm, 10 parts of cement, 20 parts of fly ash, 10 parts of HY-BS01 pumping agent and 10 parts of LQB50 quick-setting agent are mixed to obtain gangue paste; wherein the fly ash includes 20% of Class I fly ash, 50% of Class II fly ash and 30% of Class III fly ash.
[0042] The gangue slurry and the gangue paste are mixed at a weight ratio of 1:1 to obtain a gangue filling material.
[0043] Example 2
[0044] A gangue filling material:
[0045] The only difference between this embodiment and embodiment 1 is that the contents of the components in the gangue slurry and the gangue paste are different, and the specific values are shown in Table 1.
[0046] Example 3
[0047] A gangue filling material:
[0048] The only difference between this embodiment and embodiment 1 is that the contents of the components in the gangue slurry and the gangue paste are different, and the specific values are shown in Table 1.
[0049] Example 4
[0050] A gangue filling material:
[0051] The only difference between this embodiment and embodiment 1 is that the particle size of gangue A in the gangue slurry is greater than 0.2 mm; the particle size of gangue B in the gangue paste is greater than 30 mm, and the content of each component is the same as that in embodiment 1. The specific values are shown in Table 1.
[0052] Example 5
[0053] A gangue filling material:
[0054] The only difference between this embodiment and embodiment 1 is that in the gangue paste, the amount of I, II and III fly ash in the fly ash component is different. Specifically, the fly ash includes 10% of I fly ash, 70% of II fly ash and 20% of III fly ash. The content of each component is the same as in embodiment 1. The specific values are shown in Table 1.
[0055] Comparative Example 1
[0056] A gangue filling material:
[0057] The difference between this comparative example and Example 1 is that the contents of the components in the gangue slurry and the gangue paste are different. The specific values are shown in Table 1.
[0058] Comparative Example 2
[0059] A gangue filling material:
[0060] The only difference between this comparative example and Example 1 is that alumina powder and silicon powder are not added to the gangue slurry, but are replaced by an equal amount of water, and the amounts of the other components are the same as those in Example 1. The specific values are shown in Table 1.
[0061] Table 1
[0062]
[0063]
[0064] From the above description, it can be seen that the above embodiments of the present invention achieve the goal of obtaining gangue filling materials with higher compressive strength at a lower cost.
[0065] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.
[0066] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A gangue filling material, characterized in that: The gangue filling material includes gangue slurry and gangue paste; The gangue slurry comprises, by weight: 50 to 80 parts of gangue A, 10 to 20 parts of alumina powder, 10 to 20 parts of silicon powder and 0.6 to 40 parts of a water reducing agent; The gangue paste comprises, by weight: 50 to 95 parts of gangue B, 4 to 20 parts of cement, 1 to 50 parts of fly ash and 0.5 to 40 parts of additives; In the gangue filling material, the weight ratio of the gangue slurry to the gangue paste is (1.0-1.2):1; The particle size of the gangue A is smaller than the particle size of the gangue B.
2. The gangue filling material according to claim 1, characterized in that: Taking the total weight of the gangue filling material as 100%, the sum of the mass fractions of the cement and the fly ash is 2-18%.
3. The gangue filling material according to claim 1 or 2, characterized in that: In the gangue slurry, the particle size d of the gangue A is A 0<d A ≤0.1mm; in the gangue paste, the particle size d of the gangue B B 0.1<d B ≤25mm, preferably 15≤d B ≤20mm.
4. The gangue filling material according to any one of claims 1 to 3, characterized in that: In the gangue paste, the fly ash is selected from at least two of Class I fly ash, Class II fly ash and Class III fly ash.
5. The gangue filling material according to claim 4, characterized in that: In terms of weight, the fly ash comprises 18 to 20 parts of Class I fly ash, 45 to 50 parts of Class II fly ash, and 30 to 35 parts of Class III fly ash.
6. The gangue filling material according to any one of claims 1 to 3, characterized in that: In the gangue paste, the cement is PO 42.5 ordinary Portland cement.
7. The gangue filling material according to claim 6, characterized in that: In the gangue paste, the auxiliary agent is a pumping agent and / or an accelerating setting agent.
8. The gangue filling material according to claim 7, characterized in that: In the gangue slurry, the water reducer is selected from one or more of aliphatic water reducers, polycarboxylic acid water reducers and naphthalene water reducers.
9. The gangue filling material according to any one of claims 1 to 8, characterized in that: In parts by weight, the gangue slurry includes 60 parts of the gangue A, 15 parts of the alumina powder, 15 parts of the silica powder, 10 parts of the LQB50 water reducer and 80 parts of water, and the gangue paste includes 70 parts of the gangue B, 10 parts of the cement, 20 parts of the fly ash, 10 parts of the HY-BS01 pumping agent and 10 parts of the LQB50 quick-setting agent, and the weight ratio of the gangue slurry to the gangue paste is 1:1; or, in parts by weight, the gangue slurry includes 80 parts of the gangue A, 20 parts of the alumina powder, 10 parts of the silica powder, 20 parts of the LQB50 water reducer and 100 parts of water, and the gangue paste includes 90 parts of The gangue B, 5 parts of the cement, 30 parts of the fly ash, 10 parts of HY-BS01 pumping agent and 10 parts of LQB50 quick-setting agent, and the weight ratio of the gangue slurry to the gangue paste is 1:1; or, by weight, the gangue slurry includes 60 parts of the gangue A, 10 parts of the alumina powder, 10 parts of the silica powder, 40 parts of LQB50 water reducer and 60 parts of water, and the gangue paste includes 50 parts of the gangue B, 20 parts of the cement, 40 parts of the fly ash, 5 parts of HY-BS01 pumping agent and 5 parts of LQB50 quick-setting agent, and the weight ratio of the gangue slurry to the gangue paste is 1:
1.
10. Use of the gangue filling material according to any one of claims 1 to 9 as a filling material in a filling construction process of a goaf area.
Citation Information
Cited By
Shallow-burial-depth fully-mechanized caving mining grouting filling control mining space deformation method
CN120100513A